A carbon-reducing asphalt mixture and mineral powder and its preparation method
By loading Al(OH)3 and Mg(OH)2 onto steel slag-based mineral powder, an asphalt mixture with carbon reduction function was prepared, which solved the problems of high carbon emissions and difficulty in resource utilization of asphalt pavement in the existing technology, and achieved low-cost, effective carbon emission reduction and improved road performance.
Patent Information
- Application Number
- CN202410149286.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-02
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-02-02
AI Technical Summary
The construction of existing asphalt pavements generates a large amount of carbon dioxide, and existing carbon reduction technologies are costly or have poor road performance, making it difficult to achieve effective carbon emission reduction and resource utilization.
Using steel slag as a carrier, Al(OH)3 and Mg(OH)2 are loaded onto steel slag-based mineral powder. Taking advantage of their porous adsorption properties, asphalt mixtures with carbon reduction function are prepared, thereby reducing carbon emissions and improving adhesion to asphalt.
It realizes the resource utilization of steel slag, reduces the carbon emissions of asphalt mixtures, reduces processing costs, and has good road performance and stability, making it suitable for large-scale production.
Smart Images

Figure CN118164698B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of solid waste resource utilization technology, specifically relating to an asphalt mixture with carbon reduction function, mineral powder, and preparation method. Background Technology
[0002] With the increasing severity of global climate change and environmental pollution, carbon emission reduction has become a common concern for countries worldwide. The steel industry, as a high-energy-consuming and high-emission sector, generates steel slag during its production process, which not only occupies a large amount of land resources but also causes serious environmental pollution. Based on the experience of developed countries in the application of steel slag, road construction is a key area for the resource utilization of steel slag. Therefore, how to effectively utilize steel slag solid waste, turning "solid waste" into "resource treasure," and achieving resource recycling and carbon emission reduction has become an urgent problem to be solved by the industry.
[0003] Meanwhile, asphalt pavement is widely used in the highway transportation industry due to its good driving comfort and excellent performance. However, asphalt pavement construction requires high-temperature mixing, which generates a large amount of carbon dioxide. To reduce carbon emissions, technologies such as warm mix and cold mix paving, which aim to lower the construction temperature, have emerged. However, these methods still have disadvantages such as high operating costs and poor road performance.
[0004] Therefore, overcoming the shortcomings of existing technologies is a problem that urgently needs to be solved in this field. Summary of the Invention
[0005] The purpose of this invention is to overcome the shortcomings of existing technologies and provide an asphalt mixture with carbon reduction function, mineral powder, and its preparation method. The mineral powder possesses excellent adsorption properties and stable chemical properties, effectively adsorbing and fixing carbon dioxide generated during asphalt mixture production, thereby achieving carbon emission reduction. Simultaneously, it imparts strong alkalinity to the mineral powder, improving its adhesion to asphalt, and reduces costs due to the use of steel slag solid waste materials. The preparation method of this invention is simple, low-cost, and easily achievable for large-scale production.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing an asphalt mixture with carbon-reducing function includes the following steps:
[0008] Step (1) involves crushing and screening the steel slag, and then grinding it into mineral powder for asphalt mixtures to obtain steel slag-based mineral powder.
[0009] Step (2): Take AlCl3·6H2O and MgCl2·6H2O, add them to distilled water to dissolve them to form a solution containing AlCl3 and MgCl2, then add steel slag-based mineral powder to the solution to completely absorb the solution, and stir until uniform to obtain wet steel slag-based mineral powder.
[0010] Step (3): Dry the wet steel slag-based ore powder at 105℃, then cool it naturally to room temperature to obtain a cooled material; then add NH3·H2O solution with a mass fraction of 4% to 6% to the cooled material, stir and react for 9 min to 11 min, filter, take the filter residue, wash it with distilled water, and then dry it at 105℃ to obtain steel slag-based ore powder with carbon reduction function; the Al(OH)3 loading of the steel slag-based ore powder with Al(OH)3 / Mg(OH)2 is 1% to 7%, and the Mg(OH)2 loading is 1% to 7%;
[0011] Step (4): Add the Al(OH)3 / Mg(OH)2 loaded steel slag-based mineral powder to the asphalt mixture and mix evenly to obtain an asphalt mixture with carbon reduction function;
[0012] Of which, by mass percentage, coarse aggregate is 56%–71%, fine aggregate is 28%–40%, steel slag-based mineral powder loaded with Al(OH)3 / Mg(OH)2 is 1%–4%, totaling 100%, and asphalt is 4%–5% of the total aggregate mass; the total aggregate mass is the sum of the mass of coarse aggregate and fine aggregate.
