A safe, environmentally friendly, flame-retardant polystyrene board and a manufacturing method thereof

By using a modified flame retardant, combined with azide-alkynyl reaction and magnesium hydroxide, the poor combustion performance of polystyrene plates in fires was solved, significantly improved flame retardant performance and mechanical properties, and reduced environmental pollution and flames. spread.

CN118146593BActive Publication Date: 2024-11-12QINGDAO WANXING BUILDING MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410261728.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-07
Publication Date
2024-11-12
Estimated Expiration
2044-03-07

AI Technical Summary

Technical Problem

Existing polystyrene plates have poor combustion performance in fires. Thermoplastic materials will shrink, melt and flow when exposed to fire. The flame spreads rapidly. The existing flame retardants have a great impact on the mechanical properties of the materials or cause environmental pollution.

Method used

Modified flame retardant is prepared by alkynyl-containing cyclotriphosphazene, azide silica aerogel and magnesium sulfate. The modified silica aerogel is formed through azide-alkynyl reaction, and combined with hydroxide Magnesium improves the flame retardant properties and mechanical properties of polystyrene plates, and prepares safe and environmentally friendly flame retardant polystyrene plates through extrusion molding process.

Benefits of technology

The flame retardant and mechanical properties of polystyrene plates are significantly improved, flame spread and smoke generation are reduced, environmental pollution is reduced, and the compatibility and dispersion of silica aerogels and polystyrene resins are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004731119650000111
    Figure BDA0004731119650000111
  • Figure BDA0004731119650000121
    Figure BDA0004731119650000121
Patent Text Reader

Abstract

The present invention discloses a safe, environmentally friendly, flame-retardant polystyrene board and a method for making the same. The safe, environmentally friendly, flame-retardant polystyrene board comprises the following raw materials: polystyrene resin, compatibilizer, fiber, flame retardant, foaming agent, and other additives. The present invention also provides a method for making the same. Compared with the prior art, the present invention introduces a flame retardant, which not only improves the compatibility of silica aerogel with polystyrene resin, but also improves the dispersibility of silica aerogel, and increases the flame retardancy and mechanical properties of the polystyrene board.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polystyrene boards, and in particular to a safe, environmentally friendly, flame-retardant polystyrene board and a manufacturing method thereof. Background Art

[0002] The full name of polystyrene board is polystyrene foam board, also known as foam board or EPS board. It is made of expandable polystyrene beads containing volatile liquid foaming agent that are pre-expanded by heating and then heated in a mold to form white foam with a fine closed-cell structure. It can be used for building wall and roof insulation, insulation layer of composite insulation boards, insulation materials for vehicle and ship refrigeration equipment and refrigerated trucks; and for decoration and carving of various models.

[0003] However, it is a thermoplastic material, which will shrink, melt, and flow when exposed to fire. The flame will spread too quickly and the burn area will be too large. The combustion process is accompanied by thick smoke, which seriously pollutes the environment and threatens human health.

[0004] However, in the prior art, flame retardants for inorganic materials such as magnesium hydroxide have low flame retardant efficiency and need to be added in large quantities to achieve flame retardant effects. However, the addition of large amounts of inorganic flame retardants will affect the mechanical properties of the materials. Although flame retardants containing halogens such as bromine have excellent flame retardant properties, they will produce difficult-to-degrade products such as dioxins when burned, causing serious environmental pollution and endangering human health.

[0005] CN114479299A discloses a flame retardant polystyrene board and a preparation method thereof, wherein the flame retardant polystyrene board is prepared by double coating of polystyrene particles, wherein the polystyrene particles are coated with a composition of a silicate system for the first time, and the polystyrene particles are coated with a composition of a thermosetting resin system for the second time. After the first coating, the silicate system composition inorganically modifies the interface of the polystyrene particles, thereby improving the flame retardant ability of the polystyrene particles, and the polystyrene particles are coated with a thermosetting resin composition for the second time and bonded into a board, thereby improving the flame retardant performance of the polystyrene board. However, silicates and inorganic fillers are easy to precipitate in the coating agent, and it is difficult to apply them evenly during the coating process, and thus the flame retardant effect cannot be produced well. Therefore, the present application proposes a safe and environmentally friendly flame retardant polystyrene board and a preparation method thereof. Summary of the invention

[0006] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is a safe, environmentally friendly, flame-retardant polystyrene board;

[0007] To achieve the above-mentioned purpose, the present invention provides a safe, environmentally friendly, flame-retardant polystyrene board, characterized in that it comprises the following raw materials: 80-100 parts by weight of polystyrene resin, 0.1-3 parts by weight of compatibilizer, 5-10 parts by weight of fiber, 8-12 parts by weight of flame retardant, 5-10 parts by weight of foaming agent, and 0.1-5 parts by weight of other additives.

