MoTe2 / CdS 0.42 Se 0.58 Thin-film heterojunction photodetector and preparation method thereof
Through MoTe2/CdS0.42Se0.58 sheet heterojunction structure and advanced preparation technology, the problem of insufficient performance of existing MoTe2 photodetectors is solved, efficient photodetection and rapid response are achieved, and it has expanded its field in photodetection and imaging. Application prospects.
Patent Information
- Application Number
- CN202311827938.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-12-28
AI Technical Summary
The existing MoTe2 photodetector has a low photocurrent to dark current ratio, and its response speed and response rate are insufficient, which limits its application in photodetection.
MoTe2/CdS0.42Se0.58 sheet heterojunction structure was used to prepare small-layer MoTe2 and CdS0.42Se0.58 sheets through chemical vapor deposition and mechanical peeling technology, and the band arrangement of the heterostructure was optimized using first principles. Form an efficient photodetector.
The switching ratio, response rate, external quantum efficiency and detection rate of the photodetector are significantly improved, faster response speed and higher photoelectric performance are achieved, and good visible light imaging capabilities are provided.
Smart Images

Figure CN118156339B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of photoelectric imaging technology, and particularly relates to MoTe2 / CdS 0.42 Se 0.58 Thin-film heterojunction photodetector and preparation method thereof. Background Art
[0002] Two-dimensional layered materials have facilitated a new era of fundamental research and exploration of potential applications. Many two-dimensional layered materials, including graphene, hexagonal boron nitride, black phosphorus, transition metal dichalcogenides (TMDs), and post-transition metal dichalcogenides, have gained widespread attention due to their unique structures and interesting physical and chemical properties. Importantly, two-dimensional materials have potential applications in a wide range of research fields, such as catalysis, batteries, phototransistors, and photodetectors.
[0003] As a member of the transition metal dichalcogenide family (TMD), MoTe2 is a layer-dependent bandgap (1.01.1eV) semiconductor. Due to its stability and excellent electrical properties, it is a candidate material for photodetectors with high electrical performance; for example, MoTe2 has strong light absorption ability and high carrier mobility. However, single MoTe2 photodetectors exhibit relatively low photocurrent to dark current ratio, response speed (millisecond level) and low responsivity (mA / W level); these aspects hinder its further application in photodetection. Based on this situation, many researchers have conducted a lot of research to improve the photoelectric performance by applying gate voltage or constructing heterostructures. Wright et al. fabricated a four-layer MoTe2 field effect transistor (FETs) with a photoresponse time of ~160μs under 685nm laser illumination, and the photoresponsivity was only 6A / W even at a large gate voltage of 40V. He et al. also reported a MoTe2 phototransistor with a zero gate voltage responsivity of ~10 under 473nm laser illumination. 2 A / W, and increased to 2560A / W at 80V gate voltage. Chu et al. developed a few-layer MoTe2 photodetector with a photoresponsivity of 50mA / W and a detectivity of 3.1×10 9 cm Hz 1 / 2 W -1 They then designed a self-powered MoTe2 / MoS2 vertical heterojunction photodetector with a high on / off ratio (>10 5), with a fast response time of 60μs. However, at 46mA / W, the photoresponsivity is still relatively low. Lu et al. prepared a one-dimensional gallium-doped cadmium sulfide nanowire / two-dimensional MoTe2 thin film heterojunction device, realizing a self-driven photodetector with a response time of less than 50ms and a photoresponsivity of less than 60mA / W. Chen et al. made a MoTe2 / WSe2 heterojunction photodetector, achieving ~10 4 The high on-off ratio has a low response time of 72μs under 633nm laser irradiation; however, the responsivity is only 1.8mA / W. Jie et al. reported a few-layer MoTe2 / Si2D3D vertical heterojunction photodetector. Their device has an ultra-high response speed of up to 150ns and a 3.2×10 6 of the photodetectors; however, the responsivity and EQE are only 0.19 A / W and 24%, respectively. Although a lot of work has been done on photodetectors, some key parameters (such as responsivity) still need significant improvement. In addition, a lot of research has been done on visible light imaging based on MoTe2 photodetectors. Therefore, further efforts are needed to improve the light detection performance of MoTe2 photodetectors. Constructing heterojunctions is considered to be an effective method to improve the photoelectric performance of photodetectors through band engineering; this engineering can enhance the photocurrent, suppress the dark current, and promote the effective separation of photogenerated carriers. Loutfy et al. reported CdS by optimizing the composition of cadmium sulfur selenide. 0.5 Se 0.5 It has the highest photoelectrochemical conversion efficiency. In addition, it has successfully produced high-quality CdS 0.42 Se 0.58 Thin slices, whose elemental composition is similar to that of cadmium sulfur selenium CdS 0.5 Se 0.5 To our knowledge, few-layer MoTe2 and CdS have not been reported. 0.42 Se 0.58 Sheet-type heterojunction photodetector. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention provides MoTe2 / CdS 0.42 Se 0.58 Method for preparing thin-film heterojunction photodetector.
[0005] The present invention is achieved by: a few-layer MoTe2 / CdS 0.42 Se 0.58 Thin-film heterojunction photodetector, the device includes MoTe2 / CdS 0.42 Se 0.58 Thin-film heterojunction.
[0006] The CdS0.42 Se 0.58 The flakes include: Cd, Se and Se.
