A kind of lithium polyacrylate and its preparation method and application

By acidifying and modifying sodium polyacrylate and reacting with lithium hydroxide, the cross-linking problem caused by hydrogen bonding in the preparation of lithium polyacrylate is solved, the reaction rate of lithium ions and the stability of the electrode are improved, and high conductivity and The preparation of adhesive lithium polyacrylate improves the performance of lithium-ion batteries.

CN118146411BActive Publication Date: 2024-10-22GREEN ENERGY FIBER MATERIAL (CHONGQING) TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410270666.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-11
Publication Date
2024-10-22
Estimated Expiration
2044-03-11

AI Technical Summary

Technical Problem

In the existing preparation method of lithium polyacrylate, the hydrogen bonds of the carboxyl groups cause the molecular chains to be tightly cross-linked, which hinders the reaction of lithium ions and the improvement of electrode performance. At the same time, it is difficult to withstand the stress caused by the volume expansion of the active material, which affects the battery performance.

Method used

Sodium polyacrylate is used as raw material, acidified and modified, and then reacted with lithium hydroxide. The electrostatic repulsion of sodium ions stretches the molecular chain, promotes the free movement of lithium ions, and increases the reaction rate through the exchange reaction of lithium ions and hydrogen ions. Forms a more stable lithium polyacrylate.

Benefits of technology

It improves the conductivity, adhesion and stability of lithium polyacrylate, enhances the conductivity and flexibility of the electrode sheet, can better withstand the stress caused by the volume expansion of lithium ions, and improves the overall performance of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118146411B_ABST
    Figure CN118146411B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of preparation of adhesives for lithium ion batteries, and provides a preparation method of lithium polyacrylate, firstly, ethanol and concentrated sulfuric acid are mixed to prepare acid wine; sodium polyacrylate powder is added, and the mixture is washed after constant temperature reaction to obtain partially acidified sodium polyacrylate; the partially acidified sodium polyacrylate is then mixed with lithium hydroxide solution, heated, stirred and reacted in ethanol, so that the acidified modified part of the sodium polyacrylate is neutralized with the lithium hydroxide solution, washed with ethanol and dried to obtain sodium-containing lithium polyacrylate solid; and the application of the lithium polyacrylate in lithium ion batteries is also provided. The invention significantly improves the conductivity, adhesion, stability and preparation efficiency of lithium polyacrylate, and the preparation process is simple, providing a convenient route for obtaining adhesives for lithium ion batteries with multiple enhanced properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of preparation of adhesives for lithium ion batteries, in particular to lithium polyacrylate and a preparation method and application thereof. Background Art

[0002] As early as 2006, polyacrylic acid (PAA) began to be used as a binder for lithium batteries. Polyacrylic acid is a linear long-chain structure with a large number of carboxyl groups. There are a large number of carboxylic acid groups in its structure. Its molecular chains form a cross-linked structure through hydrogen bonds, which can form a strong interaction with active materials or conductive agent particles, improve the bonding performance, and can also form a stable CEI film during the battery cycle, thereby improving the stability of the electrode. However, this structure still has limitations: First, a portion of the active Li will inevitably be consumed during the formation of the CEI film. + , resulting in a decrease in electrode performance; secondly, the linear long chain structure of PAA makes it easy for the molecular chains to slide, and it is easy to undergo permanent deformation after being subjected to force, resulting in agglomeration of active materials and reducing the conductivity of the electrode sheet. It can be seen that it is difficult for polyacrylic acid lithium battery binders to achieve a harmonious unity of their conductivity, adhesion and stability. Therefore, how to improve the structure or preparation method of polyacrylic acid lithium battery binders to improve the unity of their multiple properties is the focus of current research.

