A catalyst for the preparation of methyl acetal from methanol and its preparation and application
By introducing other metals into Keggin-type heteropolyacids and modifying them with organic amines, the stability and selectivity problems of existing catalysts in the preparation of methyl acetal were solved, and efficient and low-cost methanol oxidative condensation to prepare methyl acetal was achieved.
Patent Information
- Application Number
- CN202211546422.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-05
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-12-05
AI Technical Summary
Existing catalysts for the preparation of methyl acetal suffer from problems such as the high cost of precious metals, the volatility of rhenium at high temperatures, the high toxicity of V-based catalysts, and the poor thermal stability of TiO2, which limit their large-scale industrial application.
A catalyst for the direct oxidative condensation of methanol to methyl acetal was prepared by introducing other metals at their vacancies using Keggin-type heteropolyacids and loading them onto activated carbon, and by modifying them with organic amines to reduce the number of acid centers and improve the metal distribution.
This method improves the selectivity of methylal and the stability of the catalyst, reduces costs, and provides a green synthetic route suitable for the preparation of methylal by methanol oxidative condensation.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] This invention relates to a method for preparing a catalyst for the production of methyl acetal from methanol and its application, specifically to a method for the direct oxidative condensation of methanol to methyl acetal by introducing other metals at their vacancies and loading them onto a support AC. Background Technology
[0002] Methanol is an important chemical raw material that can be produced from coal, natural gas, biomass, etc., via syngas production. Due to the maturity of syngas-to-methanol technology in recent years, there is a serious overcapacity in methanol production, leading to widespread attention on developing downstream methanol products. Methanol can be used to produce organic chemical products such as olefins and alkanes, and it can also be oxidized to prepare oxygen-containing compounds such as aldehydes or esters. The methanol oxidation route offers good atom economy and low energy consumption.
[0003] DMM (dimethyl acetal), commonly known as methyl acetal, is an important chemical material. It possesses low toxicity, a low boiling point, high oxygen content, and exhibits both hydrophilic and lipophilic properties, good solubility, low surface tension, and low heat of vaporization. It is widely used in pharmaceuticals, cosmetics, daily necessities, pesticides, automotive parts, cotton, rubber, detergents, paints, inks, and diesel additives. Due to its excellent volatility and lack of ozone depletion, it can be used as a refrigerant to replace Freon. Currently, the main industrial method for producing DM is the methanol-formaldehyde condensation method. However, this method uses a highly acidic catalyst, which is corrosive to equipment and unsuitable for long-term use. Therefore, the one-step methanol oxidation method for producing DM has attracted widespread attention.
[0004] In recent years, researchers have conducted extensive studies on the direct preparation of methylal by the oxidative condensation of methanol, developing a variety of catalysts, including Ru-based catalysts (e.g., Chemical Reaction Engineering and Technology, 2013, 29(5): 462-469), Re-based catalysts (e.g., Catal Today, 2010, 155: 177-183, patent US 6403841, CN 1911503A), heteropolyacid catalysts (e.g., patent US 0154226), and non-noble metal V-based catalysts. However, the high cost of noble metals and the high volatility of rhenium oxides at high temperatures, leading to catalyst deactivation, have limited their widespread application. V-based catalysts are the most studied catalysts, and high selectivity in the production of methyl acetal has been achieved on V-based catalysts (e.g., Chem Commun, 2011, 47: 9345-9347., Chem Commun, 2007, 21: 2172-2174., Hin J Catal, 2013, 34(11): 2110-2117.; patents CN 200410065321.6, US 6281378, CN 1634655). However, V-based catalysts suffer from problems such as high vanadium source toxicity, poor thermal stability of TiO2, and low mechanical strength, which greatly limit their further large-scale industrial application. Summary of the Invention
[0005] The main technical problem solved by this invention is to provide a Keggin-type heteropolyacid with other metals introduced at its vacancy sites and loaded onto a carrier activated carbon (denoted as AC). By modifying the heteropolyacid with organic amines, the number of acid centers and metal dispersion on the surface of the heteropolyacid are effectively reduced, the generation of the byproduct DME is inhibited, and the selectivity of methyl acetal is improved.
[0006] The catalyst was modified by using organic amines through hydrothermal synthesis to modify the heteropolyacid, thereby reducing the number of acid centers on the surface of the heteropolyacid and improving the distribution of metals.