[0008] The other auxiliary agents may be antioxidants, ultraviolet absorbers, lubricants, etc., which may be adjusted and added as needed.

[0009] The fiber is at least one of carbon fiber, potassium titanate whisker, glass fiber, rock wool fiber and polytetrafluoroethylene fiber.

[0010] Furthermore, the fiber may be modified with a silane coupling agent, a surfactant, or a titanate coupling agent.

[0011] The compatibilizer is a copolymer of styrene and maleic anhydride;

[0012] The foaming agent is at least one of pentane or butane.

[0013] The preparation method of the flame retardant is:

[0014] Add cyclotriphosphazene containing an alkynyl group, azide silica aerogel, ascorbic acid and copper sulfate to N,N-dimethylformamide, heat to 70-85°C for reaction for 1-5h under a nitrogen atmosphere, centrifuge, wash and dry after the reaction to obtain a modified silica aerogel;

[0015] The modified silica aerogel and magnesium sulfate are added into water for ultrasonic treatment for 5-15 minutes, and then 1-5% ammonia water is added to adjust the pH to 8-9, and the mixture is allowed to stand at room temperature for 24 hours. After the reaction is completed, the mixture is centrifuged, washed with water until neutral, and dried to obtain a flame retardant.

[0016] The preparation method of the alkynyl-containing cyclotriphosphazene comprises: adding hexa(4-hydroxyphenoxy)cyclotriphosphazene, 3-bromopropyne and anhydrous potassium carbonate into acetone and mixing evenly, heating and refluxing, filtering after the reaction, removing the solvent by rotary evaporation, purifying and drying to obtain the alkynyl-containing cyclotriphosphazene;

[0017] The preparation method of the azide silica aerogel is as follows: adding silica aerogel to toluene and mixing evenly, then adding halogenated siloxane, heating to 80-90° C. for reaction for 20-24 hours, filtering after the reaction, washing the precipitate, and drying to obtain the halogenated nano silica aerogel; adding halogenated silica aerogel and sodium azide to N,N-dimethylamide and mixing evenly, heating to 70-85° C., reacting in a nitrogen atmosphere for 20-24 hours, filtering after the reaction, washing the precipitate, and drying to obtain the azide silica aerogel.

[0018] Furthermore, the preparation method of the flame retardant is:

[0019] 0.1-1 parts by weight of hexa(4-hydroxyphenoxy)cyclotriphosphazene, 0.5-1.5 parts by weight of 3-bromopropyne, and 0.5-1.5 parts by weight of anhydrous potassium carbonate are added to 50-60 parts by weight of acetone and mixed evenly, heated under reflux for 10-20 hours, filtered after the reaction, the solvent is removed by rotary evaporation, purified, and dried to obtain cyclotriphosphazene containing an alkynyl group;

[0020] 1-2 parts by weight of silica aerogel are added to 50-100 parts by weight of toluene and mixed evenly, then 0.5-1 parts by weight of halogenated siloxane are added, and the mixture is heated to 80-90° C. and reacted for 20-24 hours. After the reaction is completed, the mixture is filtered, the precipitate is washed, and dried to obtain halogenated nano silica aerogel; 1-2 parts by weight of halogenated silica aerogel and 0.1-1 parts by weight of sodium azide are added to 150-200 parts by weight of N,N-dimethylamide and mixed evenly, and the mixture is heated to 75-80° C. and reacted under a nitrogen atmosphere for 20-24 hours. After the reaction is completed, the mixture is filtered, the precipitate is washed, and dried to obtain azide silica aerogel;