[0003] As a new type of solid binder material, lithium polyacrylate (PAA-Li) has both high non-crystalline and good mechanical properties. It can combine ionic conductivity and viscoelasticity of polymer materials very well, and has outstanding advantages in improving the performance of polyacrylate lithium battery binders. At present, there are related documents that disclose the preparation method of lithium polyacrylate. For example, in the prior art, patent number CN109251257A "lithium polyacrylate and its preparation method, use and lithium ion battery" directly mixes polyacrylic acid with lithium hydroxide to obtain the lithium polyacrylate; for example, patent number CN102250269A "a method for preparing lithium polyacrylate and a method for preparing a solid electrolyte membrane by mixing lithium polyacrylate with lithium salt" first uses acrylic acid and lithium hydroxide as raw materials to prepare lithium acrylate, and then polymerizes lithium acrylate to obtain lithium polyacrylate; for example, patent number CN116023563A "a method for synthesizing lithium polyacrylate using esterification wastewater containing acrylic acid" directly adds lithium hydroxide to esterification wastewater containing acrylic acid, polymerizes under controlled conditions under ultraviolet light irradiation, and then vacuum flash evaporation removes water to obtain a lithium polyacrylate solution. It can be seen that in the prior art, the synthesis of lithium polyacrylate is based on the reaction of polyacrylic acid and lithium hydroxide to obtain lithium polyacrylate. Its synthesis uses acrylic acid monomer and lithium hydroxide as raw materials. The synthesis process is nothing more than first mixing acrylic acid monomer and lithium hydroxide, first performing acid-base neutralization reaction and then polymerizing lithium acrylate; or first polymerizing acrylic acid monomer and then mixing with lithium hydroxide for acid-base neutralization reaction. However, when polyacrylic acid is used as a raw material, the hydrogen bonds generated by the presence of a large number of carboxyl groups make its own cross-linking tight, which not only hinders the free rotation of the molecular chain, but also hinders the reaction of lithium ions with it, that is, to a certain extent, the preparation efficiency of lithium polyacrylate is reduced. The tightly cross-linked structure is also not conducive to bearing the stress generated by the volume expansion of the active substance (lithium ions), thereby affecting the improvement of battery performance.

[0004] Therefore, in view of the many shortcomings of the preparation method of lithium polyacrylate, the present invention creatively uses sodium polyacrylate as a raw material, acidifies and modifies it, and then reacts it with lithium hydroxide, aiming to provide a lithium polyacrylate with high preparation efficiency and enhanced performance. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing lithium polyacrylate with high conductivity, good adhesion, strong stability and high preparation efficiency, so as to solve the problems raised in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing lithium polyacrylate comprises the following steps:

[0008] Step S1: Pour ethanol and concentrated sulfuric acid into a three-necked flask and stir for 10-15 minutes to mix evenly to obtain sour wine;

[0009] Step S2: adding sodium polyacrylate powder to the sour wine obtained in step S1, reacting for 2-3 hours under stirring conditions in a constant temperature water bath at 30-45°C, washing with ethanol, and obtaining partially acidified modified sodium polyacrylate;

[0010] Step S3: accurately weighing lithium hydroxide solid, and preparing a lithium hydroxide solution under stirring;

[0011] Step S4: mixing the partially acidified modified sodium polyacrylate obtained in step S2 and the lithium hydroxide solution obtained in step S3, adding ethanol, reacting at 30-50° C. with stirring for 2-3 hours to neutralize the acidified modified part of the sodium polyacrylate with the lithium hydroxide solution, washing with ethanol until the pH is 7-9, and drying to obtain a sodium-containing lithium polyacrylate solid.

[0012] Preferably, the mass ratio of ethanol to concentrated sulfuric acid in step S1 is (0.12-0.15):8.

[0013] Preferably, the molecular weight of the sodium polyacrylate in step S2 is 800,000-35,000,000.

[0014] Preferably, the acidification degree of the partially acid-modified sodium polyacrylate in step S2 is 60-75%.

[0015] Preferably, the concentration of the lithium hydroxide solution in step S3 is 0.8-1.2 mol / L.

[0016] Preferably, the molar ratio of the partially acid-modified sodium polyacrylate to lithium hydroxide in step S4 is 1:(0.5-2).

[0017] Preferably, the stirring rate is 110-150 r / min.

[0018] Preferably, the sodium content in the sodium-containing lithium polyacrylate solid in step S4 is 1-3%.