[0013] Further, in step (1), grinding is carried out by a grinding mill; the mineral powder for the asphalt mixture is specifically: the sieve passing rate of <0.6mm is 100%, the sieve passing rate of <0.15mm is 90% to 100%, and the sieve passing rate of <0.075mm is 75% to 100%.
[0014] Furthermore, in step (2), the mass ratio of distilled water to steel slag-based mineral powder is 3.4-3.6:1.
[0015] Furthermore, in step (3), the volume ratio of NH3·H2O solution to distilled water used in step (2) is 50:8-12; the number of times of washing with distilled water is 2; and the drying time after washing is 3 hours.
[0016] Furthermore, in step (3), the loading ratio of Al(OH)3 to Mg(OH)2 is 1:1.
[0017] Furthermore, in step (4), the particle size requirement for coarse aggregate is: 4.75mm < particle size < 26.5mm; the particle size requirement for fine aggregate is: particle size < 4.75mm.
[0018] The present invention also provides a carbon-reducing loaded Al(OH)3 / Mg(OH)2 steel slag-based mineral powder prepared by the above-mentioned method for preparing asphalt mixture with carbon-reducing function.
[0019] This invention also provides a method for preparing supported Al(OH)3 / Mg(OH)2 steel slag-based mineral powder with carbon reduction function, comprising the following steps:
[0020] Step (1) involves crushing and screening the steel slag, and then grinding it into mineral powder for asphalt mixtures to obtain steel slag-based mineral powder.
[0021] Step (2): Take AlCl3·6H2O and MgCl2·6H2O, add them to distilled water to dissolve them to form a solution containing AlCl3 and MgCl2, then add steel slag-based mineral powder to the solution to completely absorb the solution, and stir until uniform to obtain wet steel slag-based mineral powder.
[0022] Step (3): Dry the wet steel slag-based ore powder at 105℃, and then cool it naturally to room temperature to obtain a cooled material; then add NH3·H2O solution with a mass fraction of 4% to 6% to the cooled material, stir and react for 9 min to 11 min, filter, take the filter residue, wash it with distilled water, and then dry it at 105℃ to obtain steel slag-based ore powder with carbon reduction function; the Al(OH)3 loading of the steel slag-based ore powder with Al(OH)3 / Mg(OH)2 is 1% to 7%, and the Mg(OH)2 loading is 1% to 7%.
[0023] Further, in step (1), grinding is carried out by a grinding mill; the mineral powder for the asphalt mixture is specifically: the sieve passing rate of <0.6mm is 100%, the sieve passing rate of <0.15mm is 90% to 100%, and the sieve passing rate of <0.075mm is 75% to 100%.
[0024] Furthermore, in step (2), the mass ratio of distilled water to steel slag-based mineral powder is 3.4-3.6:1.
[0025] Furthermore, in step (3), the volume ratio of NH3·H2O solution to distilled water used in step (2) is 50:8-12; the number of times of washing with distilled water is 2; and the drying time after washing is 3 hours.
[0026] Furthermore, in step (3), the loading ratio of Al(OH)3 to Mg(OH)2 is 1:1.
[0027] To reduce carbon emissions, current main measures include warm-mix asphalt and cold-mix paving, both aimed at lowering production temperatures. Warm-mix methods lower the temperature by approximately 30°C compared to hot-mix methods, but are more expensive; cold-mix paving allows for construction at room temperature, but significantly reduces road performance and durability. This invention develops an asphalt mixture with carbon-reducing properties, along with mineral powder and its preparation method. This method is simple, easy to operate, and has no impact on the production process. It achieves both the resource utilization of steel slag and the reduction of carbon emissions, which is of great significance for building a resource-saving and environmentally friendly beautiful China.
[0028] This invention utilizes the porous adsorption characteristics of steel slag to load Al(OH)3 and Mg(OH)2 onto steel slag-based mineral powder, which can effectively reduce the carbon emissions of asphalt mixtures and achieve the goal of "treating waste with waste".
[0029] Compared with the prior art, the beneficial effects of this invention are as follows:
[0030] (1) This invention uses steel slag as a carrier to realize the resource utilization of steel slag. At the same time, by utilizing the porous adsorption characteristics of steel slag, Al(OH)3 and Mg(OH)2 are loaded on steel slag-based mineral powder, which can effectively reduce the carbon emissions of asphalt mixtures.
[0031] (2) The method of the present invention is simple and easy to operate, requires no complex equipment, reduces processing costs, is easy to promote and apply, and is suitable for large-scale production.
[0032] (3) This invention can truly achieve “waste treatment”, with no pollution, low cost and good stability, which is conducive to the effective utilization of steel slag resources and environmental protection. Attached Figure Description
[0033] Figure 1 The following are field photos of the AC-10 steel slag thin-layer overlay test section of G213 line; (a) paving process; (b) operation status.