[0007] A method for preparing and applying a catalyst for the production of methyl acetal from methanol, specifically comprising: Preparation of substituted heteropolyacid catalysts for the direct oxidative condensation of methanol to methyl acetal: The catalyst uses AC as a support and supports a Keggin-type heteropolyacid with the chemical formula H. 3+n PZ n X 12-n O 40 / AC, where n=0-4, the substituted metal Z is one of Bi, As, Sb, Nb, Ta, V; the central metal atom X is one of Mo, W; the catalyst is modified by using organic amines through hydrothermal synthesis to modify the heteropolyacid, thereby reducing the number of acid centers on the surface of the heteropolyacid and improving the distribution of metals.
[0008] The precursor of the substituted metal Z is one or more of the nitrates, carbonates or acetates of Bi, As, Sb, Nb, Ta, and V.
[0009] The precursors of the central metal atoms Mo and W are either Na2MoO4 or Na2WO4.
[0010] The heteropoly acid is supported on AC, and the heteropoly acid accounts for 5-50 wt% of the catalyst by mass (based on the AC support).
[0011] The organic amine modifies the heteropolyacid. The organic amine is one or more of ethylenediamine, triethanolamine, formamide, acetamide, and diethylenetriamine. The concentration of the organic amine is 0.1-1 mol / L, preferably 0.1-0.5 mol / L.
[0012] The specific preparation method of the above-mentioned catalyst for the direct oxidative condensation of methanol to prepare methyl acetal includes: (1) Weigh a certain amount of precursor of central metal atom (Na2WO4·2H2O or Na2MoO4·2H2O) and organic amine, add them to deionized water at 50-70 ℃, and a 0.1-1 mol / L aqueous solution is formed; (2) Weigh a certain precursor containing Z element and add it to deionized water at 50-70 ℃ to form an aqueous solution of 0.02-0.3 mol / L. Then add the solution to solution (1), adjust the pH of the solution to 3-7 with 40%-85% phosphoric acid and stir continuously. During the stirring process, add water continuously and stop stirring after 0.5-3.0 h.
[0013] (3) After cooling the solution (2), add it to the pressure-resistant stainless steel reactor and react it under hydrothermal conditions of 120-180℃ for 90-120 h. Then cool it down to 60-100℃ and keep it for 6-24 h until it reaches room temperature.
[0014] (4) Weigh a certain amount of carrier AC and add it to the prepared solution (3). After mixing thoroughly, dry it at 120℃ and calcine it at 300-800℃ for 2-10 h to obtain the supported heteropolyacid catalyst. The application of the catalyst is characterized in that this series of catalysts can be used to directly oxidize and condense methanol to prepare methylal. A fixed-bed reactor is used, with the substituted heteropolyacid catalyst (20-60 mesh after molding) filled in the middle section of the bed, and the upper and lower sections filled with quartz sand; the raw material is methanol, with a methanol-to-oxygen volume ratio of 1:1 to 1:6, and the remainder being any one of the inert gases Ar, He, or N2; the reaction temperature is 200-450 ℃, the reaction is carried out at atmospheric pressure, and the GHSV of the reaction process is 1000-9000 h⁻¹. -1 The product that can be collected is a mixed solution containing methylal and methanol.
[0015] The reactions involved in this invention can be represented by the following reaction equations: Beneficial technical effects of the present invention: 1. The prepared heteropolyacid is a heteropolyacid with a Keggin-type structure. By modifying it with organic amines, the number of acid centers on the surface of the heteropolyacid is reduced, thereby improving the selectivity of the product methyl acetal (selectivity is 80%-92%). 2. Due to the strong acidity of heteropoly acids and the fact that the reaction takes place at 200-450 °C with the generation of water, the loss of support components such as molecular sieves or silica gradually deactivates the catalyst. After treatment using activated carbon (AC) as a support, more hydroxyl or alcohol hydroxyl groups can form on the surface of the activated carbon, which can combine more stably with the heteropoly acids, thereby improving the stability of the catalyst.
[0016] 3. The catalyst obtained is used for the oxidative condensation of methanol to prepare methyl acetal. The process is simple, convenient, and effectively reduces costs. It is a green synthesis route with good application prospects.
[0017] The advantages of this invention are that the catalyst has redox properties and suitable B acid sites, strong activity, and good selectivity. Detailed Implementation
[0018] Example 1 The preferred embodiments of the present invention will now be described in detail so that the advantages and features of the present invention can be more easily understood by those skilled in the art, thereby providing a clearer and more explicit definition of the scope of protection of the present invention.
