A method for preparing sodium bismuth titanate nanowires with large aspect ratio

Through electrospinning and heat treatment, a large aspect ratio of bismuth sodium titanate nanowires were prepared, which solved the problem of poor continuity and flexibility of bismuth sodium titanate nanowires in hydrothermal preparation, and achieved high purity and uniformity and flexible electronics applications.

CN118147787BActive Publication Date: 2024-11-15SHANGHAI SECOND POLYTECHNIC UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410284202.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-13
Publication Date
2024-11-15
Estimated Expiration
2044-03-13

AI Technical Summary

Technical Problem

In the prior art, the preparation of sodium bismuth titanate nanowires by hydrothermal method has problems such as difficult to control the reaction degree, poor continuity of nanowire products, uneven sizes and poor flexibility, and few studies on electrospinning methods.

Method used

Electrostatic spinning method is used to prepare sodium bismuth titanate nanowires, which are mixed with titanium source, bismuth source, sodium source, acetic acid, acetylacetone, water, N,N-dimethylformamide and tackifier, and then stir evenly. Electrospinning and heat treatment were performed to obtain sodium bismuth titanate nanowires with a large aspect ratio.

Benefits of technology

The aspect ratio and flexibility of the bismuth titanate nanowires are improved, and the product has high purity, good continuity, uniform size and smooth surface, and is suitable for basic materials for flexible electronic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118147787B_ABST
    Figure CN118147787B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for preparing sodium bismuth titanate nanowires with a large aspect ratio, and belongs to the field of nanomaterial technology. The preparation method comprises the following steps: mixing a titanium source, a bismuth source, a sodium source, acetic acid, acetylacetone, water, N,N-dimethylformamide and a thickener, stirring evenly to obtain a precursor solution; electrospinning the precursor solution to obtain nanowires, and then heat-treating the nanowires to obtain the sodium bismuth titanate nanowires with a large aspect ratio. The preparation method can greatly improve the aspect ratio of the sodium bismuth titanate nanowires and improve their flexibility. The sodium bismuth titanate nanowires prepared by the method of the present invention can be used as the basic material of a new generation of flexible electronic products, so that electronic devices have both flexibility and high temperature resistance, making them ideal candidate materials for flexible electronic products such as flexible ceramic nanofilms, high-power devices, and dielectric capacitors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nanomaterials, and in particular to a method for preparing sodium bismuth titanate nanowires with a large aspect ratio. Background Art

[0002] Modern electronic components are developing towards miniaturization, integration, flexibility and systematization, and the attention paid to micro-nano materials is also increasing. Among them, one-dimensional nanomaterials have unique size and morphological characteristics, which can be used to manufacture smaller and more efficient electronic devices. They are also the key to constructing nano-level devices.

[0003] Sodium bismuth titanate ceramics do not contain lead and have outstanding environmental performance advantages. They are one of the most promising products to replace lead zirconate titanate ceramics. 0.5 Bi 0.5 TiO3, abbreviated as BNT, is considered to be one of the most likely lead-free piezoelectric ceramic systems to replace lead-based piezoelectric ceramics. BNT is a perovskite-type ferroelectric material substituted with A-site composite ions. It has excellent electrical and optical properties and high polarization strength. It can be used in capacitors, sensors, optoelectronic devices and other fields. The high residual polarization and relaxation characteristics of BNT make it a promising material for effective storage of electrical energy. At present, sodium bismuth titanate nanowire materials are mostly prepared by hydrothermal method, while there are few studies on the preparation of sodium bismuth titanate nanowire materials by electrospinning. In addition, the preparation of sodium bismuth titanate nanowires by hydrothermal method has problems such as difficult to control the reaction degree, poor continuity of nanowire products, uneven size, and poor flexibility. If sodium bismuth titanate nanowires with uniform size and good flexibility can be prepared by simple and easy-to-control electrospinning method, it will have a very broad application prospect. Summary of the invention

[0004] The purpose of the present invention is to provide a sodium bismuth titanate (Na 0.5 Bi 0.5 The invention provides a method for preparing sodium bismuth titanate (BiTiO3) nanowires to solve the problems existing in the above-mentioned prior art. The preparation method of the invention can greatly improve the aspect ratio of sodium bismuth titanate nanowires and improve their flexibility. The sodium bismuth titanate nanowire products prepared by the method of the invention have high purity, good continuity, uniform size and smooth surface, and can be used as the basic material of a new generation of flexible electronic products, so that electronic devices have both the advantages of flexibility and high temperature resistance.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] One of the technical solutions of the present invention: a method for preparing sodium bismuth titanate nanowires with a large aspect ratio, comprising the following steps:

[0007] Mix a titanium source, a bismuth source, a sodium source, acetic acid, acetylacetone, water, N,N-dimethylformamide and a thickener, and stir evenly to obtain a precursor solution;

[0008] Electrospinning the precursor solution to obtain nanowires, and then heat treating the nanowires to obtain the sodium bismuth titanate nanowires with a large aspect ratio;

[0009] The aspect ratio of the large aspect ratio bismuth titanate nanowire is 85-140.