[0034] Figure 2 The diagram shows the paving process of the SMA-13 steel slag test section of the G5621 Xinkunchu Expressway; (a) paving process; (b) road surface condition.
[0035] Figure 3 The images show the operational monitoring data for the SMA-13 steel slag test section of the G5621 Xinkunchu Expressway; (a) is a tracking test image of the lateral force coefficient; and (b) is a test image of the comprehensive pavement performance.
[0036] Figure 4 The following are on-site photos of the steel slag test section of the Tongjian Expressway; (a) completed paving view; (b) on-site testing view.
[0037] Figure 5SEM-EDS images of Al(OH)3 / Mg(OH)2 steel slag-based mineral powder with carbon reduction function; where (a) is the SEM image; (b) is the energy spectrum of Al distribution; and (c) is the energy spectrum of Mg distribution. Detailed Implementation
[0038] The present invention will now be described in further detail with reference to the embodiments.
[0039] Those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be construed as limiting the scope of the invention. Where specific techniques or conditions are not specified in the embodiments, they are performed in accordance with the techniques or conditions described in the literature in the field or according to the product instructions. Materials or equipment whose manufacturers are not specified are all conventional products that can be obtained by purchase.
[0040] Example 1
[0041] A method for preparing an asphalt mixture with carbon-reducing function includes the following steps:
[0042] Step (1) involves crushing and screening the steel slag, and then grinding it into mineral powder for asphalt mixtures to obtain steel slag-based mineral powder.
[0043] Step (2): Take AlCl3·6H2O and MgCl2·6H2O, add them to distilled water to dissolve them to form a solution containing AlCl3 and MgCl2, then add steel slag-based mineral powder to the solution to completely absorb the solution, and stir until uniform to obtain wet steel slag-based mineral powder.
[0044] Step (3): The wet steel slag-based mineral powder is dried at 105℃ and then naturally cooled to room temperature to obtain a cooled material. Then, a 5% NH3·H2O solution is added to the cooled material, the mixture is stirred and reacted for 10 min, filtered, and the filter residue is washed with distilled water and then dried at 105℃ to obtain a steel slag-based mineral powder with carbon reduction function. The Al(OH)3 loading of the steel slag-based mineral powder with Al(OH)3 / Mg(OH)2 is 3%, and the Mg(OH)2 loading is 4%.
[0045] Step (4): Add the Al(OH)3 / Mg(OH)2 loaded steel slag-based mineral powder to the asphalt mixture and mix evenly to obtain an asphalt mixture with carbon reduction function;
[0046] Of which, by mass percentage, coarse aggregate accounts for 60%, fine aggregate 37%, steel slag-based mineral powder loaded with Al(OH)3 / Mg(OH)2 accounts for 3%, totaling 100%, and asphalt accounts for 4.5% of the total aggregate mass; the total aggregate mass is the sum of the mass of coarse aggregate and fine aggregate.
[0047] Example 2
[0048] A method for preparing an asphalt mixture with carbon-reducing function includes the following steps:
[0049] Step (1) involves crushing and screening the steel slag, and then grinding it into mineral powder for asphalt mixtures to obtain steel slag-based mineral powder.
[0050] Step (2): Take AlCl3·6H2O and MgCl2·6H2O, add them to distilled water to dissolve them to form a solution containing AlCl3 and MgCl2, then add steel slag-based mineral powder to the solution to completely absorb the solution, and stir until uniform to obtain wet steel slag-based mineral powder.
[0051] Step (3): Dry the wet steel slag-based mineral powder at 105°C and then cool it naturally to room temperature to obtain a cooled material; then add 4% NH3·H2O solution to the cooled material, stir for 9 min, filter, wash the filter residue with distilled water, and then dry it at 105°C to obtain loaded Al(OH)3 / Mg(OH)2 steel slag-based mineral powder with carbon reduction function;
[0052] Step (4): Add the Al(OH)3 / Mg(OH)2 loaded steel slag-based mineral powder to the asphalt mixture and mix evenly to obtain an asphalt mixture with carbon reduction function;
[0053] Of which, by mass percentage, coarse aggregate is 56%, fine aggregate is 40%, steel slag-based mineral powder loaded with Al(OH)3 / Mg(OH)2 is 4%, totaling 100%, and asphalt is 4% of the total aggregate mass; the total aggregate mass is the sum of the mass of coarse aggregate and fine aggregate.
[0054] In step (1), grinding is carried out by a grinding mill; the mineral powder for the asphalt mixture is specifically: the sieve passing rate of <0.6mm is 100%, the sieve passing rate of <0.15mm is 90% to 100%, and the sieve passing rate of <0.075mm is 75% to 100%.
[0055] In step (2), the mass ratio of distilled water to steel slag-based mineral powder is 3.4:1.