[0019] Weigh 0.36 g Na₂MoO₄·2H₂O and 0.0902 g ethylenediamine and add them to 15 ml of deionized water at 50 °C, resulting in a solution concentration of 0.1 mol / L. Heat to boiling and record this as solution A. While stirring continuously, add 85% H₃PO₄ to adjust the pH to 6.5. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 1.5 h and record this as solution B. Then, place solution B into a pressure-resistant stainless steel reactor and react at 160 °C hydrothermally for 100 h. Subsequently, cool to 100 °C and maintain this temperature for 6 h. The substituted heteropolyacid H₃PMo₄ is obtained upon cooling to room temperature. 12 O 40 Let it be denoted as C; 2.42 g of the support AC was weighed and added to solution C, and stirred continuously with a magnetic stirrer for 6 h. The mixture was then filtered, dried at 120 ℃ for 12 h, and finally calcined in a muffle furnace at 500 ℃ in air for 6 h. The resulting sample is the catalyst for the production of methyl acetal, denoted as PMo. 12 / AC; The obtained samples were pressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:1, the reaction temperature was 340 ℃, and the GHSV was 5000 h⁻¹. -1 The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and N2 was used as the inert gas. Online gas chromatography was used for monitoring; the final analysis showed a methanol conversion rate of 67.5% and a selectivity of methyl acetal of 79.2%.
[0020] Example 2 Weigh 0.73 g Na₂MoO₄·2H₂O and 0.4476 g triethanolamine and add them to 15 ml of deionized water at 50 °C, resulting in a solution concentration of 0.2 mol / L. Heat to boiling and record this as solution A. Weigh 0.0319 g ammonium metavanadate and add it to deionized water at 50 °C to form a 0.1 mol / L aqueous solution. Add this solution to solution A while stirring, and record this as solution B. While stirring continuously, add 85% H₃PO₄ to solution B to adjust the pH to 6.5. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 1.5 h and record this as solution C. Then, place solution C in a pressure-resistant stainless steel reactor and react at 120 °C under hydrothermal conditions for 120 h. Subsequently, cool to 100 °C and maintain for 20 h. After cooling to room temperature, the substituted heteropolyacid H₅PV₂Mo₄ is obtained. 10 O 40 Let it be denoted as D; 4.54 g of support AC was weighed and added to the prepared solution D, and stirred continuously for 6 h with a magnetic stirrer. The mixture was then filtered, dried at 120 °C, and finally calcined in a muffle furnace at 800 °C in air for 2 h. The resulting sample is the catalyst for the production of methyl acetal, denoted as PV2Mo. 10 / AC; The obtained samples were pressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:4, the reaction temperature was 450 ℃, and GHSV = 9000 h⁻¹. -1 The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and N2 was used as the inert gas. Online gas chromatography was used for monitoring; the final analysis showed a methanol conversion rate of 69.8% and a selectivity of methyl acetal of 72.6%.
[0021] Example 3 Weigh 0.73 g Na₂MoO₄·2H₂O and 0.1351 g formamide and add them to 15 ml of deionized water at 70 ℃, resulting in a solution concentration of 0.2 mol / L. Heat to boiling and record as solution A. Weigh 0.1818 g ammonium niobate oxalate and add it to deionized water at 50 ℃ to form a 0.1 mol / L aqueous solution. Add this solution to solution A while stirring, and record as solution B. While stirring continuously, add 40% H₃PO₄ to solution B to adjust the pH to 7.0. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 1.5 h and record as solution C. Then, place solution C in a pressure-resistant stainless steel reactor and react at 180 ℃ hydrothermally for 90 h. Subsequently, cool to 100 ℃ and maintain for 20 h. After cooling to room temperature, the substituted heteropolyacid H₄PVMo is obtained. 11 O 40 Let it be denoted as D; 4.74 g of support AC was weighed and added to the prepared solution D, and stirred continuously with a magnetic stirrer for 6 h. The mixture was then filtered, dried at 120 ℃, and finally calcined in a muffle furnace at 600 ℃ in air for 6 h. The resulting sample is the catalyst for the production of methyl acetal, denoted as PVMo. 11 / ACS; The obtained samples were compressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:6, the reaction temperature was 200 ℃, and GHSV = 1000 h⁻¹. -1 The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and N2 was used as the inert gas. Online gas chromatography was used for monitoring; the final analysis showed a methanol conversion rate of 68.4% and a selectivity of methyl acetal of 85.4%.