[0010] Further, the titanium source includes one or more of isopropyl titanate, tetrabutyl titanate, isobutyl titanate, tetraethyl titanate and polybutyl titanate;

[0011] The bismuth source includes one or more of bismuth acetate, bismuth aluminate, bismuth molybdate, bismuth stannate, bismuth citrate and bismuth ferrite;

[0012] The sodium source includes one or more of sodium citrate, sodium carbonate, sodium acetate and sodium formate;

[0013] The tackifier includes one or more of polyvinyl chloride, polystyrene, polyvinylidene fluoride, polyethylene, polypropylene, polyethylene glycol, polyvinyl pyrrolidone, polyvinyl alcohol and polylactic acid.

[0014] Furthermore, the mass ratio of the water, N,N-dimethylformamide, acetylacetone, sodium source, titanium source, bismuth source and acetic acid is 1: (0.1-20): (0.1-30): (0.1-30): (0.1-50): (0.1-50): (0.1-100).

[0015] Furthermore, the mass ratio of the thickener, the sodium source, the titanium source and the bismuth source is 1:(0.1-30):(0.1-50):(0.1-50).

[0016] Furthermore, the stirring speed is 300-900 rpm, the time is 0.5-5 h, the stirring is carried out under heating conditions, and the heating temperature is 20-90° C.

[0017] Furthermore, the specific operation of mixing the titanium source, bismuth source, sodium source, acetic acid, acetylacetone, water, N,N-dimethylformamide and thickener is as follows: placing the sodium source in water under heating and stirring conditions to obtain a sodium source solution; placing the bismuth source in acetic acid under heating and stirring conditions to obtain a bismuth source solution; mixing the sodium source solution and the bismuth source solution, adding the titanium source, N,N-dimethylformamide and thickener to the mixed solution to complete the mixing of all raw materials; the heating and stirring temperature is 20 to 90° C., and the rotation speed is 300 to 900 rpm.

[0018] Furthermore, the electrospinning conditions include: a spinning rate of 0.1 to 3 mL / h, a voltage of 5 to 20 kV, a temperature of 20 to 50° C., a humidity of 20 to 50%, and a spinning distance of 5 to 20 cm.

[0019] Furthermore, the heat treatment is performed at a temperature of 800 to 1200° C. and for a time of 2 to 8 hours.

[0020] Furthermore, the heat treatment is performed in an air atmosphere.

[0021] The second technical solution of the present invention: a sodium bismuth titanate nanowire with a large aspect ratio prepared by the above preparation method.

[0022] The third technical solution of the present invention: an application of the above-mentioned sodium bismuth titanate nanowires with a large aspect ratio in the preparation of flexible electronic products.

[0023] The inventive concept of the present invention is as follows: the present invention first obtains a precursor solution by mixing using a solution method, then synthesizes nanowires by electrospinning technology, and then removes impurities such as a thickener by heat treatment to obtain the final target product; the one-dimensional Na prepared by the preparation method of the present invention 0.5 Bi 0.5 TiO3 nanowires have good crystallinity and dispersion characteristics, and have a large aspect ratio. The acetylacetone added in the present invention inhibits the hydrolysis of tetrabutyl titanate, shortens the gel time, and makes the sodium bismuth titanate nanowires longer; and the solvent N,N-dimethylformamide can increase the viscosity and surface tension of the spinning solution, so that the diameter of the nanowires is reduced. If other solvents are used, such as ethanol as the solvent, the viscosity and surface tension of the spinning solution are relatively reduced, which will lead to an increase in the diameter of the nanowires; adding an appropriate amount of acetic acid can balance and stabilize the hydrolysis and polymerization processes, thereby improving the surface morphology of the nanowires. Nanowires with a large aspect ratio help to improve the flexibility of the material and can be used as the basic material for a new generation of flexible electronic products, so that electronic devices have both the advantages of flexibility and high temperature resistance, making them ideal candidate materials for flexible electronic products such as flexible ceramic nanofilms, high-power devices, and dielectric capacitors. The preparation method of the present invention is simple, easy to operate and control.

[0024] The present invention discloses the following technical effects:

[0025] The sodium bismuth titanate nanowires prepared by the method of the present invention have a large aspect ratio and good flexibility, and can be used to prepare flexible electronic products, such as flexible ceramic nanofilms, and have a wide range of applications.