[0021] 0.5-1 parts by weight of cyclotriphosphazene containing an alkynyl group, 0.5-2 parts by weight of azide silica aerogel, 0.1-1 parts by weight of ascorbic acid, and 0.1-0.5 parts by weight of copper sulfate are added to 50-100 parts by weight of N,N-dimethylformamide, heated to 70-85° C. under a nitrogen atmosphere for reaction for 1-5 hours, and after the reaction is completed, centrifuged, washed, and dried to obtain a modified silica aerogel;

[0022] 1-2 parts by weight of modified silica aerogel and 5-10 parts by weight of magnesium sulfate are added to 50-100 parts by weight of water for ultrasonic treatment for 5-15 minutes, and then 1-5% ammonia water is added to adjust the pH to 8-9, and the mixture is allowed to stand at room temperature for 24 hours. After the reaction is completed, the mixture is centrifuged, washed with water until neutral, and dried to obtain a flame retardant.

[0023] The halogenated siloxane is 3-bromopropyltrichlorosilane.

[0024] The interior of the silica aerogel is a material with a spatial network structure. The aerogel fully utilizes its nanoporous structure to provide a good barrier to solid heat transfer and air convection heat transfer, and can also effectively block infrared radiation heat transfer. At the same time, the main component of the silica aerogel is silica, which has a non-flammable effect. However, the silica aerogel has poor dispersibility in resins and its flame retardant properties need to be further improved. The present application uses halogenated siloxanes and sodium azide as raw materials to modify the silica aerogel to prepare azidized silica aerogel, and uses hexa(4-hydroxyphenoxy)cyclotriphosphazene prepared by the prior art as a raw material to react with 3-bromopropyne to prepare alkynyl-containing cyclotriphosphazene. The modified silica aerogel is prepared by azide-alkynyl reaction, i.e., cyclotriphosphazene-modified silica aerogel. Cyclotriphosphazene is a type of inorganic heterocyclic structure with alternating phosphorus and nitrogen single and double bonds, in which the nitrogen and phosphorus contents are very high, and a large amount of heat can be absorbed during decomposition, which has a great impact on the material. It plays a cooling role; the phosphoric acid, metaphosphoric acid and polyphosphoric acid generated by thermal decomposition form a non-volatile protective film on the surface of the material, isolating the air; CO2, NH3, N2, and H2O gases are released after heating, which not only dilute the concentration of combustibles, but also block the supply of oxygen, achieving the purpose of flame retardant synergy and synergy, and PO· free radicals are formed during combustion, which can combine with free radicals in the flame area to inhibit the flame. The triazole ring group formed by the azide group and the alkynyl group has the characteristics of high-temperature carbonization under high temperature conditions, and effectively protects the polystyrene resin from further combustion. The phosphorus element and triazole ring contained therein have the effect of expansion and accumulation of flame retardancy; finally, the modified silica aerogel adsorbs magnesium sulfate to prepare a modified silica aerogel containing magnesium hydroxide. Magnesium hydroxide can absorb a large amount of heat during high-temperature combustion, reduce the temperature of the surface of the burning object, and thus reduce the release of volatile gases of organic combustibles.

[0025] The invention also discloses a method for manufacturing a safe, environmentally friendly and flame-retardant polystyrene board.

[0026] A method for manufacturing a safe, environmentally friendly, flame-retardant polystyrene board comprises the following steps:

[0027] Step 1, according to the formula, the raw materials are mixed evenly to obtain a blend;

[0028] Step 2, feeding the blended material into an extruder for melt extrusion, pressurized extrusion, strand cooling, and pelletizing to obtain pellets;

[0029] Step 3: Evenly mix the above particles with the foaming agent, and then add them into an extruder for extrusion molding to obtain a polystyrene board, and obtain a safe, environmentally friendly and flame-retardant polystyrene board after aging and curing.

[0030] Furthermore, the extruder in step 3 is a twin-screw extruder, wherein the temperature range of each zone is 195-250° C., and the rotation speed is 300-900 rpm.

[0031] Beneficial effects of the present invention:

[0032] Compared with the prior art, the invention introduces a flame retardant, which not only improves the compatibility of silica aerogel and polystyrene resin, but also improves the dispersibility of silica aerogel and increases the flame retardancy and mechanical properties of the polystyrene board. DETAILED DESCRIPTION

[0033] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0034] Introduction of some raw materials used in the embodiments of the present invention:

[0035] Polystyrene resin, brand name GPS-525N, Dongguan Hongchuang Plastic Co., Ltd.