[0022] Example 4 Weigh 0.44 g Na₂WO₄·2H₂O and 0.0902 g ethylenediamine and add them to 15 ml of deionized water at 50 ℃, resulting in a solution concentration of 0.1 mol / L. Heat to boiling and record this as solution A. While stirring continuously, add 85% H₃PO₄ to adjust the pH to 6.5. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 3.0 h and record this as solution B. Then, place solution B into a pressure-resistant stainless steel reactor and react at 160 ℃ hydrothermally for 100 h. Subsequently, cool to 80 ℃ and maintain this temperature for 6 h. The product, H₃PW, is the substituted heteropolyacid. 12 O 40 Let it be denoted as C; 2.94 g of the carrier AC was weighed and added to solution C, and stirred continuously with a magnetic stirrer for 6 h. The mixture was then filtered, dried at 120 ℃ for 12 h, and finally calcined in a muffle furnace at 500 ℃ in air for 6 h. The resulting sample is the catalyst for the production of methyl acetal, denoted as PW. 12 / AC; The obtained samples were pressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:1, the reaction temperature was 300 ℃, and the GHSV was 5000 h⁻¹. -1 The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and N2 was used as the inert gas. Online gas chromatography was used for monitoring; the final analysis showed a methanol conversion rate of 68.2% and a selectivity of methyl acetal of 89.6%.
[0023] Example 5 Weigh 1.45 g Na₂MoO₄·2H₂O and 0.3544 g acetamide and add them to 15 ml of deionized water at 50 °C, resulting in a solution concentration of 0.4 mol / L. Heat to boiling and record this as solution A. Weigh 0.2646 g bismuth nitrate and add it to deionized water at 70 °C to form a 0.04 mol / L aqueous solution. Add this solution to solution A while stirring, and record this as solution B. While stirring continuously, add 85% H₃PO₄ to solution B to adjust the pH to 6.5. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 0.5 h and record this as solution C. Then, place solution C in a pressure-resistant stainless steel reactor and react under hydrothermal conditions at 120 °C for 90 h. Subsequently, cool to 60 °C and maintain for 24 h. After cooling to room temperature, the substituted heteropolyacid H₄PBiMo is obtained. 11 O 40 Let it be denoted as D; 17.16 g of support AC was weighed and added to the prepared solution D, and stirred continuously with a magnetic stirrer for 6 h. The mixture was then filtered, dried at 120 ℃, and finally calcined in a muffle furnace at 300 ℃ in air for 10 h. The resulting sample is the catalyst for the production of methyl acetal, denoted as PBiMo. 11 / AC; The obtained samples were pressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:6, the reaction temperature was 200 ℃, and the GHSV was 3000 h⁻¹. -1 The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and N2 was used as the inert gas. Online gas chromatography was used for monitoring; the final analysis showed a methanol conversion rate of 66.3% and a selectivity of methyl acetal of 86.5%.
[0024] Example 6 Weigh 2.18 g Na₂MoO₄·2H₂O and 0.9285 g diethylenetriamine and add them to 15 ml of deionized water at 60 °C, resulting in a solution concentration of 0.6 mol / L. Heat to boiling and record this as solution A. Weigh 0.9179 g bismuth carbonate and add it to deionized water at 60 °C to form a 0.12 mol / L aqueous solution. Add this solution to solution A while stirring, and record this as solution B. While stirring continuously, add 85% H₃PO₄ to solution B to adjust the pH to 4.0. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 1.5 h and record this as solution C. Then, place solution C in a pressure-resistant stainless steel reactor and react at 140 °C under hydrothermal conditions for 110 h. Subsequently, cool to 100 °C and maintain for 12 h. After cooling to room temperature, the substituted heteropolyacid H₅PBi₂Mo₄ is obtained. 10 O 40 Let it be denoted as D; 20.64 g of support AC was weighed and added to the prepared solution D, and stirred continuously with a magnetic stirrer for 6 h. The mixture was then filtered, dried at 120 ℃, and finally calcined in a muffle furnace at 300 ℃ in air for 10 h. The resulting sample is the catalyst for the production of methyl acetal, denoted as PBi2Mo. 10 / AC; The obtained samples were pressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:6, the reaction temperature was 200 ℃, and the GHSV was 3000 h⁻¹. -1The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and He was the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methanol conversion rate of 70.2% and a selectivity of methyl acetal of 86.1%.