[0026] The titanium source, bismuth source and sodium source used in the present invention are widely available, easy to obtain and inexpensive;

[0027] The tackifier used in the present invention is of various types, low in price and good in viscosity effect, and is conducive to forming a one-dimensional structure with good surface morphology;

[0028] The present invention can realize mass preparation of sodium bismuth titanate nanowires through an electrostatic spinning method, and the electrostatic spinning method is simple, easy to operate and control, and is easy to scale up for production. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0030] Figure 1 The X-ray diffraction patterns of the sodium bismuth titanate nanowire powder after heat treatment in Example 1 are compared with those before heat treatment;

[0031] Figure 2 This is a scanning electron microscope image of the sodium bismuth titanate nanowire powder prepared in Example 1;

[0032] Figure 3 The length and diameter distribution diagram of sodium bismuth titanate nanowires prepared in Example 1;

[0033] Figure 4 This is a length and diameter distribution diagram of sodium bismuth titanate nanowires prepared in Example 2;

[0034] Figure 5 The length and diameter distribution diagram of sodium bismuth titanate nanowires prepared in Example 3;

[0035] Figure 6 The length and diameter distribution diagram of sodium bismuth titanate nanowires prepared in Example 4;

[0036] Figure 7 This is a length and diameter distribution diagram of sodium bismuth titanate nanowires prepared in Example 5;

[0037] Figure 8 This is a length and diameter distribution diagram of sodium bismuth titanate nanowires prepared in Example 6;

[0038] Fig. 9 This is a length and diameter distribution diagram of the sodium bismuth titanate nanowires prepared in Example 7. DETAILED DESCRIPTION

[0039] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0040] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0041] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0042] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0043] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0044] The present invention provides a method for preparing sodium bismuth titanate nanowires with a large aspect ratio, comprising the following steps:

[0045] Mix a titanium source, a bismuth source, a sodium source, acetic acid, acetylacetone, water, N,N-dimethylformamide and a thickener, and stir evenly to obtain a precursor solution;

[0046] Electrospinning the precursor solution to obtain nanowires, and then heat treating the nanowires to obtain the sodium bismuth titanate nanowires with a large aspect ratio;

[0047] The aspect ratio (average aspect ratio) of the large aspect ratio bismuth titanate nanowires is 85-140.

[0048] Furthermore, the titanium source includes one or more of isopropyl titanate, tetrabutyl titanate, isobutyl titanate, tetraethyl titanate and polybutyl titanate; when the titanium source is two or more of the above specific selections, the present invention has no special limitation on the ratio of the above specific substances, and they can be mixed in any ratio;

[0049] The bismuth source includes one or more of bismuth acetate, bismuth aluminate, bismuth molybdate, bismuth stannate, bismuth citrate and bismuth ferrite; when the bismuth source is two or more of the above specific selections, the present invention has no special restrictions on the ratio of the above specific substances, and they can be mixed in any ratio;

[0050] The sodium source includes one or more of sodium citrate, sodium carbonate, sodium acetate and sodium formate; when the sodium source is two or more of the above specific selections, the present invention has no special limitation on the ratio of the above specific substances, and they can be mixed in any ratio;

[0051] The thickener includes one or more of polyvinyl chloride, polystyrene, polyvinylidene fluoride, polyethylene, polypropylene, polyethylene glycol, polyvinyl pyrrolidone, polyvinyl alcohol and polylactic acid; when the thickener is two or more of the above specific options, the present invention has no special limitation on the ratio of the above specific substances, and they can be mixed in any ratio.

[0052] Furthermore, the water is preferably deionized water.

[0053] Furthermore, the mass ratio of the water, N,N-dimethylformamide, acetylacetone, sodium source, titanium source, bismuth source and acetic acid is 1: (0.1-20): (0.1-30): (0.1-30): (0.1-50): (0.1-50): (0.1-100); preferably, it is 1: (0.5-15): (0.5-25): (0.5-25): (1-40): (1-40): (2-80); more preferably, it is 1: (0.5-10): (0.5-20): (0.5-20): (2-30): (2-30): (5-60).

[0054] Furthermore, the mass ratio of the thickener, sodium source, titanium source and bismuth source is 1: (0.1-30): (0.1-50): (0.1-50); preferably 1: (0.5-20): (0.5-40): (0.5-40); more preferably 1: (0.5-10): (0.5-20): (0.5-20).

[0055] In the present invention, the role of the acetic acid is to serve as a buffer solution to promote the reaction of the sodium source, bismuth source and titanium source, balance and stabilize hydrolysis, and improve the surface morphology of the nanowires; the role of the acetylacetone is to inhibit the hydrolysis of tetrabutyl titanate, shorten the gel time, increase the surface tension of the mixed solution, and make the nanowires longer; the role of the N,N-dimethylformamide is to prevent the appearance of Taylor cones, avoid condensation due to insufficient tension, increase the surface tension of the mixed solution, and reduce the diameter of the nanowires.

[0056] Furthermore, the stirring speed is 300-900 rpm, preferably 350-850 rpm, more preferably 400-700 rpm; the time is 0.5-5 h, preferably 1-4.5 h, more preferably 1.5-3 h; the stirring is carried out under heating conditions, and the heating temperature is 20-90°C, preferably 40-80°C, more preferably 50-70°C.