[0056] In step (3), the volume ratio of NH3·H2O solution to distilled water used in step (2) is 50:8; the number of times of washing with distilled water is 2; the drying time after washing is 3h; the Al(OH)3 loading of Al(OH)3 / Mg(OH)2 steel slag-based ore powder is 1%, and the Mg(OH)2 loading is 1%.
[0057] In step (4), the particle size requirement for coarse aggregate is: 4.75mm < particle size < 26.5mm; the particle size requirement for fine aggregate is: particle size < 4.75mm.
[0058] Example 3
[0059] A method for preparing an asphalt mixture with carbon-reducing function includes the following steps:
[0060] Step (1) involves crushing and screening the steel slag, and then grinding it into mineral powder for asphalt mixtures to obtain steel slag-based mineral powder.
[0061] Step (2): Take AlCl3·6H2O and MgCl2·6H2O, add them to distilled water to dissolve them to form a solution containing AlCl3 and MgCl2, then add steel slag-based mineral powder to the solution to completely absorb the solution, and stir until uniform to obtain wet steel slag-based mineral powder.
[0062] Step (3): Dry the wet steel slag-based mineral powder at 105℃, and then cool it naturally to room temperature to obtain a cooled material; then add 6% NH3·H2O solution to the cooled material, stir and react for 11 min, filter, take the filter residue, wash it with distilled water, and then dry it at 105℃ to obtain loaded Al(OH)3 / Mg(OH)2 steel slag-based mineral powder with carbon reduction function;
[0063] Step (4): Add the Al(OH)3 / Mg(OH)2 loaded steel slag-based mineral powder to the asphalt mixture and mix evenly to obtain an asphalt mixture with carbon reduction function;
[0064] Of which, by mass percentage, coarse aggregate is 71%, fine aggregate is 28%, steel slag-based mineral powder loaded with Al(OH)3 / Mg(OH)2 is 1%, totaling 100%, and asphalt is 5% of the total mass of aggregate; the total mass of aggregate is the sum of the mass of coarse aggregate and fine aggregate.
[0065] In step (1), grinding is carried out by a grinding mill; the mineral powder for the asphalt mixture is specifically: the sieve passing rate of <0.6mm is 100%, the sieve passing rate of <0.15mm is 90% to 100%, and the sieve passing rate of <0.075mm is 75% to 100%.
[0066] In step (2), the mass ratio of distilled water to steel slag-based mineral powder is 3.6:1.
[0067] In step (3), the volume ratio of NH3·H2O solution to distilled water used in step (2) is 50:12; the number of times of washing with distilled water is 2; the drying time after washing is 3h; the Al(OH)3 loading of the Al(OH)3 / Mg(OH)2 steel slag-based ore powder is 7%, and the Mg(OH)2 loading is 7%.
[0068] In step (3), the loading ratio of Al(OH)3 to Mg(OH)2 is 1:1.
[0069] In step (4), the particle size requirement for coarse aggregate is: 4.75mm < particle size < 26.5mm; the particle size requirement for fine aggregate is: particle size < 4.75mm.
[0070] Example 4
[0071] A method for preparing an asphalt mixture with carbon-reducing function includes the following steps:
[0072] Step (1) involves crushing and screening the steel slag, and then grinding it into mineral powder for asphalt mixtures to obtain steel slag-based mineral powder.
[0073] Step (2): Take AlCl3·6H2O and MgCl2·6H2O, add them to distilled water to dissolve them to form a solution containing AlCl3 and MgCl2, then add steel slag-based mineral powder to the solution to completely absorb the solution, and stir until uniform to obtain wet steel slag-based mineral powder.
[0074] Step (3): Dry the wet steel slag-based mineral powder at 105°C, and then cool it naturally to room temperature to obtain a cooled material; then add 5% NH3·H2O solution to the cooled material, stir and react for 10 min, filter, take the filter residue, wash it with distilled water, and then dry it at 105°C to obtain loaded Al(OH)3 / Mg(OH)2 steel slag-based mineral powder with carbon reduction function;
[0075] Step (4): Add the Al(OH)3 / Mg(OH)2 loaded steel slag-based mineral powder to the asphalt mixture and mix evenly to obtain an asphalt mixture with carbon reduction function;
[0076] Of which, by mass percentage, coarse aggregate is 65%, fine aggregate is 32%, steel slag-based mineral powder loaded with Al(OH)3 / Mg(OH)2 is 3%, totaling 100%, and asphalt is 4.4% of the total aggregate mass; the total aggregate mass is the sum of the mass of coarse aggregate and fine aggregate.
[0077] In step (1), grinding is carried out by a grinding mill; the mineral powder for the asphalt mixture is specifically: the sieve passing rate of <0.6mm is 100%, the sieve passing rate of <0.15mm is 90% to 100%, and the sieve passing rate of <0.075mm is 75% to 100%.