[0036] Copolymer of styrene and maleic anhydride, molecular weight: 20,000, Shanghai Myrrel Chemical Technology Co., Ltd.

[0037] Carbon fiber, nanoscale, OD: 150-200nm, length: 10-30 microns, Zhejiang Yamei Nanotechnology Co., Ltd.

[0038] The silica aerogel was prepared by referring to the preparation method of Example 1 in patent CN103708476B.

[0039] The preparation method of hexa(4-hydroxyphenoxy)cyclotriphosphazene is prepared by referring to the preparation method of Example 1 in patent CN111153939A.

[0040] Other raw materials not mentioned are common raw materials in the art. The above content is only to help illustrate the present invention and should not be construed as a strict limitation of the present invention. Those skilled in the art can directly purchase or prepare the same / similar raw materials from the market. These contents will not be repeated in the examples.

[0041] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Example 1

[0043] A method for manufacturing a safe, environmentally friendly, flame-retardant polystyrene board comprises the following steps:

[0044] Step 1, according to the formula, 100 parts by weight of polystyrene resin, 3 parts by weight of a copolymer of styrene and maleic anhydride, 8 parts by weight of carbon fiber, 10 parts by weight of silica aerogel, and 1 part by weight of antioxidant 1010 are mixed uniformly to obtain a blend;

[0045] Step 2, feeding the blended material into an extruder for melt extrusion, pressurized extrusion, strand cooling, and pelletizing to obtain pellets;

[0046] Step 3, mix the above particles evenly with 10 parts by weight of pentane, then add them into a twin-screw extruder for extrusion molding to obtain a polystyrene board, and obtain a safe, environmentally friendly and flame-retardant polystyrene board after aging and curing, wherein the twin-screw extruder has a temperature of 220°C in zone 1, 225°C in zone 2, 230°C in zone 3, 235°C in zone 4, 238°C in zone 5, and a rotation speed of 500rpm.

[0047] Example 2

[0048] A method for manufacturing a safe, environmentally friendly, flame-retardant polystyrene board comprises the following steps:

[0049] Step 1: According to the formula, 100 parts by weight of polystyrene resin, 3 parts by weight of a copolymer of styrene and maleic anhydride, 8 parts by weight of modified carbon fiber, 10 parts by weight of silica aerogel, and 1 part by weight of antioxidant 1010 are mixed uniformly to obtain a blend;

[0050] The preparation method of the modified carbon fiber is as follows: 2 parts by weight of methyltrimethoxysilane and 8 parts by weight of carbon fiber are added to 100 parts by weight of 75wt% ethanol aqueous solution and mixed evenly, heated to 85°C for reaction for 3h, and after the reaction is completed, centrifuged to obtain a precipitate, washed, and dried to obtain the modified carbon fiber;

[0051] Step 2, feeding the blended material into an extruder for melt extrusion, pressurized extrusion, strand cooling, and pelletizing to obtain pellets;

[0052] Step 3, mix the above particles evenly with 10 parts by weight of pentane, then add them into a twin-screw extruder for extrusion molding to obtain a polystyrene board, and obtain a safe, environmentally friendly and flame-retardant polystyrene board after aging and curing, wherein the twin-screw extruder has a temperature of 220°C in zone 1, 225°C in zone 2, 230°C in zone 3, 235°C in zone 4, 238°C in zone 5, and a rotation speed of 500rpm.

[0053] Example 3

[0054] A method for manufacturing a safe, environmentally friendly, flame-retardant polystyrene board comprises the following steps:

[0055] Step 1: According to the formula, 100 parts by weight of polystyrene resin, 3 parts by weight of a copolymer of styrene and maleic anhydride, 8 parts by weight of modified carbon fiber, 10 parts by weight of a flame retardant, and 1 part by weight of an antioxidant 1010 are uniformly mixed to obtain a blend;

[0056] The preparation method of the modified carbon fiber is as follows: 2 parts by weight of methyltrimethoxysilane and 8 parts by weight of carbon fiber are added to 100 parts by weight of 75wt% ethanol aqueous solution and mixed evenly, heated to 85°C for reaction for 3h, and after the reaction is completed, centrifuged to obtain a precipitate, washed, and dried to obtain the modified carbon fiber;