[0007] Another object of the present invention is to provide a method for preparing the few-layer MoTe2 / CdS 0.42 Se 0.58 A method for preparing a thin-film heterojunction photodetector, the method comprising:
[0008] S1: CdS 0.42 Se 0.58 Preparation of thin slices;
[0009] S2: MoTe2 / CdS 0.42 Se 0.58 Preparation of heterojunction photodetectors;
[0010] S3: First principles calculations.
[0011] Further, the S1 specifically includes:
[0012] S11: combining high purity cadmium sulfide and cadmium selenide powders with a purity of 99.99% in a ceramic boat at a molar ratio of 1:1;
[0013] S12: placing the mixture in the central evaporation zone of the quartz tube;
[0014] S13: Cut the silicon wafer into pieces measuring 1.5×1.0 cm 2 The thin slice was placed in a beaker containing acetone; ultrasonic cleaning was performed in the acetone solution for 10 minutes, and then cleaning was performed with ethanol and deionized water for 10 minutes; after the cleaning process, gold particles were sprayed on the silicon dioxide substrate, and the substrate was placed in the upstream and downstream areas of the quartz tube;
[0015] S14: The quartz tube is introduced into the tubular furnace, and the temperature is gradually increased to 835°C at a rate of 5.6°C / min. The system is maintained at this temperature for 150 minutes with a 95:5 ratio of Ar:H2 gas mixture at a flow rate of 17 sccm;
[0016] S15: When the tube furnace cools down to room temperature naturally, CdS is obtained. 0.42 Se 0.58 Flakes were obtained, and few-layer MoTe2 flakes were obtained by mechanical exfoliation.
[0017] Further, the S2 specifically includes:
[0018] S21: Cr and Au were sequentially deposited on a clean silicon dioxide substrate using an electron beam evaporation device to form an electrode with a channel length of 5 μm; the MoTe2 flakes were transferred to the gold electrode using a two-dimensional material transfer system;
[0019] S22: Preparation of CdS 0.42 Se 0.58 The thin film was immersed in an ethanol solution and then dropped onto another clean silica substrate. 0.42 Se 0.58 After the ethanol evaporated, the flakes remained on the substrate;
[0020] S23: CdS 0.42 Se 0.58 The flakes were separated from the initial substrate and transferred onto the top of the MoTe2 flakes using a PDMS film, thus completing the heterojunction construction.
[0021] Further, the S3 specifically includes:
[0022] All first-principles calculations were performed within the framework of the DFTLCAO method, which is implemented in the QuantumATKT2022.03SP1 software package to simulate the trilayer MoTe2 / CdS 0.42 Se 0.58 A slab model consisting of 336 atoms was established; the projected density of states of the heterostructure was calculated more accurately using the HSE hybridization function.
[0023] Furthermore, the thickness of the vacuum layer of the flat plate model is 22 angstroms, and the atomic ratio of Cd, S, and Se is 1:0.42:0.58 in CdS 0.42 Se 0.58 The experimental values are consistent; the structure optimization uses the GrimmeDFTD2 method to take into account the van der Waals correction; the total energy and force converge to a value of ~10 4 eV and 0.05 eV / A, respectively; the cutoff energy and k-point grid are set to 105 Hartrees and 4×4×1, respectively.
[0024] Another object of the present invention is to provide a method for implementing the few-layer MoTe2 / CdS 0.42 Se 0.58 A method and system for preparing a thin-film heterojunction photodetector, the system comprising:
[0025] Thin-sheet preparation module for preparing CdS from cadmium sulfide 0.42 Se 0.58 Thin slices;
[0026] Photodetector preparation module, connected to the wafer preparation module, is used to utilize CdS 0.42 Se 0.58 MoTe2 / CdS thin film preparation 0.42 Se 0.58 Heterojunction photodetectors;
[0027] Computation module, connected to the photodetector preparation module, for MoTe2 / CdS 0.42 Se 0.58 First-principles calculations of heterojunction photodetectors.
[0028] Another object of the present invention is to provide a system for preparing the MoTe2 / CdS0.42Se0.58 thin film heterojunction photodetector as described above, the system comprising:
[0029] Heterostructure component module: It is composed of a few-layer MoTe2 / CdS0.42Se0.58 thin film heterostructure, in which the CdS0.42Se0.58 thin film contains Cd, S and Se elements.
[0030] Detection function module: Utilize the unique photoelectric properties of the above heterostructure for photoelectric detection.
[0031] Electrode construction module: This module includes Cr and Au materials to form electrodes for connecting and operating heterostructures.
[0032] Further, including:
[0033] Raw material preparation module: High-purity cadmium sulfide and cadmium selenide powders are mixed in a specific ratio to prepare CdS0.42Se0.58 flakes.
[0034] Temperature Control Module: Used to control the temperature in the tubular furnace to achieve suitable growth conditions for CdS0.42Se0.58 thin sheets.
[0035] Material transfer module: includes a two-dimensional material transfer system and PDMS film, used to transfer MoTe2 and CdS0.42Se0.58 flakes between different substrates.
[0036] Further, including:
[0037] Chemical Vapor Deposition (CVD) Module: Used to grow CdS0.42Se0.58 thin sheets in a quartz tube by chemical vapor deposition.
[0038] Mechanical exfoliation module: used to exfoliate few-layer MoTe2 flakes from bulk materials.
[0039] Electron beam evaporation equipment: used to deposit Cr and Au materials on silicon dioxide substrates to form electrode structures.