[0019] To achieve the above object, the present invention also provides lithium polyacrylate prepared by the above method.

[0020] To achieve the above object, the present invention also provides the use of lithium polyacrylate prepared by the above method in lithium ion batteries.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention creatively uses sodium polyacrylate as a raw material and provides a new preparation method of lithium polyacrylate: in the preparation process, sodium polyacrylate is firstly acidified and modified, and then lithium hydroxide is added, and the temperature is increased, and lithium ions in the solution enter into the cross-linked network structure of part of the acidified and modified sodium polyacrylate, and are exchanged with hydrogen ions in the carboxyl groups of the acidified and modified sodium polyacrylate. Since there is electrostatic repulsion between sodium ions in the long chain of sodium polyacrylate, the molecular chain is fully stretched, which is not only conducive to the free rotation of the molecular chain, but also can promote the free movement of lithium ions, improve the exchange rate of lithium ions and hydrogen ions, accelerate the reaction rate, and avoid the agglomeration of active substances to improve the conductivity of the electrode sheet; in addition, the radius of sodium ions is larger than the radius of lithium ions. In the preparation process, under heating, part of the sodium ions (whose activity is relatively low) are absorbed by water molecules in the solution and enter the solution system, and the sodium polyacrylate sites occupied by them are occupied by lithium ions with a smaller radius. Therefore, the formed lithium polyacrylate is more conducive to bearing the stress generated by the volume expansion of the active substance (lithium ions), thereby improving its stability. In summary, the present invention produces a lithium polyacrylate product having both high bonding strength and ionic conductivity, and improves the flexibility and stability of the lithium polyacrylate binder. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The present invention is a schematic flow chart of a method for preparing lithium polyacrylate. DETAILED DESCRIPTION

[0024] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] See also Figure 1 , the present invention provides:

[0026] Embodiment 1

[0027] A method for preparing lithium polyacrylate comprises the following steps:

[0028] Step S101: prepare 75% volume concentration of ethanol, accurately weigh concentrated sulfuric acid, pour them into a three-necked flask, stir at 110r / min for 10min, mix evenly (the mass ratio of ethanol to concentrated sulfuric acid is 0.12:8), and obtain sour wine.

[0029] Step S102: Add sodium polyacrylate powder with a molecular weight of 800,000 to the sour wine obtained in step S101, react for 3 hours under stirring in a constant temperature water bath at 30°C, wash with ethanol with a volume concentration of 90%, and obtain partially acidified sodium polyacrylate (acidity of 60%).

[0030] Step S103: Accurately weigh lithium hydroxide solid, and prepare a lithium hydroxide solution with a concentration of 0.8 mol / L under stirring.

[0031] Step S104: Mix the partially acid-modified sodium polyacrylate obtained in step S102 and the lithium hydroxide solution obtained in step S103 (the molar ratio of the partially acid-modified sodium polyacrylate to lithium hydroxide is 1:0.5), add ethanol with a volume concentration of 75%, and react for 3 hours at 30°C and 110r / min stirring conditions to neutralize the acid-modified part of the sodium polyacrylate with the lithium hydroxide solution, wash with ethanol with a volume concentration of 90% to a pH of 7, and obtain sodium-containing lithium polyacrylate solid (sodium content is 1%) after drying. Specific embodiment 2

[0033] A method for preparing lithium polyacrylate comprises the following steps:

[0034] Step S201: prepare ethanol with a volume concentration of 85%, then accurately weigh concentrated sulfuric acid, pour them into a three-necked flask, stir at 150 r / min for 15 minutes, mix them evenly (the mass ratio of ethanol to concentrated sulfuric acid is 0.15:8), and obtain sour wine.

[0035] Step S202: Add sodium polyacrylate powder with a molecular weight of 35 million to the sour wine obtained in step S201, react for 2 hours under stirring in a constant temperature water bath at 45°C, wash with ethanol with a volume concentration of 95%, and obtain partially acidified sodium polyacrylate (acidity of 75%).