[0025] Example 7 Weigh 1.76 g Na₂WO₄·2H₂O and 0.3606 g ethylenediamine and add them to 15 ml of deionized water at 70 °C, resulting in a solution concentration of 0.4 mol / L. Heat to boiling and record this as solution A. Weigh 0.4777 g bismuth oxalate and add it to deionized water at 70 °C to form a 0.08 mol / L aqueous solution. Add this solution to solution A while stirring, and record this as solution B. While stirring continuously, add 85% H₃PO₄ to solution B to adjust the pH to 5.0. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 1.5 h and record this as solution C. Then, place solution C in a pressure-resistant stainless steel reactor and react at 150 °C under hydrothermal conditions for 90 h. Subsequently, cool to 100 °C and maintain for 6 h. After cooling to room temperature, the substituted heteropolyacid H₅PBi₂W₃ is obtained. 10 O 40 Let it be denoted as D; 16 g of support AC was weighed and added to the prepared solution D, and stirred continuously with a magnetic stirrer for 6 h. The mixture was then filtered, dried at 120 ℃, and finally calcined in a muffle furnace at 450 ℃ in air for 4 h. The resulting sample is the catalyst for the production of methyl acetal, denoted as PBi2W. 10 / AC; The obtained samples were compressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:6, the reaction temperature was 280 ℃, and the GHSV was 3000 h⁻¹. -1 The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and N2 was used as the inert gas. Online gas chromatography was used for monitoring; the final analysis showed a methanol conversion rate of 67.1% and a selectivity of methyl acetal of 87.5%.
[0026] Example 8 Weigh 3.63 g Na₂MoO₄·2H₂O and 2.2379 g triethanolamine and add them to 15 ml of deionized water at 50 °C, resulting in a solution concentration of 1.0 mol / L. Heat to boiling and record this as solution A. Weigh 0.4258 g of orthoarsic acid and add it to deionized water at 50 °C to form a 0.20 mol / L aqueous solution. Add this solution to solution A while stirring, and record this as solution B. While stirring continuously, add 85% H₃PO₄ to solution B to adjust the pH to 7.0. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 1.5 h and record this as solution C. Then, place solution C in a pressure-resistant stainless steel reactor and react under hydrothermal conditions at 150 °C for 120 h. Subsequently, cool to 100 °C and maintain for 16 h. After cooling to room temperature, the substituted heteropolyacid H₅PAs₂Mo is obtained. 10 O 40 Let it be denoted as D; 22.53 g of support AC was weighed and added to the prepared solution D, and stirred continuously with a magnetic stirrer for 6 h. The mixture was then filtered, dried at 120 ℃, and finally calcined in a muffle furnace at 550 ℃ in air for 5 h. The resulting sample is the catalyst for the production of methyl acetal, denoted as PAs2Mo. 10 / AC; The obtained samples were pressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:6, the reaction temperature was 220 ℃, and the GHSV was 6000 h⁻¹. -1 The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and N2 was used as the inert gas. Online gas chromatography was used for monitoring; the final analysis showed a methanol conversion rate of 60.3% and a selectivity of methyl acetal of 83.2%.
[0027] Example 9 Weigh 2.90 g Na₂MoO₄·2H₂O and 0.5405 g formamide and add them to 15 ml of deionized water at 50 ℃, resulting in a solution concentration of 0.8 mol / L. Heat to boiling and record this as solution A. Weigh 3.4079 g metaarsenic acid and add it to deionized water at 50 ℃ to form a 0.07 mol / L aqueous solution. Add this solution to solution A while stirring, and record this as solution B. While stirring continuously, add 85% H₃PO₄ to solution B to adjust the pH to 5.5. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 1.5 h and record this as solution C. Then, place solution C in a pressure-resistant stainless steel reactor and react under hydrothermal conditions at 150 ℃ for 90 h. Subsequently, cool to 100 ℃ and maintain for 8 h. After cooling to room temperature, the substituted heteropolyacid H₄PAsMo is obtained. 11 O 40 Let it be denoted as D; 18.56 g of support AC was weighed and added to the prepared solution D, and stirred continuously for 6 h with a magnetic stirrer. The mixture was then filtered, dried at 120 °C, and finally calcined in a muffle furnace at 450 °C in air for 4.5 h. The resulting sample is the catalyst for the production of methyl acetal, denoted as PAsMo. 11 / AC; The obtained samples were pressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:2, the reaction temperature was 260 ℃, and the GHSV was 3500 h⁻¹. -1 The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and N2 was used as the inert gas. Online gas chromatography was used for monitoring; the final analysis showed a methanol conversion rate of 65.1% and a selectivity of methyl acetal of 70.9%.