[0057] Step 2, feeding the blended material into an extruder for melt extrusion, pressurized extrusion, strand cooling, and pelletizing to obtain pellets;

[0058] Step 3, mix the above particles evenly with 10 parts by weight of pentane, then add them into a twin-screw extruder for extrusion molding to obtain a polystyrene board, and obtain a safe, environmentally friendly and flame-retardant polystyrene board after aging and curing, wherein the twin-screw extruder has a temperature of 220°C in zone 1, 225°C in zone 2, 230°C in zone 3, 235°C in zone 4, 238°C in zone 5, and a rotation speed of 500rpm.

[0059] The preparation method of the flame retardant is:

[0060] 0.8 parts by weight of hexa(4-hydroxyphenoxy)cyclotriphosphazene, 1 part by weight of 3-bromopropyne, and 0.78 parts by weight of anhydrous potassium carbonate were added to 50 parts by weight of acetone and mixed evenly, and heated under reflux for 15 hours. After the reaction was completed, the solvent was removed by filtration, purified, and dried to obtain an alkynyl-containing cyclotriphosphazene;

[0061] 2 parts by weight of silica aerogel are added to 100 parts by weight of toluene and mixed evenly, then 1 part by weight of 3-bromopropyltrichlorosilane is added, and the mixture is heated to 85° C. and reacted for 24 hours. After the reaction is completed, the mixture is filtered, the precipitate is washed, and dried to obtain halogenated nano silica aerogel; 2 parts by weight of halogenated silica aerogel and 1 part by weight of sodium azide are added to 160 parts by weight of N,N-dimethylamide and mixed evenly, and the mixture is heated to 80° C. and reacted for 24 hours under a nitrogen atmosphere. After the reaction is completed, the mixture is filtered, the precipitate is washed, and dried to obtain azide silica aerogel;

[0062] 1 part by weight of cyclotriphosphazene containing an alkynyl group, 2 parts by weight of azide silica aerogel, 0.8 parts by weight of ascorbic acid, and 0.3 parts by weight of copper sulfate are added to 90 parts by weight of N,N-dimethylformamide, and the mixture is heated to 85° C. under a nitrogen atmosphere for reaction for 3 hours. After the reaction is completed, the mixture is centrifuged, washed, and dried to obtain a modified silica aerogel;

[0063] 2 parts by weight of modified silica aerogel and 10 parts by weight of magnesium sulfate were added to 100 parts by weight of water and ultrasonically treated for 10 minutes, wherein the ultrasonic power was 300 W and the ultrasonic frequency was 15 kHz, and then 2% ammonia water was added to adjust the pH to 8.5, and the mixture was allowed to stand at room temperature for 24 hours. After the reaction was completed, the mixture was centrifuged, washed with water until neutral, and dried to obtain a flame retardant.

[0064] Example 4

[0065] A method for manufacturing a safe, environmentally friendly, flame-retardant polystyrene board comprises the following steps:

[0066] Step 1: According to the formula, 100 parts by weight of polystyrene resin, 3 parts by weight of a copolymer of styrene and maleic anhydride, 8 parts by weight of modified carbon fiber, 10 parts by weight of a flame retardant, and 1 part by weight of an antioxidant 1010 are uniformly mixed to obtain a blend;

[0067] The preparation method of the modified carbon fiber is as follows: 2 parts by weight of methyltrimethoxysilane and 8 parts by weight of carbon fiber are added to 100 parts by weight of 75wt% ethanol aqueous solution and mixed evenly, heated to 85°C for reaction for 3h, and after the reaction is completed, centrifuged to obtain a precipitate, washed, and dried to obtain the modified carbon fiber;

[0068] Step 2, feeding the blended material into an extruder for melt extrusion, pressurized extrusion, strand cooling, and pelletizing to obtain pellets;

[0069] Step 3, mix the above particles evenly with 10 parts by weight of pentane, then add them into a twin-screw extruder for extrusion molding to obtain a polystyrene board, and obtain a safe, environmentally friendly and flame-retardant polystyrene board after aging and curing, wherein the twin-screw extruder has a temperature of 220°C in zone 1, 225°C in zone 2, 230°C in zone 3, 235°C in zone 4, 238°C in zone 5, and a rotation speed of 500rpm.