[0078] In step (2), the mass ratio of distilled water to steel slag-based mineral powder is 3.5:1.
[0079] In step (3), the volume ratio of NH3·H2O solution to distilled water used in step (2) is 50:10; the number of times of washing with distilled water is 2; the drying time after washing is 3h; the Al(OH)3 loading of the Al(OH)3 / Mg(OH)2 steel slag-based ore powder is 4%, and the Mg(OH)2 loading is 4%, that is, the loading ratio of Al(OH)3 to Mg(OH)2 is 1:1.
[0080] In step (4), the particle size requirement for coarse aggregate is: 4.75mm < particle size < 26.5mm; the particle size requirement for fine aggregate is: particle size < 4.75mm.
[0081] Example 5
[0082] A method for preparing Al(OH)3 / Mg(OH)2 supported steel slag-based mineral powder with carbon reduction function includes the following steps:
[0083] Step (1) involves crushing and screening the steel slag, and then grinding it into mineral powder for asphalt mixtures to obtain steel slag-based mineral powder.
[0084] Step (2): Take AlCl3·6H2O and MgCl2·6H2O, add them to distilled water to dissolve them to form a solution containing AlCl3 and MgCl2, then add steel slag-based mineral powder to the solution to completely absorb the solution, and stir until uniform to obtain wet steel slag-based mineral powder.
[0085] Step (3): Dry the wet steel slag-based mineral powder at 105°C and then cool it naturally to room temperature to obtain a cooled material. Then add 4% NH3·H2O solution to the cooled material, stir for 9 min, filter, wash the filter residue with distilled water, and then dry it at 105°C to obtain a loaded Al(OH)3 / Mg(OH)2 steel slag-based mineral powder with carbon reduction function.
[0086] In step (1), grinding is carried out by a grinding mill; the mineral powder for the asphalt mixture is specifically: the sieve passing rate of <0.6mm is 100%, the sieve passing rate of <0.15mm is 90% to 100%, and the sieve passing rate of <0.075mm is 75% to 100%.
[0087] In step (2), the mass ratio of distilled water to steel slag-based mineral powder is 3.4:1.
[0088] In step (3), the volume ratio of NH3·H2O solution to distilled water used in step (2) is 50:8; the number of times of washing with distilled water is 2; the drying time after washing is 3h; the Al(OH)3 loading of Al(OH)3 / Mg(OH)2 steel slag-based ore powder is 1%, and the Mg(OH)2 loading is 1%.
[0089] Example 6
[0090] A method for preparing Al(OH)3 / Mg(OH)2 supported steel slag-based mineral powder with carbon reduction function includes the following steps:
[0091] Step (1) involves crushing and screening the steel slag, and then grinding it into mineral powder for asphalt mixtures to obtain steel slag-based mineral powder.
[0092] Step (2): Take AlCl3·6H2O and MgCl2·6H2O, add them to distilled water to dissolve them to form a solution containing AlCl3 and MgCl2, then add steel slag-based mineral powder to the solution to completely absorb the solution, and stir until uniform to obtain wet steel slag-based mineral powder.
[0093] Step (3): Dry the wet steel slag-based mineral powder at 105°C and then cool it naturally to room temperature to obtain a cooled material. Then add 6% NH3·H2O solution to the cooled material, stir and react for 11 min, filter, take the filter residue, wash it with distilled water, and then dry it at 105°C to obtain loaded Al(OH)3 / Mg(OH)2 steel slag-based mineral powder with carbon reduction function.
[0094] In step (1), grinding is carried out by a grinding mill; the mineral powder for the asphalt mixture is specifically: the sieve passing rate of <0.6mm is 100%, the sieve passing rate of <0.15mm is 90% to 100%, and the sieve passing rate of <0.075mm is 75% to 100%.
[0095] In step (2), the mass ratio of distilled water to steel slag-based mineral powder is 3.6:1.
[0096] In step (3), the volume ratio of NH3·H2O solution to distilled water used in step (2) is 50:12; the number of times of washing with distilled water is 2; the drying time after washing is 3h; the Al(OH)3 loading of the Al(OH)3 / Mg(OH)2 steel slag-based ore powder is 7%, and the Mg(OH)2 loading is 7%.
[0097] In step (3), the loading ratio of Al(OH)3 to Mg(OH)2 is 1:1.
[0098] Example 7
[0099] A method for preparing Al(OH)3 / Mg(OH)2 supported steel slag-based mineral powder with carbon reduction function includes the following steps:
[0100] Step (1) involves crushing and screening the steel slag, and then grinding it into mineral powder for asphalt mixtures to obtain steel slag-based mineral powder.