[0040] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows:
[0041] First, the few-layer MoTe2 / CdS prepared by the present invention 0.42 Se0.58 The thin-film heterojunction photodetector has excellent photoelectric performance and a high switching ratio of 1.73×10 4 , the response rate is high, which is 7221A / W, and the EQE is high, which is 1.52×10 6 %, the detection rate is even higher, at 1.67×10 15 cm Hz 1 / 2 W -1 and faster response speed (rise / fall time of 90 / 120μs); based on these results, the proposed photodetector outperforms other MoTe2-based photodetectors. First-principles calculations show that the superior performance of the proposed heterojunction photodetector is attributed to the unique band alignment at the interface. Finally, visible light imaging was successfully achieved on MoTe2 / CdS 0.42 Se 0.58 Photodetector devices. Based on these results, the few-layer MoTe2 / CdS 0.42 Se 0.58 Thin-film photodetectors have good application prospects in optoelectronic devices.
[0042] Second, the present invention prepares a few-layer MoTe2 / CdS 0.42 Se 0.58 High-performance photodetectors and MoTe2 / CdS 0.42 Se 0.58 The high responsivity of the thin-film heterojunction photodetector is 7221A / W, and the large current breaking ratio is 1.73×10 4 , fast response speed of 90 / 120μs, external quantum efficiency (EQE) up to 1.52×10 6 % and detection rate (D * ) reaches 1.67×10 15 cm Hz 1 / 2 W -1 The excellent performance of heterojunction photodetectors was analyzed through photocurrent mapping tests and first-principles calculations. 0.42 Se 0.58 The visible light imaging function was successfully obtained, which shows that the device has practical imaging application prospects. The results of this study provide a reference for the design of ultra-high performance MoTe2 based photodetectors.
[0043] Third, as auxiliary evidence of the inventiveness of the claims of the present invention, it is also reflected in the following important aspects:
[0044] (1) The technical solution of the present invention fills the technical gap in the industry at home and abroad:
[0045] MoTe2 / CdS 0.42 Se0.58 Heterojunction photodetectors are a new type of photodetector that uses different semiconductor materials to form a heterojunction to achieve efficient detection of optical signals. Compared with traditional two-dimensional material photodetectors, heterojunction photodetectors show higher performance and broader application prospects. First, the Institute of Metal Research, Chinese Academy of Sciences, in collaboration with scientific research teams from many domestic units, proposed a new method to improve optical gain. By selecting suitable channel and electrode materials for band matching, the potential barriers at the source and drain ends of the transistor are reduced under illumination and positive feedback is formed, thereby obtaining an ultra-high sensitivity two-dimensional material photodetector. Secondly, research progress on heterojunction photodetectors based on TMD two-dimensional materials such as tungsten disulfide (WS2), molybdenum disulfide (MoS2), and molybdenum ditelluride (MoTe2) has also been reported, but because their switching ratio limits their application in the technology industry, the MoTe2 / CdS prepared by us 0.42 Se 0.58 Heterojunction photodetectors fill the technical gaps in the industry at home and abroad in terms of heterojunction device structure design and new two-dimensional semiconductor processes. In addition, the research group of Associate Professor Liu Kai from the School of Materials Science and Engineering at Tsinghua University published a research paper titled "High-Performance Dual-Mode Photodetectors Based on Phase Change Modulation of WSe2 / VO2 Heterojunctions" in the journal Applied Physics Reviews published by the American Institute of Physics (AIP). The research of others and us has further promoted the development of heterojunction-based photodetector technology.
[0046] (2) The technical solution of the present invention solves a technical problem that people have been eager to solve but have never been able to solve successfully:
[0047] The present invention solves the technical problem of MoTe2 due to its small light-dark current ratio by constructing MoTe2 / CdS 0.42 Se 0.58 The heterogeneous structure significantly improves the switching ratio of the device.
[0048] Fourth, based on the design and fabrication of few-layer MoTe2 / CdS0.42Se0.58 thin-film heterojunction photodetectors, this technology has brought about the following significant technological advances:
[0049] 1) Improve the performance of photodetectors:
[0050] By utilizing the unique photoelectric properties of the MoTe2 and CdS0.42Se0.58 heterostructures, a higher photoelectric responsivity and spectral response range can be achieved, which means that the detector can capture and convert light energy more effectively, improving the photoelectric conversion efficiency.
[0051] 2) Enhance the stability and durability of the device:
[0052] The low-layer structure and optimized material combination make the device more stable and durable. This design reduces the performance degradation of the device in long-term use and prolongs its service life.
[0053] 3) Expand application areas:
[0054] Due to its efficient photoelectric conversion and broad spectral response, this heterojunction photodetector can be used in many fields such as solar cells, optical communications, light detection and imaging systems.
[0055] 4) More accurate spectral detection capability:
[0056] The MoTe2 / CdS0.42Se0.58 heterostructure provides more accurate spectral detection capabilities. This accuracy is particularly important for applications that require high-resolution spectral analysis (such as chemical composition analysis, biological imaging, etc.).
[0057] 5) Innovative preparation method:
[0058] The use of advanced chemical vapor deposition and mechanical exfoliation techniques enables precise preparation of high-quality heterostructures. This innovation not only improves manufacturing efficiency but also reduces production costs.
[0059] 6) Environmental friendliness and sustainability:
[0060] Environmental considerations in material selection and preparation, such as the use of non-toxic or low-toxic materials, make the entire production process more environmentally friendly and sustainable.