[0070] The preparation method of the flame retardant is:

[0071] 0.8 parts by weight of hexa(4-hydroxyphenoxy)cyclotriphosphazene, 1 part by weight of 3-bromopropyne, and 0.78 parts by weight of anhydrous potassium carbonate were added to 50 parts by weight of acetone and mixed evenly, and heated under reflux for 15 hours. After the reaction was completed, the solvent was removed by filtration, purified, and dried to obtain an alkynyl-containing cyclotriphosphazene;

[0072] 2 parts by weight of silica aerogel are added to 100 parts by weight of toluene and mixed evenly, then 1 part by weight of 3-bromopropyltrichlorosilane is added, and the mixture is heated to 85° C. and reacted for 24 hours. After the reaction is completed, the mixture is filtered, the precipitate is washed, and dried to obtain halogenated nano silica aerogel; 2 parts by weight of halogenated silica aerogel and 1 part by weight of sodium azide are added to 160 parts by weight of N,N-dimethylamide and mixed evenly, and the mixture is heated to 80° C. and reacted for 24 hours under a nitrogen atmosphere. After the reaction is completed, the mixture is filtered, the precipitate is washed, and dried to obtain azide silica aerogel;

[0073] 1 part by weight of alkynyl-containing cyclotriphosphazene, 2 parts by weight of azide silica aerogel, 0.8 parts by weight of ascorbic acid and 0.3 parts by weight of copper sulfate were added to 90 parts by weight of N,N-dimethylformamide, heated to 85°C under a nitrogen atmosphere for reaction for 3 hours, and after the reaction was completed, centrifuged, washed and dried to obtain a flame retardant.

[0074] Example 5

[0075] A method for manufacturing a safe, environmentally friendly, flame-retardant polystyrene board comprises the following steps:

[0076] Step 1: According to the formula, 100 parts by weight of polystyrene resin, 3 parts by weight of a copolymer of styrene and maleic anhydride, 8 parts by weight of modified carbon fiber, 10 parts by weight of a flame retardant, and 1 part by weight of an antioxidant 1010 are uniformly mixed to obtain a blend;

[0077] The preparation method of the modified carbon fiber is as follows: 2 parts by weight of methyltrimethoxysilane and 8 parts by weight of carbon fiber are added to 100 parts by weight of 75wt% ethanol aqueous solution and mixed evenly, heated to 85°C for reaction for 3h, and after the reaction is completed, centrifuged to obtain a precipitate, washed, and dried to obtain the modified carbon fiber;

[0078] Step 2, feeding the blended material into an extruder for melt extrusion, pressurized extrusion, strand cooling, and pelletizing to obtain pellets;

[0079] Step 3, mix the above particles evenly with 10 parts by weight of pentane, then add them into a twin-screw extruder for extrusion molding to obtain a polystyrene board, and obtain a safe, environmentally friendly and flame-retardant polystyrene board after aging and curing, wherein the twin-screw extruder has a temperature of 220°C in zone 1, 225°C in zone 2, 230°C in zone 3, 235°C in zone 4, 238°C in zone 5, and a rotation speed of 500rpm.

[0080] The preparation method of the flame retardant is:

[0081] 0.8 parts by weight of hexa(4-hydroxyphenoxy)cyclotriphosphazene, 1 part by weight of 3-bromopropyne and 0.78 parts by weight of anhydrous potassium carbonate were added to 50 parts by weight of acetone and mixed evenly, and heated under reflux for 15 hours. After the reaction was completed, the flame retardant was filtered, the solvent was removed by rotary evaporation, purified and dried to obtain a flame retardant.