[0057] Furthermore, the specific operation of mixing the titanium source, bismuth source, sodium source, acetic acid, acetylacetone, water, N,N-dimethylformamide and thickener is as follows: placing the sodium source in water under heating and stirring conditions to obtain a sodium source solution; placing the bismuth source in acetic acid under heating and stirring conditions to obtain a bismuth source solution; mixing the sodium source solution and the bismuth source solution, adding the titanium source, N,N-dimethylformamide and thickener to the mixed solution to complete the mixing of all raw materials; the heating and stirring temperatures are all 20 to 90°C, preferably 40 to 80°C, and more preferably 50 to 70°C; the rotation speeds are all 300 to 900rpm, preferably 350 to 850rpm, and more preferably 400 to 700rpm.

[0058] Furthermore, after all the raw materials are mixed and stirred evenly, a defoaming treatment method including ultrasonic treatment and standing treatment is preferably performed in sequence. The present invention does not have any special limitation on the ultrasonic treatment and standing treatment process, and the treatment can be performed using operations familiar to those skilled in the art.

[0059] Furthermore, the conditions for the electrospinning include: a spinning rate of 0.1 to 3 mL / h, preferably 0.15 to 2.5 mL / h, more preferably 0.2 to 2.0 mL / h; a voltage of 5 to 20 kV, preferably 10 to 20 kV, more preferably 12 to 18 kV; a temperature of 20 to 50 ° C, preferably 30 to 45 ° C, more preferably 35 to 40 ° C; a humidity of 20 to 50%, preferably 25 to 45%, more preferably 30 to 40%; a spinning distance of 5 to 20 cm, preferably 8 to 18 cm, more preferably 10 to 15 cm.

[0060] Furthermore, the heat treatment temperature is 800-1200° C., preferably 850-1150° C., more preferably 900-1100° C.; the time is 2-8 h, preferably 3-7 h, more preferably 4-6 h.

[0061] Furthermore, the heat treatment is performed in an air atmosphere.

[0062] In the present invention, the heat treatment is used to promote the reaction of the titanium source, bismuth source and sodium source, and is also the most important step in the preparation of ceramic fillers. Sodium bismuth titanate is synthesized by sintering during the heat treatment process, and at the same time, the thermal decomposition and removal of residual organic matter is also promoted.

[0063] The present invention also provides sodium bismuth titanate nanowires with a large aspect ratio prepared by the above preparation method.

[0064] The present invention also provides an application of the sodium bismuth titanate nanowire with a large aspect ratio in the preparation of flexible electronic products.

[0065] The preparation method of sodium bismuth titanate nanowires with a large aspect ratio provided by the present invention is further described in detail below in conjunction with specific examples, but they should not be construed as limiting the scope of protection of the present invention.

[0066] The raw materials used in the following examples and comparative examples are all commercially available products known to those skilled in the art. Among them, bismuth acetate, N,N-dimethylformamide, and acetic acid were purchased from Shanghai Titan Technology Co., Ltd. (Adamas); sodium acetate was purchased from Shanghai Titan Technology Co., Ltd. (Greagent); acetylacetone and tetrabutyl titanate were purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.; and polyvinyl pyrrolidone was purchased from Sigma-Aldrich (Shanghai) Trading Co., Ltd.

[0067] Example 1

[0068] Weigh the raw materials according to the mass ratio of deionized water: N,N-dimethylformamide: acetylacetone: sodium acetate: tetrabutyl titanate: bismuth acetate: acetic acid: polyvinyl pyrrolidone = 1: 0.56: 0.56: 0.5: 4.2: 2.3: 5.9: 0.5, and under heating and stirring conditions (temperature of 70°C, speed of 650rpm), first put sodium acetate in deionized water, then put bismuth acetate in acetic acid, and stir for several minutes until the solution is clear to obtain sodium acetate solution and Bismuth acetate solution, then the two are mixed, and then tetrabutyl titanate, N, N-dimethylformamide, acetylacetone and polyvinyl pyrrolidone are added to the mixed solution, and heating and stirring are continued for 2 hours (temperature is 70°C, speed is 650rpm), and then ultrasonic and static defoaming treatment methods are carried out in sequence, wherein the ultrasonic time is 10 minutes, the ultrasonic electric power is 150W, the ultrasonic frequency is 40KHz, and the static time is 30 minutes, thereby obtaining a precursor solution (sodium bismuth titanate spinning solution);

[0069] The precursor solution was loaded into a syringe, and a 23G needle (inner diameter 0.33 mm, outer diameter 0.63 mm) was used for electrospinning (voltage 15 kV, temperature 35 ° C, humidity 35%, spinning distance 15 cm, spinning rate of spinning solution 0.2 mL / h), and then heat treated in air atmosphere (900 ° C, 4 h) to obtain sodium bismuth titanate nanowire powder (Na 0.5 Bi 0.5 TiO3 nanowire powder).

[0070] The crystal structure and phase of the sodium bismuth titanate nanowire powder before and after the heat treatment were observed using an X-ray diffractometer (XRD, Bruker, Germany). Figure 1 The X-ray diffraction patterns of the sodium bismuth titanate nanowire powder after heat treatment and the sodium bismuth titanate nanowire powder before heat treatment are compared. Figure 1 It can be seen that the sodium bismuth titanate nanowire powder after heat treatment presents a distinct crystalline structure without obvious stray peaks. In addition, the sodium bismuth titanate nanowire powder has 7 peaks at 22.8°, 32.4°, 40.2°, 46.6°, 52.7°, 58.1° and 68.3°, corresponding to the (100), (101), (111), (200), (201), (211) and (301) crystal planes, respectively. Corresponding to the standard card below; the overall linearity of the image before heat treatment tends to be flat, without any characteristic peaks, and no obvious crystal crystallinity.