[0036] Step S203: Accurately weigh lithium hydroxide solid, and prepare a lithium hydroxide solution with a concentration of 1.2 mol / L under stirring.

[0037] Step S204: Mix the partially acid-modified sodium polyacrylate obtained in step S202 and the lithium hydroxide solution obtained in step S203 (the molar ratio of the partially acid-modified sodium polyacrylate to lithium hydroxide is 1:2), add ethanol with a volume concentration of 85%, and react for 2 hours at 50° C. and 150 r / min stirring conditions to neutralize the acid-modified part of the sodium polyacrylate with the lithium hydroxide solution, wash with ethanol with a volume concentration of 95% to a pH of 9, and obtain sodium-containing lithium polyacrylate solid (sodium content is 3%) after drying. Specific embodiment 3

[0039] A method for preparing lithium polyacrylate comprises the following steps:

[0040] Step S301: prepare 78% volume concentration of ethanol, accurately weigh concentrated sulfuric acid, pour them into a three-necked flask, stir at 120r / min for 12min, mix evenly (the mass ratio of ethanol to concentrated sulfuric acid is 0.122:8), and obtain sour wine.

[0041] Step S302: Add sodium polyacrylate powder with a molecular weight of 24 million to the sour wine obtained in step S301, react for 2 hours under stirring in a constant temperature water bath at 35°C, wash with ethanol with a volume concentration of 95%, and obtain partially acidified sodium polyacrylate (acidity of 68%).

[0042] Step S303: Accurately weigh lithium hydroxide solid, and prepare a lithium hydroxide solution with a concentration of 0.9 mol / L under stirring.

[0043] Step S304: Mix the partially acid-modified sodium polyacrylate obtained in step S302 and the lithium hydroxide solution obtained in step S303 (the molar ratio of the partially acid-modified sodium polyacrylate to the lithium hydroxide is 1:1), add ethanol with a volume concentration of 78%, and react for 3 hours at 40° C. and 120 r / min stirring conditions to neutralize the acid-modified part of the sodium polyacrylate with the lithium hydroxide solution, wash with ethanol with a volume concentration of 95% to a pH of 8, and obtain sodium-containing lithium polyacrylate solid (sodium content is 2%) after drying. Specific embodiment 4

[0045] Application of lithium polyacrylate prepared by the above method in lithium ion batteries.

[0046] The relevant properties of the lithium polyacrylate prepared in specific examples 1 to 3 were tested (including the control group: polyacrylic acid adhesive), and the test results are shown in Table 1:

[0047] Table 1 Detection data of lithium polyacrylate obtained in each embodiment

[0048]

[0049] It can be seen from Table 1 that the conductivity of the lithium polyacrylate prepared in the present invention is higher than 6.5×10 -5 S cm -1 That is, the preparation method designed by the present invention significantly improves the ionic conductivity of lithium polyacrylate (higher than the highest room temperature ionic conductivity of lithium polyacrylate in the reference document CN102250269A, which is 6.0×10 -5 S cm -1). The peel strength of the lithium polyacrylate prepared by the present invention is close to that of polyacrylic acid, which means that the addition of lithium ions to polyacrylic acid does not change the overall basic structure of polyacrylic acid, and its bonding performance does not change, thus maintaining the excellent bonding performance of the polyacrylic acid adhesive. In addition, the glass transition temperature of lithium polyacrylate is measured to be 68-72°C, which is significantly lower than 106°C of polyacrylic acid, indicating that the flexibility of the lithium polyacrylate prepared by the present invention has been significantly improved, which is beneficial to its application in lithium ion battery adhesives.