[0101] Step (2): Take AlCl3·6H2O and MgCl2·6H2O, add them to distilled water to dissolve them to form a solution containing AlCl3 and MgCl2, then add steel slag-based mineral powder to the solution to completely absorb the solution, and stir until uniform to obtain wet steel slag-based mineral powder.
[0102] Step (3): Dry the wet steel slag-based mineral powder at 105°C and then cool it naturally to room temperature to obtain a cooled material. Then add 5% NH3·H2O solution to the cooled material, stir and react for 10 min, filter, take the filter residue, wash it with distilled water, and then dry it at 105°C to obtain loaded Al(OH)3 / Mg(OH)2 steel slag-based mineral powder with carbon reduction function.
[0103] In step (1), grinding is carried out by a grinding mill; the mineral powder for the asphalt mixture is specifically: the sieve passing rate of <0.6mm is 100%, the sieve passing rate of <0.15mm is 90% to 100%, and the sieve passing rate of <0.075mm is 75% to 100%.
[0104] In step (2), the mass ratio of distilled water to steel slag-based mineral powder is 3.5:1.
[0105] In step (3), the volume ratio of NH3·H2O solution to distilled water used in step (2) is 50:10; the number of times of washing with distilled water is 2; the drying time after washing is 3h; the Al(OH)3 loading of the Al(OH)3 / Mg(OH)2 steel slag-based ore powder is 4%, and the Mg(OH)2 loading is 4%, that is, the loading ratio of Al(OH)3 to Mg(OH)2 is 1:1.
[0106] Application Examples
[0107] This invention provides an asphalt mixture with carbon reduction function, mineral powder, and preparation method. After steel slag is ground into mineral powder, Al(OH)3 / Mg(OH)2 is loaded onto it to produce an asphalt mixture with carbon reduction function, which plays the role of "treating waste with waste".
[0108] The specific method is as follows:
[0109] 1. First, the steel slag is crushed and screened. Then, the steel slag is ground into mineral powder for asphalt mixture through a grinding mill. The passing rate of the sieve with a particle size of <0.6mm is 100%, the passing rate of the sieve with a particle size of <0.15mm is 90-100%, and the passing rate of the sieve with a particle size of <0.075mm is 75-100%.
[0110] 2. To obtain steel slag-based mineral powder with a loading of 1-7% Al(OH)3 / Mg(OH)2, AlCl3 and MgCl2 are first loaded onto the steel slag-based mineral powder using an equal volume absorption method. Then, AlCl3 and MgCl2 are reacted in situ with excess NH3·H2O on the inner surface of the steel slag-based mineral powder. The loading ratio of Al(OH)3 to Mg(OH)2 is 1:1.
[0111] Sample preparation example:
[0112] Taking the preparation of steel slag-based mineral powder with a loading of 4% Al(OH)3 / Mg(OH)2 as an example:
[0113] Weigh 2g of AlCl3·6H2O and 1.79g of MgCl2·6H2O into a 200mL beaker, add 93g of distilled water to dissolve them, forming a solution containing AlCl3 and MgCl2.
[0114] In a separate small beaker, weigh out 29.92 g of steel slag-based mineral powder. The mass ratio of distilled water to steel slag-based mineral powder is controlled at 3.5 to ensure that the steel slag-based mineral powder can completely absorb the solution containing AlCl3 and MgCl2.
[0115] Pour the steel slag-based mineral powder into the solution containing AlCl3 and MgCl2, and stir until the powder has completely absorbed the AlCl3 and MgCl2 solutions. Place the wet steel slag-based mineral powder that has absorbed the AlCl3 and MgCl2 solutions into an oven at 105°C and dry it, stirring occasionally, until it reaches a constant weight.
[0116] After drying, remove the powder from the oven and allow it to cool naturally to room temperature in a desiccator. Add 500 mL of a 5% (w / w) NH3·H2O solution, stir for 10 min, filter, wash the steel slag-based ore powder twice with distilled water, and then place it in a 105℃ oven to dry for 3 h. Remove and cool in a desiccator for later use. The loading amounts of Al(OH)3 and Mg(OH)2 can be calculated based on the amounts of AlCl3·6H2O, MgCl2·6H2O, and steel slag-based ore powder added.
[0117]
[0118]
[0119] 3. Add the steel slag-based mineral powder loaded with Al(OH)3 / Mg(OH)2 to the asphalt mixture and mix evenly to obtain an asphalt mixture with carbon reduction function (i.e., carbon emission reduction asphalt mixture);
[0120] Of which, by mass percentage, coarse aggregate is 56%–71%, fine aggregate is 28%–40%, steel slag-based mineral powder loaded with Al(OH)3 / Mg(OH)2 is 1%–4%, totaling 100%, and asphalt is 4%–5% of the total aggregate mass; the total aggregate mass is the sum of the mass of coarse aggregate and fine aggregate.