[0071] The morphology of the sodium bismuth titanate nanowire powder (after heat treatment) finally obtained in this embodiment was observed using a transmission electron microscope (JEM 2100F, JEOL, Japan). The scanning electron microscope image is as follows: Figure 2 As shown by Figure 2 It can be seen that the sodium bismuth titanate nanowires prepared in this embodiment have a large aspect ratio, and the nanowires have good continuity, a smooth surface, and uniform size.

[0072] Example 2

[0073] Weigh the raw materials according to the mass ratio of deionized water: N,N-dimethylformamide: acetylacetone: sodium acetate: tetrabutyl titanate: bismuth acetate: acetic acid: polyvinyl pyrrolidone = 1: 0.56: 0.56: 0.5: 4.2: 2.3: 5.9: 0.5, and under heating and stirring conditions (temperature of 70°C, speed of 650rpm), first put sodium acetate in deionized water, then put bismuth acetate in acetic acid, and stir for several minutes until the solution is clear to obtain sodium acetate solution and Bismuth acetate solution, then the two are mixed, and then tetrabutyl titanate, N, N-dimethylformamide, acetylacetone and polyvinyl pyrrolidone are added to the mixed solution, and heating and stirring are continued for 2 hours (temperature is 70°C, speed is 650rpm), and then ultrasonic and static defoaming treatment methods are carried out in sequence, wherein the ultrasonic time is 10 minutes, the ultrasonic electric power is 150W, the ultrasonic frequency is 40KHz, and the static time is 30 minutes, thereby obtaining a precursor solution (sodium bismuth titanate spinning solution);

[0074] The precursor solution was loaded into a syringe, and a 23G needle (inner diameter 0.33 mm, outer diameter 0.63 mm) was used for electrospinning (voltage 15 kV, temperature 35 ° C, humidity 35%, spinning distance 15 cm, spinning rate of spinning solution 0.2 mL / h), and then heat treated in air atmosphere (950 ° C, 4 h) to obtain sodium bismuth titanate nanowire powder (Na 0.5 Bi 0.5 TiO3 nanowire powder).

[0075] The difference between this embodiment and embodiment 1 is only the temperature of the heat treatment. XRD and SEM tests were performed on the sodium bismuth titanate nanowire powder finally obtained in this embodiment (since the XRD and SEM images of embodiments 2-7 are very similar to those of embodiment 1, the XRD images and SEM images of embodiments 2-7 are not provided here again, and only the results are described). The XRD results show that the sodium bismuth titanate nanowire powder finally obtained in this embodiment presents a distinct crystalline structure, and no obvious impurity peaks appear, indicating that impurities are completely removed by heat treatment; the XRD results show that the sodium bismuth titanate nanowire powder obtained has a large aspect ratio, and the nanowires have good continuity, a smooth surface, and uniform size.

[0076] Example 3

[0077] Weigh the raw materials according to the mass ratio of deionized water: N,N-dimethylformamide: acetylacetone: sodium acetate: tetrabutyl titanate: bismuth acetate: acetic acid: polyvinyl pyrrolidone = 1: 0.56: 0.56: 0.5: 4.2: 2.3: 5.9: 0.5, and under heating and stirring conditions (temperature of 70°C, speed of 650rpm), first put sodium acetate in deionized water, then put bismuth acetate in acetic acid, and stir for several minutes until the solution is clear to obtain sodium acetate solution and Bismuth acetate solution, then the two are mixed, and then tetrabutyl titanate, N, N-dimethylformamide, acetylacetone and polyvinyl pyrrolidone are added to the mixed solution, and heating and stirring are continued for 2 hours (temperature is 70°C, speed is 650rpm), and then ultrasonic and static defoaming treatment methods are carried out in sequence, wherein the ultrasonic time is 10 minutes, the ultrasonic electric power is 150W, the ultrasonic frequency is 40KHz, and the static time is 30 minutes, thereby obtaining a precursor solution (sodium bismuth titanate spinning solution);

[0078] The precursor solution was loaded into a syringe, and a 23G needle (inner diameter 0.33 mm, outer diameter 0.63 mm) was used for electrospinning (voltage 15 kV, temperature 35 ° C, humidity 35%, spinning distance 15 cm, spinning rate of spinning solution 0.2 mL / h), and then heat treated in air atmosphere (1000 ° C, 4 h) to obtain sodium bismuth titanate nanowire powder (Na 0.5 Bi0.5 TiO3 nanowire powder).