[0061] In general, this few-layer MoTe2 / CdS0.42Se0.58 thin film heterojunction photodetector shows significant technological progress in performance, stability, application range, preparation method and environmental protection, providing new opportunities for the development of photodetectors. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 The few-layer MoTe2 / CdS provided in the embodiment of the present invention 0.42 Se 0.58 Flow chart of the preparation method of thin-film heterojunction photodetector;
[0063] Figure 2 The preparation method of cadmium sulfur selenide CdS provided in the embodiment of the present invention is 0.42 Se 0.58 Flow chart of thin section method;
[0064] Figure 3 The MoTe2 / CdS provided in the embodiment of the present invention 0.42 Se 0.58Preparation flow chart of heterojunction photodetector method;
[0065] Figure 4 (a) XRD pattern, (b) PL, (c) EDS and (d) element distribution diagram of cadmium sulfide provided by the embodiment of the present invention 0.42 Se 0.58 Thin film; (e) Raman spectrum and (f) EDS map of few-layer MoTe2;
[0066] Figure 5 HRTEM images of (a) MoTe2 and (b) CdS provided in the embodiments of the present invention 0.42 Se 0.58 The inset is the corresponding FFT pattern. (c) AFM profile along the red line in the inset. The inset is a 2D AFM region of a single MoTe2 heterojunction device. (d) 3D AFM topography of a single MoTe2 and CdS 0.42 Se 0.58 region in a heterojunction device;
[0067] Figure 6 (a) IV curve of a few-layer MoTe2 flake provided in an embodiment of the present invention, a single CdS 0.42 Se 0.58 ,MoTe2 and MoTe2 / CdS 0.42 Se 0.58 At 1.5mW / cm 2 Sheet heterojunction device under white light. The inset is an optical image where the black arrow points to the selected test electrode (b) Responsivity as a function of illumination wavelength; (c) IV curves of the device under different light power densities; (d) Photocurrent variation with light power density and fitting; (e) Dependence of R, EQE and (f) D* on power density under 560nm light irradiation;
[0068] Figure 7 (a) Long cycle stability measurement of few-layer MoTe2 / CdS 0.42 Se 0.58 Heterojunction photodetector; (b) Response speed at a switching frequency of 1 kHz;
[0069] Figure 8 (a) Optical microscope image and (b) MoTe2 / CdS provided in the embodiment of the present invention 0.42 Se 0.58 Photocurrent mapping image of heterojunction device. (c) Calculated energy band diagram of MoTe2 / CdS 0.42 Se 0.58 Heterojunction;
[0070] Fig. 9(a) is a schematic diagram of an imaging measurement system provided by an embodiment of the present invention. (b) is an imaging result of the letter "U" under visible light;
[0071] Fig.10 The few-layer MoTe2 / CdS provided in the embodiment of the present invention 0.42 Se 0.58 Structural diagram of the fabrication system for thin-film heterojunction photodetectors. DETAILED DESCRIPTION
[0072] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0073] The embodiment of the present invention provides a few-layer MoTe2 / CdS 0.42 Se 0.58 Thin-film heterojunction photodetector, the device includes MoTe2 / CdS 0.42 Se 0.58 Thin-sheet heterojunction;
[0074] The CdS 0.42 Se 0.58 The flakes include: Cd, S and Se.
[0075] like Figure 1 As shown, the embodiment of the present invention provides a method for preparing the few-layer MoTe2 / CdS 0.42 Se 0.58 A method for preparing a thin-film heterojunction photodetector, the method comprising:
[0076] S1: CdS 0.42 Se 0.58 Preparation of thin slices;
[0077] S2: MoTe2 / CdS 0.42 Se 0.58 Preparation of heterojunction photodetectors;
[0078] S3: First principles calculations.
[0079] Further, the S1 specifically includes:
[0080] S11: combining high purity cadmium sulfide and cadmium selenide powders with a purity of 99.99% in a ceramic boat at a molar ratio of 1:1;
[0081] S12: placing the mixture in the central evaporation zone of the quartz tube;
[0082] S13: Cut the silicon wafer into pieces measuring 1.5×1.0 cm2 The thin slice was placed in a beaker containing acetone; ultrasonic cleaning was performed in the acetone solution for 10 minutes, and then cleaning was performed with ethanol and deionized water for 10 minutes; after the cleaning process, gold particles were sprayed on the silicon dioxide substrate, and the substrate was placed in the upstream and downstream areas of the quartz tube;
[0083] S14: The quartz tube is introduced into the tubular furnace, and the temperature is gradually increased to 835°C at a rate of 5.6°C / min. The system is maintained at this temperature for 150 minutes with a 95:5 ratio of Ar:H2 gas mixture at a flow rate of 17 sccm;
[0084] S15: When the tube furnace cools down to room temperature naturally, CdS is obtained. 0.42 Se 0.58 Flakes were obtained, and few-layer MoTe2 flakes were obtained by mechanical exfoliation.
[0085] like Figure 3 As shown, the S2 specifically includes:
[0086] S21: Cr and Au were sequentially deposited on a clean silicon dioxide substrate using an electron beam evaporation device to form an electrode with a channel length of 5 μm; the MoTe2 flakes were transferred to the gold electrode using a two-dimensional material transfer system;
[0087] S22: Preparation of CdS 0.42 Se 0.58 The thin film was immersed in an ethanol solution and then dropped onto another clean silica substrate. 0.42 Se 0.58 After the ethanol evaporated, the flakes remained on the substrate;
[0088] S23: CdS 0.42 Se 0.58 The flakes were separated from the initial substrate and transferred onto the top of the MoTe2 flakes using a PDMS film, thus completing the heterojunction construction.