[0028] Example 10 Weigh 2.64 g Na₂WO₄·2H₂O and 0.5316 g acetamide and add them to 15 ml of deionized water at 60 ℃, resulting in a solution concentration of 0.6 mol / L. Heat to boiling and record this as solution A. Weigh 0.2175 g pyroarsic acid and add it to deionized water at 50 ℃ to form a 0.05 mol / L aqueous solution. Add this solution to solution A while stirring, and record this as solution B. While stirring continuously, add 85% H₃PO₄ to solution B to adjust the pH to 6.5. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 1.5 h and record this as solution C. Then, place solution C in a pressure-resistant stainless steel reactor and react under hydrothermal conditions at 150 ℃ for 90 h. Subsequently, cool to 100 ℃ and maintain for 8 h. After cooling to room temperature, the substituted heteropolyacid H₄PAsW is obtained.11 O40, denoted as D; 13.01 g of support AC was weighed and added to the prepared solution D, and stirred continuously with a magnetic stirrer for 6 h. The mixture was then filtered, dried at 120 ℃, and finally calcined in a muffle furnace at 450 ℃ in air for 4.5 h. The resulting sample is the catalyst for the production of methyl acetal, denoted as PAsW. 11 / AC; The obtained samples were pressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:2, the reaction temperature was 380 ℃, and GHSV = 3500 h⁻¹. -1 The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and N2 was used as the inert gas. Online gas chromatography was used for monitoring; the final analysis showed a methanol conversion rate of 67.3% and a selectivity of methyl acetal of 81.5%.
[0029] Example 11 Weigh 0.73 g Na₂MoO₄·2H₂O and 0.3095 g diethylenetriamine and add them to 15 ml of deionized water at 60 °C, resulting in a solution concentration of 0.2 mol / L. Heat to boiling and record this as solution A. Weigh 0.3235 g antimony pentoxide and add it to deionized water at 60 °C to form a 0.07 mol / L aqueous solution. Add this solution to solution A while stirring, and record this as solution B. While stirring continuously, add 85% H₃PO₄ to solution B to adjust the pH to 6.0. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 1.5 h and record this as solution C. Then, place solution C in a pressure-resistant stainless steel reactor and react at 120 °C under hydrothermal conditions for 120 h. Subsequently, cool to 100 °C and maintain for 6 h. After cooling to room temperature, the substituted heteropolyacid H₆PSb₃Mo₹O₃ is obtained. 40 Let it be denoted as D; 14.99 g of carrier AC was weighed and added to the prepared solution D, and stirred continuously for 6 h under magnetic stirring. Then it was filtered, dried at 120 ℃, and finally calcined in a muffle furnace at 300 ℃ in air atmosphere for 8 h. The obtained sample is the catalyst for the production of methyl acetal, denoted as PSb3Mo9 / AC. The obtained samples were pressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:3, the reaction temperature was 240 ℃, and GHSV = 1900 h⁻¹. -1The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and N2 was used as the inert gas. Online gas chromatography was used for monitoring; the final analysis showed a methanol conversion rate of 62.2% and a selectivity of methyl acetal of 85.2%.
[0030] Example 12 Weigh 1.45 g Na₂MoO₄·2H₂O and 0.3606 g ethylenediamine and add them to 15 ml of deionized water at 50 °C, resulting in a solution concentration of 0.4 mol / L. Heat to boiling and record this as solution A. Weigh 0.3498 g antimony trioxide and add it to deionized water at 50 °C to form a 0.08 mol / L aqueous solution. Add this solution to solution A while stirring, and record this as solution B. While stirring continuously, add 85% H₃PO₄ to solution B to adjust the pH to 4.5. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 1.5 h and record this as solution C. Then, place solution C in a pressure-resistant stainless steel reactor and react at 120 °C under hydrothermal conditions for 100 h. Subsequently, cool to 100 °C and maintain for 10 h. After cooling to room temperature, the substituted heteropolyacid H₅PSb₂Mo₂ is obtained. 10 O 40 Let it be denoted as D; 12.10 g of support AC was weighed and added to the prepared solution D, and stirred continuously for 6 h with a magnetic stirrer. The mixture was then filtered, dried at 120 °C, and finally calcined in a muffle furnace at 450 °C in air for 4 h. The resulting sample is the catalyst for the production of methyl acetal, denoted as PSb2Mo. 10 / AC; The obtained samples were pressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:1, the reaction temperature was 280 ℃, and GHSV = 2400 h⁻¹. -1 The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and He was the inert gas. Online gas chromatography was used for monitoring; the final analysis showed a methanol conversion rate of 66.9% and a selectivity of methyl acetal of 82.1%.