[0079] The difference between this embodiment and embodiment 1 is only the temperature of the heat treatment. XRD and SEM tests were performed on the sodium bismuth titanate nanowire powder finally obtained in this embodiment. The XRD results showed that the sodium bismuth titanate nanowire powder finally obtained in this embodiment showed a clear crystalline structure without obvious impurity peaks, indicating that the impurities were completely removed by heat treatment; the XRD results showed that the sodium bismuth titanate nanowire powder obtained had a large aspect ratio, and the nanowires had good continuity, smooth surface, and uniform size.

[0080] Example 4

[0081] Weigh the raw materials according to the mass ratio of deionized water: N,N-dimethylformamide: acetylacetone: sodium acetate: tetrabutyl titanate: bismuth acetate: acetic acid: polyvinyl pyrrolidone = 1: 0.56: 0.56: 0.5: 4.2: 2.3: 5.9: 0.5, and under heating and stirring conditions (temperature of 70°C, speed of 650rpm), first put sodium acetate in deionized water, then put bismuth acetate in acetic acid, and stir for several minutes until the solution is clear to obtain sodium acetate solution and Bismuth acetate solution, then the two are mixed, and then tetrabutyl titanate, N, N-dimethylformamide, acetylacetone and polyvinyl pyrrolidone are added to the mixed solution, and heating and stirring are continued for 2 hours (temperature is 70°C, speed is 650rpm), and then ultrasonic and static defoaming treatment methods are carried out in sequence, wherein the ultrasonic time is 10 minutes, the ultrasonic electric power is 150W, the ultrasonic frequency is 40KHz, and the static time is 30 minutes, thereby obtaining a precursor solution (sodium bismuth titanate spinning solution);

[0082] The precursor solution was loaded into a syringe, and a 23G needle (inner diameter 0.33 mm, outer diameter 0.63 mm) was used for electrospinning (voltage 15 kV, temperature 35 ° C, humidity 35%, spinning distance 15 cm, spinning rate of spinning solution 0.2 mL / h), and then heat treated in air atmosphere (1050 ° C, 4 h) to obtain sodium bismuth titanate nanowire powder (Na 0.5 Bi 0.5 TiO3 nanowire powder).

[0083] The difference between this embodiment and embodiment 1 is only the temperature of the heat treatment. XRD and SEM tests were performed on the sodium bismuth titanate nanowire powder finally obtained in this embodiment. The XRD results showed that the sodium bismuth titanate nanowire powder finally obtained in this embodiment showed a clear crystalline structure without obvious impurity peaks, indicating that the impurities were completely removed by heat treatment; the XRD results showed that the sodium bismuth titanate nanowire powder obtained had a large aspect ratio, and the nanowires had good continuity, smooth surface, and uniform size.

[0084] Example 5

[0085] Weigh the raw materials according to the mass ratio of deionized water: N,N-dimethylformamide: acetylacetone: sodium acetate: tetrabutyl titanate: bismuth acetate: acetic acid: polyvinyl pyrrolidone = 1: 0.56: 0.56: 0.5: 4.2: 2.3: 5.9: 0.5, and under heating and stirring conditions (temperature of 70°C, speed of 650rpm), first put sodium acetate in deionized water, then put bismuth acetate in acetic acid, and stir for several minutes until the solution is clear to obtain sodium acetate solution and Bismuth acetate solution, then the two are mixed, and then tetrabutyl titanate, N, N-dimethylformamide, acetylacetone and polyvinyl pyrrolidone are added to the mixed solution, and heating and stirring are continued for 2 hours (temperature is 70°C, speed is 650rpm), and then ultrasonic and static defoaming treatment methods are carried out in sequence, wherein the ultrasonic time is 10 minutes, the ultrasonic electric power is 150W, the ultrasonic frequency is 40KHz, and the static time is 30 minutes, thereby obtaining a precursor solution (sodium bismuth titanate spinning solution);

[0086] The precursor solution was loaded into a syringe, and a 23G needle (inner diameter 0.33 mm, outer diameter 0.63 mm) was used for electrospinning (voltage 15 kV, temperature 35 ° C, humidity 35%, spinning distance 15 cm, spinning rate of spinning solution 0.2 mL / h), and then heat treated in air atmosphere (1100 ° C, 4 h) to obtain sodium bismuth titanate nanowire powder (Na 0.5 Bi 0.5 TiO3 nanowire powder).

[0087] The difference between this embodiment and embodiment 1 is only the temperature of the heat treatment. XRD and SEM tests were performed on the sodium bismuth titanate nanowire powder finally obtained in this embodiment. The XRD results showed that the sodium bismuth titanate nanowire powder finally obtained in this embodiment showed a clear crystalline structure without obvious impurity peaks, indicating that the impurities were completely removed by heat treatment; the XRD results showed that the sodium bismuth titanate nanowire powder obtained had a large aspect ratio, and the nanowires had good continuity, smooth surface, and uniform size.