[0089] The S3 specifically includes:
[0090] All first-principles calculations were performed within the framework of the DFTLCAO method, which is implemented in the QuantumATKT2022.03SP1 software package to simulate the trilayer MoTe2 / CdS 0.42 Se 0.58 A slab model consisting of 336 atoms was established; the projected density of states of the heterostructure was calculated more accurately using the HSE hybridization function.
[0091] The thickness of the vacuum layer of the flat plate model is ~22A, and the atomic ratio of Cd, S, and Se is 1:0.42:0.58 in CdS0.42 Se 0.58 The experimental values in are consistent; the structure optimization uses the GrimmeDFTD2 method to take into account the van der Waals correction; the total energy and force converge to a value of ~10 4 eV and 0.05 eV / A; the cutoff energy and k-point grid were set to 105 Hartrees and 4 × 4 × 1, respectively.
[0092] Figure 4 (a) shows CdS 0.42 Se 0.58 X-ray diffraction (XRD) pattern. Obviously, the diffraction peaks are consistent with the JCPDS No: 500720 standard card, in which the ratio of S to Se is 0.42:0.58. A small peak appears at about 2θ = 37.8°, which is related to the (203) diffraction peak of SiO2. The substrate peak of SiO2 is completely consistent with the JCPDS No: 471300 card. Figure 4 (b) represents CdS 0.42 Se 0.58 Photoluminescence (PL) spectrum. A peak was observed at a wavelength of 630 nm; starting from this peak, the band gap of CdS 0.42 Se 0.58 The calculated result is about 1.9 eV. Figure 4 (c) shows CdS 0.42 Se 0.58 Energy dispersive x-ray spectroscopy (EDS). Si, O, Cd, Se and S are all present in CdS 0.42 Se 0.58 In which Si and O come from SiO2 substrate. Figure 4 (d) CdS 0.42 Se 0.58 Elemental mapping images of these elements in CdS 0.42 Se 0.58 The scanning electron microscope after magnification shows that CdS 0.42 Se 0.58 The surface of the flakes is very smooth, showing the CdS 0.42 Se 0.58 Excellent crystalline quality of the flakes. Figure 4 (e) shows the Raman spectrum of a few-layer MoTe2 flake; the number of MoTe2 layers can be known based on the wave numbers of the three vibration modes, and the MoTe2 obtained by mechanical exfoliation is 3 layers. Figure 4(f) shows the EDS image of few-layer MoTe2. The EDS image clearly shows the presence of Mo, Te, O, and Si, providing solid evidence for the few-layer MoTe2 flakes. The MoTe2 flakes are composed of Mo and Te, while the O and Si elements can be attributed to the SiO2 substrate. The relatively low detection values of Te and Mo can be attributed to the thin MoTe2 and the abundant distribution of SiO2 on the substrate.
[0093] In order to further study the morphology, crystal structure and surface roughness of the prepared MoTe2 and CdS 0.42 Se 0.58 For thin sections, we performed high-resolution transmission electron microscopy (HRTEM) and atomic force microscopy (AFM) measurements. Figure 5 (a) and (b) show the HRTEM images of MoTe2 and CdS, respectively. 0.42 Se 0.58 Thin sheets; MoTe2 (101) and CdS 0.42 Se 0.58 The (002) plane of MoTe2 and CdS corresponds to lattice spacings of 0.29 and 0.31 nm, respectively. 0.42 Se 0.58 The fast Fourier transform (FFT) image (inset) shows that they have high-quality single-crystalline nanostructures. The thickness at the edge of the flake is 2.4 nm, indicating that the MoTe2 flakes are three-layer [ Figure 5 (c)], the results are consistent with the Raman spectroscopy analysis. Figure 5 (d)] shows the smooth surface of the as-prepared MoTe2 and CdS 0.42 Se 0.58 Thin slices.
[0094] Figure 6 (a) Drawing of a few layers of MoTe2 / CdS 0.42 Se 0.58 Current-voltage (IV) curves of a thin-film heterojunction photodetector under dark and white light illumination. For comparison, the IV characteristics of a single MoTe2 and CdS 0.42 Se 0.58 The device was also plotted under the same conditions. The photocurrent increases dramatically with the increase of bias voltage. At 5V, the MoTe2 device shows a lower on-off current ratio (~24) due to its high dark current. For CdS 0.42 Se 0.58 Device, the on-off current ratio reaches 1.87×10 3 Because of its high photocurrent and low dark current. When the two materials are hybridized to form a heterojunction, the photocurrent increases slightly (1.66×10 7A), while the dark current dropped by nearly an order of magnitude (9.62×10 12 A), with CdS 0.42 Se 0.58 This remarkable dark current suppression leads to a device on / off current ratio of 1.73×10 4 Therefore, MoTe2 / CdS 0.42 Se 0.58 Thin-film heterojunction photodetectors have strong photoelectric performance. Figure 6 (b) shows the spectral response of the heterojunction photodetector from 300 to 1600 nm. Obviously, the heterojunction device exhibits a strong response to visible light (400-600 nm) and near-infrared (1100-1400 nm) wavelengths, which is consistent with MoTe2 and CdS 0.42 Se 0.58 The band gaps correspond, and the excitons of both materials contribute to the photocurrent. Figure 6 (c) Few-layer MoTe2 / CdS 0.42 Se 0.58 IV curves of thin-film heterojunction photodetectors at different light intensities at 560nm. Obviously, at the same bias voltage, the photocurrent increases with the increase of light power density, indicating that the number of photogenerated carriers is proportional to the absorbed photon flux. When the light power density is 0.413mW / cm 2 When the photocurrent reaches 1.11×10 7 The calculation results show that the switching ratio of the device is 1.15×10 4 Compared to white light illumination, the on / off ratio is reduced but remains on the same order of magnitude. Figure 6 (d) shows the few-layer MoTe2 / CdS 0.42 Se 0.58 The relationship between the photocurrent and the optical power density of the photodetector when the bias voltage is 1V. According to the formula I = AP α , I is the photocurrent, A is the proportionality coefficient, P is the optical power density, and the exponent α is the fitting coefficient, which reflects the capture and recombination activity of photocarriers. The α value is determined to be 0.54 according to the above fitting formula; this result indicates that there are trap states in the contact interface, which affects the capture and recombination of photogenerated carriers.