[0121] 4. Take a clean 200mL beaker and weigh 100.00g±0.1g of asphalt mixture with carbon reduction function.
[0122] 5. Turn on the constant temperature heating plate of the CO2 emission concentration measuring device and set the temperature to 200℃. Simultaneously, turn on the CO2 detector of the CO2 emission concentration measuring device. After the constant temperature heating plate stabilizes at 200℃ for 30 minutes, place the beaker containing the asphalt mixture sample with carbon reduction function on the constant temperature heating plate. Immediately cover the system with a glass cover and start timing, continuously recording the CO2 concentration in the cover. The increase in CO2 concentration is considered as the CO2 produced by the sample being heated, i.e., the carbon emission concentration.
[0123] The experimental results are shown in Table 1.
[0124] Table 1. Effect of adding steel slag-based mineral powder on carbon emission concentration of asphalt mixtures (ppm)
[0125]
[0126]
[0127] The experimental results show that:
[0128] (1) The addition of steel slag-based mineral powder has a positive effect on carbon emission reduction of asphalt mixtures under heating. However, the trend shows that the increase in CO2 emission concentration of asphalt mixtures under heating mainly occurs in the later stage, that is, when the asphalt heating temperature rises to a higher level. This means that the carbon emission reduction effect of steel slag-based mineral powder on asphalt mixtures under low-temperature conditions is more obvious, while the carbon emission reduction effect under high-temperature conditions is poor. The main reason is that under high-temperature conditions, the oxidation reaction between the light components of asphalt and air intensifies, and the adsorption effect of steel slag-based mineral powder on the light components of asphalt binder is not enough to inhibit the increasingly intensified oxidation reaction. To this end, this invention loads Al(OH)3 / Mg(OH)2 onto steel slag-based mineral powder, utilizing the endothermic and flame-retardant effects of Al(OH)3 and Mg(OH)2 (quenching oxygen free radicals), and synergistically with the adsorption effect of the mixture, to further reduce the CO2 emission concentration of asphalt under heating.
[0129] (2) Steel slag-based mineral powder has a rich porous structure. After loading Al(OH)3 / Mg(OH)2, the surface is relatively rough with obvious fibrous and lamellar crystals. Combined with CO2 emission concentration and SEM-EDS (such as... Figure 5 The test results show that Al(OH)3 and Mg(OH)2 have been efficiently attached to the surface of steel slag-based mineral powder. The loaded steel slag-based mineral powder has a further promoting effect on reducing the CO2 emission concentration of asphalt mixtures when heated. The emission reduction effect is: loaded Al(OH)3 / Mg(OH)2 steel slag-based mineral powder > steel slag-based mineral powder >> no additives.
[0130] (3) The loading of Al(OH)3 and Mg(OH)2 has a certain impact on the CO2 emission concentration of asphalt mixtures under heating. Under the same heating time, the CO2 emission concentration of steel slag-based mineral powder with a loading of 4% Al(OH)3 / Mg(OH)2 is lower than 2% and 6%, respectively, indicating that there is an optimal loading of Al(OH)3 / Mg(OH)2. A low loading results in a smaller endothermic and flame-retardant effect of Al(OH)3 / Mg(OH)2, contributing less to the carbon emission reduction of asphalt mixtures; a high loading may cause pore blockage, which is detrimental to reducing the carbon emission concentration of asphalt mixtures. For steel slag-based mineral powder loaded with Al(OH)3 / Mg(OH)2, a balance needs to be found between adsorption performance and endothermic and flame-retardant performance to achieve the optimal comprehensive effect. The carbon emission reduction of steel slag-based mineral powder with a loading of 4% Al(OH)3 / Mg(OH)2 within 1 hour reached over 90%, demonstrating a significant emission reduction effect.
[0131] (4) Steel slag-based mineral powder loaded with Al(OH)3 / Mg(OH)2 showed the best carbon emission reduction effect on asphalt mixtures. Compared with ordinary mineral powder ground from limestone, the carbon emission concentration was reduced by 94.3% after heating for 10 min; 90.7% after heating for 20 min; 90.1% after heating for 30 min; 90.2% after heating for 40 min; 90.7% after heating for 50 min; and 90.5% after heating for 60 min.