[0088] Example 6

[0089] Weigh the raw materials according to the mass ratio of deionized water: N,N-dimethylformamide: acetylacetone: sodium acetate: tetrabutyl titanate: bismuth acetate: acetic acid: polyvinyl pyrrolidone = 1: 0.56: 0.56: 0.5: 4.2: 2.3: 5.9: 0.5, and under heating and stirring conditions (temperature of 70°C, speed of 650rpm), first put sodium acetate in deionized water, then put bismuth acetate in acetic acid, and stir for several minutes until the solution is clear to obtain sodium acetate solution and Bismuth acetate solution, then the two are mixed, and then tetrabutyl titanate, N, N-dimethylformamide, acetylacetone and polyvinyl pyrrolidone are added to the mixed solution, and heating and stirring are continued for 2 hours (temperature is 70°C, speed is 650rpm), and then ultrasonic and static defoaming treatment methods are carried out in sequence, wherein the ultrasonic time is 10 minutes, the ultrasonic electric power is 150W, the ultrasonic frequency is 40KHz, and the static time is 30 minutes, thereby obtaining a precursor solution (sodium bismuth titanate spinning solution);

[0090] The precursor solution was loaded into a syringe, and a 23G needle (inner diameter 0.33 mm, outer diameter 0.63 mm) was used for electrospinning (voltage 18 kV, temperature 40 ° C, humidity 40%, spinning distance 10 cm, spinning rate of spinning solution 1 mL / h), and then heat treated in air atmosphere (900 ° C, 4 h) to obtain sodium bismuth titanate nanowire powder (Na 0.5 Bi 0.5 TiO3 nanowire powder).

[0091] The difference between this embodiment and embodiment 1 lies in the different electrospinning conditions, namely, the voltage, temperature, humidity, spinning distance and spinning rate. The sodium bismuth titanate nanowire powder finally obtained in this embodiment was subjected to XRD and SEM tests. The XRD results showed that the sodium bismuth titanate nanowire powder finally obtained in this embodiment showed a distinct crystalline structure without obvious impurity peaks, indicating that impurities were completely removed by heat treatment; the XRD results showed that the sodium bismuth titanate nanowire powder obtained had a large aspect ratio, and the nanowires had good continuity, a smooth surface and uniform size.

[0092] Example 7

[0093] Weigh the raw materials according to the mass ratio of deionized water: N,N-dimethylformamide: acetylacetone: sodium acetate: tetrabutyl titanate: bismuth acetate: acetic acid: polyvinyl pyrrolidone = 1: 0.56: 0.56: 0.5: 4.2: 2.3: 5.9: 0.5, and under heating and stirring conditions (temperature of 50°C, speed of 400rpm), first put sodium acetate in deionized water, then put bismuth acetate in acetic acid, and stir for several minutes until the solution is clear to obtain sodium acetate solution and Bismuth acetate solution, then the two are mixed, and then tetrabutyl titanate, N, N-dimethylformamide, acetylacetone and polyvinyl pyrrolidone are added to the mixed solution, and heating and stirring are continued for 3 hours (temperature is 50°C, speed is 400rpm), and then ultrasonic and static defoaming treatment methods are carried out in sequence, where the ultrasonic time is 10 minutes, the ultrasonic electric power is 150W, the ultrasonic frequency is 40KHz, and the static time is 30 minutes, thereby obtaining a precursor solution (sodium bismuth titanate spinning solution);

[0094] The precursor solution was loaded into a syringe, and a 23G needle (inner diameter 0.33 mm, outer diameter 0.63 mm) was used for electrospinning (voltage 15 kV, temperature 35 ° C, humidity 35%, spinning distance 15 cm, spinning rate of spinning solution 0.2 mL / h), and then heat treated in air atmosphere (900 ° C, 4 h) to obtain sodium bismuth titanate nanowire powder (Na 0.5 Bi 0.5 TiO3 nanowire powder).

[0095] The difference between this embodiment and embodiment 1 is the temperature of heating and stirring, the time of stirring and the speed of rotation. The sodium bismuth titanate nanowire powder finally obtained in this embodiment was subjected to XRD and SEM tests. The XRD results showed that the sodium bismuth titanate nanowire powder finally obtained in this embodiment showed a clear crystalline structure without obvious impurity peaks, indicating that the impurities were completely removed by heat treatment; the XRD results showed that the sodium bismuth titanate nanowire powder obtained had a large aspect ratio, and the nanowires had good continuity, smooth surface and uniform size.

[0096] Comparative Example 1

[0097] A method for preparing sodium bismuth titanate nanowires by a hydrothermal method, specifically: preparing 42.5 mL of a NaOH solution and adjusting its pH to 14; after the NaOH solution is cooled to room temperature, 0.9 g of TiO2 and 2.7 g of Bi(NO3)3·5H2O are added thereto in sequence, and stirred for 45 minutes to form a yellow suspension, wherein the molar ratio of TiO2 to Bi(NO3)3·5H2O is 2:1, and at this time, Bi 3+The concentration is 0.13 mol / L; 0.8 g of hexadecyltrimethylammonium bromide is added to the yellow suspension and stirred for 55 min to obtain a hydrothermal precursor solution; the hydrothermal precursor solution is transferred to a 50 mL reactor for hydrothermal reaction. At this time, the filling rate of the reactor is 85%, the heating rate is 2 ° C / min, and the hydrothermal reaction is carried out at 165 ° C for 18 hours. The product is washed with deionized water for 4 times until the washing liquid after washing is neutral, and then washed with anhydrous ethanol for 3 times. After standing for 2 hours, the obtained product is dried at 50 ° C for 12 hours to obtain a one-dimensional Na 0.5 Bi 0.5 TiO3 nanowires.