[0095] In order to further study the few-layer MoTe2 / CdS 0.42 Se 0.58 The performance of the thin film and some key parameters of the heterojunction photodetector are calculated. As we all know, R, EQE and D * These are three important parameters for studying the optoelectronic performance of the device. These parameters can be calculated using the following formulas:
[0096]
[0097]
[0098]
[0099] I p represents the photocurrent, I d represents dark current, P represents light power density, A represents device area, h represents Planck constant, c represents speed of light, q represents electron charge, and λ represents incident wavelength. Figure 6 (ef) shows few-layer MoTe2 / CdS 0.42 Se 0.58 R, EQE and D of heterojunction photodetector under 5V bias * From Figure 6 (ef), R, EQE and D * As the optical power density increases, it decreases, which is mainly due to the fact that it is fully occupied by excited state photocarriers at high power density; this leads to a decrease in the available state density and a decrease in gain. 2 R, EQE and D under 5V bias * The maximum value is 7221A / W, 1.52×10 6 % and 1.67×10 15 cm Hz 1 / 2 W -1 These key parameters are much better than those of most reported MoTe2, indicating that our devices have excellent optoelectronic properties.
[0100] Cyclic stability and fast response speed are important parameters of photodetectors. Figure 7 Few-layer MoTe2 / CdS 0.42 Se 0.58 Heterojunction Photodetector. Figure 7 (a) MoTe2 / CdS 0.42 Se 0.58 It graph of the device under continuous switching cycles. Obviously, after the 2000-second cycle test, the on and off state changes are very small, with good stability and repeatability. Figure 7 (b) MoTe2 / CdS 0.42 Se 0.58 Graph of the photodetector response speed in a single switching state at 5V bias. The rise time is defined as the time required for the photocurrent to increase from 10% to 90%, while the fall time is defined as the time required for the photocurrent to decrease from 90% to 10% in one switching cycle. MoTe2 / CdS 0.42 Se 0.58Photodetectors are as short as 90 / 120μs respectively. MoTe2 / CdS 0.42 Se 0.58 The fast response speed of the photodetector can be attributed to the few-layer MoTe2 and CdS 0.42 Se 0.58 Good crystal quality and effective interface charge separation between them. Many studies have reported response speeds of milliseconds or even longer, which limits the practical application of photodetectors. In our study, MoTe2 / CdS 0.42 Se 0.58 The response time of the photodetector is reduced to only 90 μs, which is significantly lower than the values reported in many photodetector fields; therefore, our MoTe2 / CdS 0.42 Se 0.58 Photodetectors have broad application prospects.
[0101] To facilitate comparison with other reported studies, we summarize our MoTe2 / CdS 0.42 Se 0.58 Devices and based on reported MoTe2 and CdS x Se 1x The key parameters of the photodetector are shown in Table 1. Compared with other MoTe2 and CdS x Se 1x Compared with MoTe2 / CdS devices 0.42 Se 0.58 The device has excellent optoelectronic properties, such as high R, EQE and D * , faster response speed.