[0050] It can be seen from the above embodiments that the present invention uses sodium polyacrylate as a raw material and provides a new method for preparing lithium polyacrylate: in the preparation process, sodium polyacrylate is firstly acidified and modified, and then lithium hydroxide is added, and the temperature is increased, and the lithium ions in the solution enter the partially acidified and modified sodium polyacrylate cross-linked network structure and exchange with the hydrogen ions in the acidified and modified sodium polyacrylate carboxyl group. Since there is electrostatic repulsion between the sodium ions in the long chain of sodium polyacrylate, the molecular chain is fully stretched, which is not only conducive to the free rotation of the molecular chain, but also can promote the free activity of lithium ions, improve the exchange rate of lithium ions and hydrogen ions, accelerate the reaction rate, and avoid the agglomeration of active substances to improve the conductivity of the electrode sheet; in addition, the radius of sodium ions is larger than the radius of lithium ions. During the preparation process, under heating, part of the sodium ions (whose activity is relatively low) are absorbed by the water molecules in the solution and enter the solution system, and the sodium polyacrylate sites occupied by them are occupied by lithium ions with a smaller radius. Therefore, the formed lithium polyacrylate is more conducive to bearing the stress generated by the volume expansion of the active substance (lithium ions), thereby improving its stability. In summary, the present invention produces a lithium polyacrylate product having both high bonding strength and ionic conductivity, and improves the flexibility and stability of the lithium polyacrylate binder.

[0051] The polyacrylate lithium (PAA-Li) prepared by the present invention is obtained by the H between the carboxyl "hydrogen" and the carboxyl "lithium". + / Li + The reversible exchange reaction effectively assists Li + transport at the electrode interface, which is beneficial to the construction of Li +The conductive path will not cause significant decomposition of the electrolyte, which helps to improve the electrochemical performance of the electrode and effectively solves the defects such as low rate performance. PAA-Li is a water-soluble lithium battery binder containing lithium ions. Using water as a dispersant, it can better disperse the electrode material, make the electrode material particles relatively evenly distributed, and make the conductivity and flexibility better. The mechanical and stability become stronger, which is conducive to improving the electrochemical performance of the battery. In addition, the overall process is simple, and the performance of the final product is good, achieving a synergistic effect. It can supplement the consumption of active lithium in the battery during the cycle and improve the comprehensive performance of the lithium battery. It can also effectively inhibit the leakage and pyroelectric problems caused by oxidation, so that lithium batteries can be widely used in various fields such as automotive batteries, power tools, and mobile phone batteries. Therefore, lithium polyacrylate is a conductive polymer material with application prospects, and its development prospects are very broad and bright.

[0052] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing lithium polyacrylate, characterized in that: The following steps are involved: Step S1: Pour ethanol and concentrated sulfuric acid in a mass ratio of (0.12-0.15):8 into a three-necked flask and stir for 10-15 minutes to mix evenly to obtain sour wine; Step S2: adding sodium polyacrylate powder to the sour wine obtained in step S1, reacting for 2-3 hours in a constant temperature water bath at 30-45°C with stirring, washing with ethanol to obtain partially acidified sodium polyacrylate, wherein the acidification degree of the partially acidified sodium polyacrylate is 60-75%; Step S3: accurately weighing lithium hydroxide solid, and preparing a lithium hydroxide solution under stirring; Step S4: mixing the partially acidified modified sodium polyacrylate obtained in step S2 and the lithium hydroxide solution obtained in step S3 at a molar ratio of 1:(0.5-2), adding ethanol, reacting at 30-50°C and stirring for 2-3h to neutralize the acidified modified part of the sodium polyacrylate with the lithium hydroxide solution, washing with ethanol until the H is 7-9, and drying to obtain a sodium-containing lithium polyacrylate solid, wherein the sodium content of the sodium-containing lithium polyacrylate solid is 1-3%.

2. The method for preparing lithium polyacrylate according to claim 1, characterized in that: The molecular weight of the sodium polyacrylate in step S2 is 800,000 to 35,000,000.

3. The method for preparing lithium polyacrylate according to claim 1, characterized in that: The concentration of the lithium hydroxide solution in step S3 is 0.8-1.2 mol / L.

4. The method for preparing lithium polyacrylate according to claim 1, characterized in that: The stirring rate is 110-150 r / min.

5. Lithium polyacrylate obtained by the method according to any one of claims 1 to 4.

6. Use of the lithium polyacrylate prepared by the method according to any one of claims 1 to 4 or the lithium polyacrylate according to claim 5 in lithium ion batteries.