[0082] Example 6

[0083] A method for manufacturing a safe, environmentally friendly, flame-retardant polystyrene board comprises the following steps:

[0084] Step 1: According to the formula, 100 parts by weight of polystyrene resin, 3 parts by weight of a copolymer of styrene and maleic anhydride, 8 parts by weight of modified carbon fiber, 10 parts by weight of a flame retardant, and 1 part by weight of an antioxidant 1010 are uniformly mixed to obtain a blend;

[0085] The preparation method of the modified carbon fiber is as follows: 2 parts by weight of methyltrimethoxysilane and 8 parts by weight of carbon fiber are added to 100 parts by weight of 75wt% ethanol aqueous solution and mixed evenly, heated to 85°C for reaction for 3h, and after the reaction is completed, centrifuged to obtain a precipitate, washed, and dried to obtain the modified carbon fiber;

[0086] Step 2, feeding the blended material into an extruder for melt extrusion, pressurized extrusion, strand cooling, and pelletizing to obtain pellets;

[0087] Step 3, mix the above particles evenly with 10 parts by weight of pentane, then add them into a twin-screw extruder for extrusion molding to obtain a polystyrene board, and obtain a safe, environmentally friendly and flame-retardant polystyrene board after aging and curing, wherein the twin-screw extruder has a temperature of 220°C in zone 1, 225°C in zone 2, 230°C in zone 3, 235°C in zone 4, 238°C in zone 5, and a rotation speed of 500rpm.

[0088] The preparation method of the flame retardant is:

[0089] 2 parts by weight of silica aerogel are added to 100 parts by weight of toluene and mixed evenly, then 1 part by weight of 3-bromopropyltrichlorosilane is added, and the mixture is heated to 85° C. and reacted for 24 hours. After the reaction is completed, the mixture is filtered, the precipitate is washed, and dried to obtain halogenated nano silica aerogel; 2 parts by weight of halogenated silica aerogel and 1 part by weight of sodium azide are added to 160 parts by weight of N,N-dimethylamide and mixed evenly, and the mixture is heated to 80° C. and reacted for 24 hours in a nitrogen atmosphere. After the reaction is completed, the mixture is filtered, the precipitate is washed, and dried to obtain a flame retardant.

[0090] Test Example 1

[0091] Test the impact strength with reference to GB / T 1843-2008 "Izod beam impact strength of plastics";

[0092] Table 1 Impact strength test results of safe, environmentally friendly and flame-retardant polystyrene boards

[0093] <![CDATA[Impact strength (KJ / m 2 )]]> Example 1 16.1 Example 2 16.6 Example 3 17.5 Example 5 17.0 Example 6 17.3

[0094] Refer to GB / T 29906-2013 "Molded polystyrene board thin plaster exterior wall insulation system materials" to test the tensile strength perpendicular to the board surface;

[0095] Table 2 Thermal conductivity test results of safe, environmentally friendly and flame-retardant polystyrene boards

[0096] Thermal conductivity 25℃W / (mk) Example 2 0.21 Example 3 0.15

[0097] Refer to GB / T2408-2008 "Determination of Combustion Performance of Plastics" to test oxygen index;

[0098] Table 3 Flame retardant test results of safe and environmentally friendly flame retardant polystyrene board

[0099]

[0100]

[0101] As shown in Tables 2-3, the polyphenylene board prepared in Example 3 has good thermal conductivity and flame retardancy. In Example 3, halogenated siloxane and sodium azide are used as raw materials to modify silica aerogel to prepare azidized silica aerogel, and hexa(4-hydroxyphenoxy)cyclotriphosphazene prepared by the prior art is used as a raw material to react with 3-bromopropyne to prepare cyclotriphosphazene containing alkynyl. The modified silica aerogel, i.e. cyclotriphosphazene-modified silica aerogel, is prepared by azide-alkynyl reaction. Cyclotriphosphazene is a type of inorganic heterocyclic structure with alternating phosphorus and nitrogen single and double bonds, in which the nitrogen and phosphorus content is very high, and a large amount of heat can be absorbed during decomposition, which has a cooling effect on the material; phosphoric acid, metaphosphoric acid and polyphosphoric acid generated by thermal decomposition form a non-volatile protective film on the surface of the material, isolating the air. Gas; CO2, NH3, N2, H2O gas is released after heating, which not only dilutes the concentration of combustibles, but also blocks the supply of oxygen, achieving the purpose of flame retardant synergy and synergy, and PO· free radicals are formed during combustion, which can combine with free radicals in the flame area to inhibit the flame. The triazole ring group formed by the azide group and the alkynyl group has the characteristics of high-temperature carbonization under high temperature conditions, and effectively protects the polystyrene resin from further combustion. The phosphorus element and triazole ring contained therein have the effect of expansion and accumulation of flame retardancy; finally, the modified silica aerogel adsorbs magnesium sulfate to prepare a modified silica aerogel containing magnesium hydroxide. Magnesium hydroxide can absorb a large amount of heat during high-temperature combustion, reduce the temperature of the surface of the burning object, and thus reduce the release of volatile gases of organic combustibles. At the same time, the compatibility and dispersibility of silica aerogel with polystyrene resin are improved.