[0102] Table 1 Based on CdS x Se 1x Comparison of key parameters with MoTe2 photodetectors
[0103]
[0104] Figure 8 (a) shows the few-layer MoTe2 / CdS 0.42 Se 0.58 Optical image of heterojunction device, where the golden part is the interdigitated electrode. The width of the device channel is 5μm, MoTe2 / CdS 0.42 Se 0.58 The device area is 1.65×10 7 cm 2 To determine the photocurrent in MoTe2 / CdS 0.42 Se 0.58 We first studied the photocurrent imaging of the device under 560nm laser irradiation at a bias of 5V, such as Figure 8 (b) which corresponds to the green area in the figure. Figure 8 (a) From the photocurrent imaging results, the photocurrent is mainly distributed in MoTe2 and CdS 0.42 Se 0.58 The overlapped area of the sheets indicates that the photogenerated electron-hole pairs are effectively separated at the interface. This result indicates that the heterojunction photodetector has the same ability to separate photogenerated carriers as other vertical heterojunction devices. Next, we studied the 0.42 Se 0.58 Energy band arrangement at the interface between them based on first-principles calculations. Figure 8 (c) MoTe2 / CdS calculated using Quantum ATK software package 0.42 Se 0.58 Projected local density of states (PLDOS) of a heterojunction. CdS 0.42 Se 0.58 The band gaps of CdS and MoTe2 are 2.18eV and 0.96eV respectively, which is consistent with the experimental results. 0.42 Se 0.58 Diffusion into MoTe2 is driven by bias voltage, while holes in MoTe2 cannot move to CdS 0.42 Se 0.58 , which is due to the large energy barrier at the valence band and the accumulation of holes at the interface. Due to the smaller band gap of MoTe2 and the higher probability of recombination of the few electrons present in MoTe2 with the accumulated holes under dark conditions, it leads to lower dark current. Under illumination, CdS 0.42 Se 0.58 and MoTe2 absorb photons of different energies, generating a large number of photogenerated carriers. 0.42 Se 0.58 Move to MoTe2, and the holes on MoTe2 can also be easily transferred to CdS 0.42 Se 0.58 This is because the accumulation of a large number of holes in the valence band leads to a decrease in the energy barrier height. Therefore, the photogenerated carriers are effectively separated [see Figure 8 (c)]. The co-absorption and efficient separation of photogenerated carriers lead to the MoTe2 / CdS 0.42 Se 0.58 Higher photocurrent and responsivity of heterojunction photodetectors. As a result, the device exhibits higher photocurrent and lower dark current, and compared with other reported MoTe2 photodetectors, our heterojunction has higher responsivity, faster response speed, higher EQE and detectivity.
[0105] The imaging capability of photodetectors plays an important role in both civilian and military fields. We explored the 0.42 Se 0.58 The practical application potential of the photodetector was studied by using an imaging system [see Fig. 9 (a)]. The laser irradiates the heterojunction through a U-shaped mask. After being tested by a semiconductor analyzer and controlled by an imaging computer, the U-shaped pattern on the mask is successfully replicated. Fig. 9 (b) shows a uniform U-shaped photocurrent distribution, indicating that the prepared photodetector has good visible light imaging capability and confirms the few-layer MoTe2 / CdS 0.42 Se 0.58 Photodetectors have unique advantages in the field of imaging.
[0106] like Fig.10 As shown, the embodiment of the present invention provides a method for implementing the few-layer MoTe2 / CdS 0.42 Se 0.58 A method and system for preparing a thin-film heterojunction photodetector, the system comprising:
[0107] Thin-sheet preparation module for preparing CdS from CdS 0.42 Se 0.58 Thin slices;
[0108] Photodetector preparation module, connected to the wafer preparation module, is used to utilize CdS 0.42 Se 0.58 MoTe2 / CdS thin film preparation 0.42 Se 0.58 Heterojunction photodetectors;
[0109] Computation module, connected to the photodetector preparation module, for MoTe2 / CdS 0.42 Se 0.58 First-principles calculations of heterojunction photodetectors.
[0110] MoTe2 / CdS provided by the embodiment of the present invention 0.42 Se 0.58 Preparation method of thin-film heterojunction photodetector:
[0111] Example 1 CdS 0.42 Se 0.58 and preparation method of MoTe2
[0112] refer to Figure 2 , the CdS described in this embodiment 0.42 Se 0.58 The preparation method comprises the following steps:
[0113] S1: CdS 0.42 Se 0.58 Preparation of thin slices;
[0114] S2: MoTe2 / CdS 0.42 Se 0.58 Preparation of heterojunction photodetectors;
[0115] S3: First principles calculations.
[0116] Further, the S1 specifically includes:
[0117] S11: combining high purity cadmium sulfide and cadmium selenide powders with a purity of 99.99% in a ceramic boat at a molar ratio of 1:1;
[0118] S12: placing the mixture in the central evaporation zone of the quartz tube;
[0119] S13: Cut the silicon wafer into pieces measuring 1.5×1.0 cm 2 The thin slice was placed in a beaker containing acetone; ultrasonic cleaning was performed in the acetone solution for 10 minutes, and then cleaning was performed with ethanol and deionized water for 10 minutes; after the cleaning process, gold particles were sprayed on the silicon dioxide substrate, and the substrate was placed in the upstream and downstream areas of the quartz tube;
[0120] S14: The quartz tube is introduced into the tubular furnace, and the temperature is gradually increased to 835°C at a rate of 5.6°C / min. The system is maintained at this temperature for 150 minutes with a 95:5 ratio of Ar:H2 gas mixture at a flow rate of 17 sccm;
[0121] S15: When the tube furnace cools down to room temperature naturally, CdS is obtained. 0.42 Se 0.58 Flakes were obtained, and few-layer MoTe2 flakes were obtained by mechanical exfoliation.
[0122] Example 2 MoTe2 / CdS 0.42 Se 0.58 Preparation method
[0123] refer to Figure 3 , the MoTe2 / CdS described in this embodiment 0.42 Se 0.58 The preparation method comprises the following steps:
[0124] S21: Cr and Au were sequentially deposited on a clean silicon dioxide substrate using an electron beam evaporation device to form an electrode with a channel length of 5 μm; the MoTe2 flakes were transferred to the gold electrode using a two-dimensional material transfer system;
[0125] S22: Preparation of CdS 0.42 Se0.58 The thin film was immersed in an ethanol solution and then dropped onto another clean silica substrate. 0.42 Se 0.58 After the ethanol evaporated, the flakes remained on the substrate;
[0126] S23: CdS 0.42 Se 0.58 The flakes were separated from the initial substrate and transferred onto the top of the MoTe2 flakes using a PDMS film, thus completing the heterojunction construction.