[0031] Example 13 Weigh 0.73 g Na₂MoO₄·2H₂O and 0.1803 g ethylenediamine and add them to 15 ml of deionized water at 50 °C, resulting in a solution concentration of 0.2 mol / L. Heat to boiling and record as solution A. Weigh 0.0826 g ammonium niobate oxalate and add it to deionized water at 50 °C to form a 0.02 mol / L aqueous solution. Add this solution to solution A while stirring, and record as solution B. While stirring continuously, add 85% H₃PO₄ to solution B to adjust the pH to 6.5. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 1.5 h and record as solution C. Then, place solution C in a pressure-resistant stainless steel reactor and react at 110 °C under hydrothermal conditions for 120 h. Subsequently, cool to 100 °C and maintain for 7 h. After cooling to room temperature, the substituted heteropolyacid H₄PNbMo₄ is obtained. 11 O 40 Let it be denoted as D; 16.17 g of support AC was weighed and added to the prepared solution D, and stirred continuously with a magnetic stirrer for 6 h. The mixture was then filtered, dried at 120 ℃, and finally calcined in a muffle furnace at 450 ℃ in air for 4 h. The resulting sample is the catalyst for the production of methyl acetal, denoted as PNbMo. 11 / AC; The obtained samples were pressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:2, the reaction temperature was 220 ℃, and GHSV = 2400 h⁻¹. -1 The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and N2 was used as the inert gas. Online gas chromatography was used for monitoring; the final analysis showed a methanol conversion rate of 69.0% and a selectivity of methylal of 85.2%.
[0032] Example 14 Weigh 2.18 g of Na₂MoO₄·2H₂O and 0.4054 g of formamide and add them to 15 ml of deionized water at 70 ℃, resulting in a solution concentration of 0.6 mol / L. Heat to boiling and record this as solution A. Weigh 1.1961 g of niobium pentoxide and add it to deionized water at 70 ℃ to form a 0.30 mol / L aqueous solution. Add this solution to solution A while stirring, and record this as solution B. While stirring continuously, add 85% H₃PO₄ to solution B to adjust the pH to 6.5. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 1.5 h and record this as solution C. Then, place solution C in a pressure-resistant stainless steel reactor and react under hydrothermal conditions at 100 ℃ for 120 h. Subsequently, cool to 100 ℃ and maintain for 12 h. After cooling to room temperature, the substituted heteropolyacid H₇PNb₄Mo₈O₃ is obtained. 40 Let it be denoted as D; 28.11 g of carrier AC was weighed and added to the prepared solution D, and stirred continuously for 6 h under magnetic stirring. Then it was filtered, dried at 120 ℃, and finally calcined in a muffle furnace at 600 ℃ in air atmosphere for 3 h. The obtained sample is the catalyst for the production of methyl acetal, denoted as PNb4Mo8 / AC. The obtained samples were pressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:2, the reaction temperature was 400 ℃, and GHSV = 8900 h⁻¹. -1 The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and He was the inert gas. Online gas chromatography was used for monitoring; final analysis showed a methanol conversion rate of 63.6% and a selectivity of methyl acetal of 68.3%.
[0033] Example 15 Weigh 4.41 g Na₂WO₄·2H₂O and 1.5476 g diethylenetriamine and add them to 15 ml of deionized water at 50 °C, resulting in a solution concentration of 1.0 mol / L. Heat to boiling and record as solution A. Weigh 0.7337 g niobium oxalate hydrate and add it to deionized water at 50 °C to form a 0.09 mol / L aqueous solution. Add this solution to solution A while stirring, and record as solution B. Add 85% H₃PO₄ to solution B while stirring continuously to adjust the pH to 3.5. Continuously add water during stirring to maintain a constant system volume. Stop stirring after 1.5 h and record as solution C. Place solution C in a pressure-resistant stainless steel reactor and react at 110 °C hydrothermally for 120 h. Then cool to 100 °C and maintain for 7 h. The substituted heteropolyacid H₄PNbW₄ is obtained when the temperature drops to room temperature. 11 O40 Let it be denoted as D; 10.28 g of support AC was weighed and added to the prepared solution D, and stirred continuously for 6 h with a magnetic stirrer. The mixture was then filtered, dried at 120 °C, and finally calcined in a muffle furnace at 450 °C in air for 4 h. The resulting sample is the catalyst for the production of methyl acetal, denoted as PNbMo. 11 / AC; The obtained samples were pressed into tablets to a mesh size of 20-60 and then loaded into a stainless steel tube fixed-bed reactor (fixed bed inner diameter 8 mm). The methanol:oxygen volume ratio was 1:2, the reaction temperature was 220 ℃, and GHSV = 2400 h⁻¹. -1 The carrier gas was an inert gas, an oxygen-containing inert atmosphere (oxygen content 20 vol%), and Ar was used as the inert gas. Online gas chromatography monitoring was performed; the final analysis showed a methanol conversion rate of 67.5% and a selectivity of methyl acetal of 85.2%.
[0034] The above description is merely an embodiment of the present invention and does not limit the patent scope of the present invention. Any equivalent structural or procedural transformations made based on the content of the present invention's specification and drawings, or direct or indirect applications in other related technical fields, are similarly included within the patent protection scope of the present invention.