[0102] The flame retardant performance of Example 3 is significantly better than that of Examples 4-6. The flame retardant prepared in Example 3 contains NP-Si and combines multiple substances to improve its flame retardant performance.

[0103] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A safe, environmentally friendly, flame-retardant polystyrene board. It is characterized in that The invention comprises the following raw materials: 80-100 parts by weight of polystyrene resin, 0.1-3 parts by weight of compatibilizer, 5-10 parts by weight of fiber, 8-12 parts by weight of flame retardant, 5-10 parts by weight of foaming agent and 0.1-5 parts by weight of auxiliary agent; The preparation method of the flame retardant is: Add cyclotriphosphazene containing an alkynyl group, azide silica aerogel, ascorbic acid and copper sulfate to N,N-dimethylformamide, heat to 70-85°C for reaction for 1-5h under a nitrogen atmosphere, centrifuge, wash and dry after the reaction to obtain a modified silica aerogel; The modified silica aerogel and magnesium sulfate are added to water for ultrasonic treatment for 5-15 minutes, and then 1-5% ammonia water is added to adjust the pH to 8-9, and the mixture is allowed to stand at room temperature for 24 hours. After the reaction is completed, the mixture is centrifuged, washed with water until neutral, and dried to obtain a flame retardant; The preparation method of the alkynyl-containing cyclotriphosphazene comprises: adding hexa(4-hydroxyphenoxy)cyclotriphosphazene, 3-bromopropyne and anhydrous potassium carbonate into acetone and mixing evenly, heating and refluxing, filtering after the reaction, removing the solvent by rotary evaporation, purifying and drying to obtain the alkynyl-containing cyclotriphosphazene; The preparation method of the azide silica aerogel is as follows: adding silica aerogel to toluene and mixing evenly, then adding halogenated siloxane, heating to 80-90° C. and reacting for 20-24 hours, filtering after the reaction, washing the precipitate, and drying to obtain halogenated nano silica aerogel; adding halogenated silica aerogel and sodium azide to N,N-dimethylformamide and mixing evenly, heating to 70-85° C. and reacting for 20-24 hours in a nitrogen atmosphere, filtering after the reaction, washing the precipitate, and drying to obtain the azide silica aerogel; The auxiliary agent is at least one of an antioxidant, an ultraviolet absorber and a lubricant.

2. The safe, environmentally friendly, flame-retardant polystyrene board according to claim 1, Features: The fiber is at least one of carbon fiber, potassium titanate whisker, glass fiber, rock wool fiber and polytetrafluoroethylene fiber.

3. The safe, environmentally friendly, flame-retardant polystyrene board according to claim 1, Features: The fiber is at least one of fibers modified by a silane coupling agent and a titanate coupling agent.

4. The safe, environmentally friendly, flame-retardant polystyrene board according to claim 1, Features: The compatibilizer is a copolymer of styrene and maleic anhydride.

5. The safe, environmentally friendly, flame-retardant polystyrene board according to claim 1, Features: The foaming agent is at least one of pentane and butane.

6. A method for preparing the safe, environmentally friendly, flame-retardant polystyrene board according to any one of claims 1 to 5, It is characterized in that The following steps are involved: Step 1, according to the formula, the raw materials are mixed evenly to obtain a blend; Step 2, feeding the blended material into an extruder for melt extrusion, pressurized extrusion, strand cooling, and pelletizing to obtain pellets; Step 3: Evenly mix the above particles with the foaming agent, and then add them into an extruder for extrusion molding to obtain a polystyrene board, and obtain a safe, environmentally friendly and flame-retardant polystyrene board after aging and curing.

7. The method for preparing the safe, environmentally friendly and flame-retardant polystyrene board according to claim 6, Features: The extruder in step 3 is a twin-screw extruder, wherein the temperature range of each zone is 195-250° C. and the rotation speed is 300-900 rpm.