[0098] Comparative Example 2

[0099] The same as Example 1, except that the use of acetylacetone is omitted, that is, the raw materials are weighed according to the mass ratio of deionized water: N,N-dimethylformamide: sodium acetate: tetrabutyl titanate: bismuth acetate: acetic acid: polyvinyl pyrrolidone = 1:0.56:0.5:4.2:2.3:5.9:0.5.

[0100] Comparative Example 3

[0101] The same as Example 1, except that the use of N,N-dimethylformamide is omitted, that is, the raw materials are weighed according to the mass ratio of deionized water: acetylacetone: sodium acetate: tetrabutyl titanate: bismuth acetate: acetic acid: polyvinyl pyrrolidone = 1:0.56:0.5:4.2:2.3:5.9:0.5.

[0102] Test Case

[0103] The sodium bismuth titanate nanowire powders prepared in Examples 1-7 and Comparative Examples 1-3 were taken and photographed using a scanning electron microscope to measure the length and diameter distribution of the sodium bismuth titanate nanowires, and the average length and average diameter were calculated. The length and diameter distribution of the sodium bismuth titanate nanowires prepared in Examples 1-7 are shown in Figures 1 and 2. Figure 3-9 The average length, average diameter and aspect ratio of each embodiment and comparative example are shown in Table 1:

[0104] Table 1

[0105] Preparation method Average length (μm) Average diameter (μm) Average aspect ratio Electrospinning (Example 1) 85.63 1.00 85.63 Electrospinning (Example 2) 90.99 0.96 94.78 Electrospinning (Example 3) 107.01 0.82 130.5 Electrospinning (Example 4) 101.73 1.04 97.82 Electrospinning (Example 5) 98.60 1.15 85.74 Electrospinning (Example 6) 84.46 0.99 85.31 Electrospinning (Example 7) 85.83 0.94 91.31 Hydrothermal method (Comparative Example 1) 1.00 0.15 6.67 Electrospinning (Comparative Example 2) 21.38 1.66 12.88 Electrospinning (Comparative Example 3) 86.23 1.57 54.92

[0106] Depend on Figure 3-9 As shown in Table 1, the sodium bismuth titanate nanowires prepared in Examples 1-7 of the present invention have uniform sizes and a large aspect ratio.

[0107] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing sodium bismuth titanate nanowires with a large aspect ratio, characterized in that: The following steps are involved: Mix a titanium source, a bismuth source, a sodium source, acetic acid, acetylacetone, water, N,N-dimethylformamide and a thickener, and stir evenly to obtain a precursor solution; Electrospinning the precursor solution to obtain nanowires, and then heat treating the nanowires to obtain the sodium bismuth titanate nanowires with a large aspect ratio; The aspect ratio of the sodium bismuth titanate nanowire with a large aspect ratio is 85 to 140; The tackifier includes one or more of polyvinyl chloride, polystyrene, polyvinylidene fluoride, polyethylene, polypropylene, polyethylene glycol, polyvinyl pyrrolidone, polyvinyl alcohol and polylactic acid; The mass ratio of water, N,N-dimethylformamide, acetylacetone, sodium source, titanium source, bismuth source and acetic acid is 1: (0.1-20): (0.1-30): (0.1-30): (0.1-50): (0.1-50): (0.1-100); The mass ratio of the thickener, the sodium source, the titanium source and the bismuth source is 1: (0.1-30): (0.1-50): (0.1-50); The electrospinning conditions include: a spinning rate of 0.1 to 3 mL / h, a voltage of 5 to 20 kV, a temperature of 20 to 50° C., a humidity of 20 to 50%, and a spinning distance of 5 to 20 cm; The heat treatment temperature is 800-1200° C. and the time is 2-8 hours.

2. The preparation method according to claim 1, characterized in that The titanium source includes one or more of isopropyl titanate, tetrabutyl titanate, isobutyl titanate, tetraethyl titanate and polybutyl titanate; The bismuth source includes one or more of bismuth acetate, bismuth aluminate, bismuth molybdate, bismuth stannate, bismuth citrate and bismuth ferrite; The sodium source includes one or more of sodium citrate, sodium carbonate, sodium acetate and sodium formate.

3. The preparation method according to claim 1, characterized in that: The heat treatment is performed in an air atmosphere.

4. A sodium bismuth titanate nanowire with a large aspect ratio prepared by the preparation method according to any one of claims 1 to 3.

5. Use of the sodium bismuth titanate nanowire with a large aspect ratio as claimed in claim 4 in the preparation of flexible electronic products.