Claims
1. A process for the preparation of a catalyst for the preparation of methylal from methanol, characterized in that: The catalyst is Keggin type heteropoly acid supported on activated carbon AC, chemical formula is H 3+n PZ n X 12-n O 40 / AC, wherein n=0-4, the substituted metal Z is one or more than two of As, Sb, Nb, V; the central metal atom X is one or two of Mo, W. (1) Weigh the precursor of the central metal atom X and the nitrogen-containing organic matter, add them to water to form solution A; Take no or weigh the precursor containing element Z, add it to water to form a solution, and then add this solution to the above solution A to form solution B; (2) Adjust the pH of solution A or solution B to 3-7 with phosphoric acid and stir continuously for 0.5-3.0 h; (3) Add the solution obtained in step (2) into the reactor and react at 120-180℃ for 90-120 h under hydrothermal conditions. Then cool down to 60-100℃ and maintain for 6-24 h until it reaches room temperature. (4) Weigh the support AC and add it to the solution obtained in step (3), dry it thoroughly, and calcine it at 300-800 ℃ for 1-10 h to obtain the supported heteropolyacid catalyst. Nitrogen-containing organic compounds are used to modify heteropolyacids. The types of nitrogen-containing organic compounds are one or more of ethylenediamine, triethanolamine, formamide, acetamide, and diethylenetriamine. The concentration of nitrogen-containing organic compounds in solution A is 0.1-1 mol / L.
2. The method of claim 1, wherein the catalyst is prepared by a method comprising: The substituted metal Z is one or more of the nitrate, carbonate or acetate of the substituted metal Z; the precursor of the central metal atom X is one or two of Na2MoO4 and Na2WO4, and the concentration of the precursor of the central metal atom X in solution A is 0.1-1 mol / L.
3. The method of claim 1, wherein the catalyst is prepared by the steps of: The concentration of nitrogen-containing organic matter in solution A is 0.1-0.5 mol / L, and the concentration of the precursor of the central metal atom X in solution A is 0.1-0.5 mol / L.
4. The method of claim 1, wherein the catalyst is prepared by the steps of: The heteropoly acid is loaded onto AC as a carrier, and the mass fraction of the heteropoly acid relative to the carrier AC is 5-50 wt%.
5. The method for preparing the catalyst according to any one of claims 1-4, characterized in that: The specific process is as follows: (1) Weigh the precursor of the central metal atom X, Na2WO4·2H2O or Na2MoO4·2H2O, and the organic amine, and add them to deionized water at 50-70℃ to form a solution A with the concentrations of the precursor of the central metal atom X and the organic amine being 0.1-1 mol / L respectively. Take no precursor or weigh one containing element Z, add it to deionized water at 50-70 ℃ to form an aqueous solution of 0.02-0.3 mol / L, and then add this aqueous solution to solution A to form solution B; (2) Adjust the pH of the solution to 3-7 with 40%-85% phosphoric acid and stir continuously. Stop stirring after 0.5-3.0 h. (3) Add the solution obtained in step (2) into the reactor and react at 120-180℃ for 90-120 h under hydrothermal conditions. Then cool down to 60-100℃ and maintain for 6-24 h until it reaches room temperature. (4) Weigh the support AC and add it to the prepared solution (3). After mixing thoroughly, dry it and calcine it at 300-800 °C for 1-10 h to obtain the supported heteropolyacid catalyst.
6. A supported heteropolyacid catalyst prepared by any one of the preparation methods described in claims 1-5.
7. The application of the catalyst according to claim 6, characterized in that: This catalyst is used to catalyze the direct oxidative condensation of methanol to prepare methylal.
8. The application of the catalyst according to claim 7, characterized in that: Utilizing a fixed bed reactor, the middle section of the bed is filled with the supported heteropoly acid catalyst, the catalyst is selected from 20-60 mesh shaped catalyst, the upper and lower sections are filled with quartz sand; the raw material is methanol, the volume ratio of methanol to oxygen is 1:1-1:6, the rest is any one or two or more of inert atmospheres Ar, He or N2; the reaction temperature is 200-450℃, normal pressure reaction, the GHSV of the reaction process is 1000-9000 h -1 .
Citation Information
Patent Citations
Catalyst for producing methylal by selective oxidation of methanol and preparation method and use thereof
CN1305562C
Catalyst for synthesizing methy acetal by oxidizing methanol and its preparation method and application
CN1911503A
Improvement in bronzing-machines
US154226A
Vanadium-containing catalysts, process for manufacturing and use of the same
US6281378B1
Oxidation of methanol and / or dimethyl ether using supported molybdenum-containing heteropolyacid catalysts
US20050154226A1