[0127] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A few-layer MoTe2 / CdS 0.42 Se 0.58 A thin-film heterojunction photodetector, characterized in that: Including MoTe2 / CdS 0.42 Se 0.58 Thin-sheet heterojunction; The CdS 0.42 Se 0.58 The flakes include: Cd, S and Se; Preparation of the few-layer MoTe2 / CdS 0.42 Se 0.58 A method for preparing a thin-film heterojunction photodetector, comprising: S1: CdS 0.42 Se 0.58 Preparation of thin slices; S2: MoTe2 / CdS 0.42 Se 0.58 Fabrication of heterojunction photodetectors; S3: First principles calculations; MoTe2 / CdS 0.42 Se 0.58 The method for preparing a thin-sheet heterojunction, wherein S1 specifically comprises: S11: combining high purity cadmium sulfide and cadmium selenide powders with a purity of 99.99% in a ceramic boat at a molar ratio of 1:1; S12: placing the mixture in the central evaporation zone of the quartz tube; S13: Cut the silicon wafer into pieces measuring 1.5×1.0 cm 2 The thin slice was placed in a beaker containing acetone; ultrasonic cleaning was performed in the acetone solution for 10 minutes, and then cleaning was performed with ethanol and deionized water for 10 minutes; after the cleaning process, gold particles were sprayed on the silicon dioxide substrate, and the substrate was placed in the upstream and downstream areas of the quartz tube; S14: The quartz tube is introduced into the tubular furnace, and the temperature is gradually increased to 835°C at a rate of 5.6°C / min; the system is maintained at this temperature for 150 minutes with a 95:5 ratio of Ar:H2 gas mixture at a flow rate of 17 sccm; S15: When the tube furnace cools down to room temperature naturally, CdS is obtained. 0.42 Se 0.58 Flakes, few-layer MoTe2 flakes were obtained by mechanical exfoliation; MoTe2 / CdS 0.42 Se 0.58 Thin-sheet heterojunction photodetector, wherein S2 specifically comprises: S21: Cr and Au were sequentially deposited on a clean silicon dioxide substrate using an electron beam evaporation device to form an electrode with a channel length of 5 μm; the MoTe2 flakes were transferred to the gold electrode using a two-dimensional material transfer system; S22: Preparation of CdS 0.42 Se 0.58 The thin film was immersed in an ethanol solution and then dropped onto another clean silica substrate. 0.42 Se 0.58 After the ethanol evaporated, the flakes remained on the substrate; S23: CdS 0.42 Se 0.58 The flakes were separated from the initial substrate and transferred onto the top of the MoTe2 flakes using a PDMS film, thus completing the heterojunction construction.
2. The few-layer MoTe2 / CdS as claimed in claim 1 0.42 Se 0.58 A thin-film heterojunction photodetector, characterized in that: The method for preparing a heterojunction photodetector, wherein S3 specifically comprises: All first-principles calculations were performed within the framework of the DFTLCAO method, which is implemented in the QuantumATKT2022.03SP1 software package to simulate the trilayer MoTe2 / CdS 0.42 Se 0.58 A slab model consisting of 336 atoms was established; the projected density of states of the heterostructure was calculated more accurately using the HSE hybridization function.
3. The few-layer MoTe2 / CdS as claimed in claim 2 0.42 Se 0.58 A thin-film heterojunction photodetector, characterized in that: A method for preparing a heterojunction photoelectric detector, wherein the vacuum layer thickness of the flat plate model is 22A, and the atomic ratio of Cd, S, and Se is consistent with the experimental value of 1:0.42:0.58 in cadmium sulfur and selenium; The structure optimization uses the GrimmeDFTD2 method to take into account the van der Waals correction; the total energy and force converge to values of 10 4 eV and 0.05 eV / A; the cutoff energy and k-point grid were set to 105 Hartrees and 4 × 4 × 1, respectively.
4. A method for implementing the few-layer MoTe2 / CdS as claimed in any one of claims 1 and 3 0.42 Se 0.58 A system for preparing a thin-film heterojunction photodetector, characterized in that: The system includes: Heterostructure component module: composed of a few-layer MoTe2 / CdS0.42Se0.58 thin sheet heterostructure, where the CdS0.42Se0.58 thin sheet contains Cd, S and Se elements; Detection function module: utilizing the unique photoelectric properties of the above heterostructures for photoelectric detection; Electrode construction module: This module includes Cr and Au materials to form electrodes for connecting and operating heterostructures.
5. The preparation system according to claim 4, characterized in that: include: Raw material preparation module: Mix high-purity cadmium sulfide and cadmium selenide powders to prepare CdS0.42Se0.58 flakes; Temperature control module: used to control the temperature in the tubular furnace to achieve suitable growth conditions for CdS0.42Se0.58 thin sheets; Material transfer module: includes a two-dimensional material transfer system and PDMS film, used to transfer MoTe2 and CdS0.42Se0.58 flakes between different substrates.
6. The preparation system according to claim 4, characterized in that: include: Chemical vapor deposition (CVD) module: used to grow CdS0.42Se0.58 thin sheets in a quartz tube by chemical vapor deposition; Mechanical exfoliation module: used to exfoliate few-layer MoTe2 flakes from bulk materials; Electron beam evaporation equipment: used to deposit Cr and Au materials on silicon dioxide substrates to form electrode structures.