[0132] (5) Loading Al(OH)3 / Mg(OH)2 steel slag-based mineral powder can reduce CO2 emissions from asphalt mixtures. The main reason is that the high free energy generated by the high specific surface area of steel slag-based mineral powder allows asphalt gas to adhere to the surface and gradually diffuse into the internal pores. The gas is then fixed in the pores of the steel slag-based mineral powder due to intermolecular forces. Simultaneously, Al(OH)3 and Mg(OH)2 absorb a large amount of heat when heated, carrying away heat from the asphalt surface and lowering the surface temperature, thereby reducing the generation of gas. Therefore, the adsorption performance of steel slag-based mineral powder and the endothermic performance of Al(OH)3 / Mg(OH)2 exhibit a good synergistic effect.
[0133] 6. Verification of engineering performance of asphalt mixtures with carbon reduction function
[0134] Taking AC-16 as an example, the properties of asphalt mixtures with carbon reduction function are as follows:
[0135] Table 2. Proportions of Various Minerals in AC-16C
[0136]
[0137] Table 3. Results of the AC-16C Marshall test
[0138]
[0139] Table 4 shows the performance test results of AC-16C mixture.
[0140]
[0141] The test results above show that the water stability, permeability, high temperature stability, and low temperature crack resistance of AC-16C asphalt mixture with carbon reduction function can meet the technical requirements of the "Technical Specification for Construction of Highway Asphalt Pavement" (JTG F40-2004).
[0142] Project Implementation Cases:
[0143] (1) In May 2020, a 300m test section of AC-10 thin-layer overlay was paved on the G213 line from Huize Steel Plant to Xundian Huaqingshao section (this section is subject to heavy traffic). The AC-10 asphalt mixture used in this invention is an asphalt mixture with carbon reduction function, such as... Figure 1 This marks the first time that steel slag solid waste has been applied to asphalt pavement engineering in Yunnan Province. The road section has been in operation for three and a half years, during which time multiple follow-up visits and tracking have been conducted. All relevant indicators meet the technical requirements, with its skid resistance and attenuation performance being far superior to that of conventional asphalt pavement.
[0144] (2) In September and December 2021, SMA-13 (such as...) was laid in the road surface project of the G5621 New Kunming-Chuxiong Expressway. Figure 2 and Figure 3 The AC-20C and AC-25C test sections all used the asphalt mixture with carbon reduction function of this invention. The paving length is about 3.0km. This is the first time that steel slag solid waste has been applied to highway asphalt pavement engineering in Yunnan Province. The road section has been in operation for 2 years and the pavement is in good service condition during the operation period.
[0145] (3) On June 30, 2023, Longjian Yuxi Engineering Co., Ltd. successfully paved 500m of asphalt mixture pavement with carbon reduction function on the long longitudinal slope section from K13+600 to K14+100 of the Tongjian Expressway. After testing, all indicators met the relevant technical requirements, and the water permeability and anti-skid performance were excellent.
[0146] From September 20 to 22, 2023, the Department of Comprehensive Planning of the Ministry of Transport conducted a survey on the utilization of solid waste resources in Yunnan Province. During the survey, the team visited the Kunming-Chuxiong Expressway to observe and learn in detail about the application of steel slag asphalt pavement test sections for heavy-duty traffic upper, middle and lower layers. They highly affirmed Yunnan Province's policy guarantees, advanced practices and experience in promoting the construction of a beautiful China's transportation system and the intensive, economical and circular use of resources.
[0147] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely illustrative of the principles of the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of this invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing an asphalt mixture with carbon-reducing function, characterized in that, Includes the following steps: Step (1): Crush and screen the steel slag, and grind it into mineral powder for asphalt mixture to obtain steel slag-based mineral powder; Step (2): Take AlCl3·6H2O and MgCl2·6H2O, add them to distilled water to dissolve them and form a solution containing AlCl3 and MgCl2. Then add steel slag-based mineral powder to the solution to completely absorb the solution and stir until uniform to obtain wet steel slag-based mineral powder. Step (3): The wet steel slag-based ore powder is dried at 105℃ and then naturally cooled to room temperature to obtain a cooled material; then, a 4%~6% NH3·H2O solution is added to the cooled material, the mixture is stirred for 9min-11min, filtered, the filter residue is washed with distilled water, and then dried at 105℃ to obtain a steel slag-based ore powder with carbon reduction function; the Al(OH)3 loading of the Al(OH)3 / Mg(OH)2 steel slag-based ore powder is 1%~7%, and the Mg(OH)2 loading is 1%~7%; Step (4): Add the Al(OH)3 / Mg(OH)2 steel slag-based mineral powder loaded with Al(OH)3 / Mg(OH)2 to the asphalt mixture and mix evenly to obtain an asphalt mixture with carbon reduction function; Of which, by mass percentage, coarse aggregate is 56%~71%, fine aggregate is 28%~40%, steel slag-based mineral powder loaded with Al(OH)3 / Mg(OH)2 is 1%~4%, totaling 100%, and asphalt is 4%~5% of the total aggregate mass; the total aggregate mass is the sum of the mass of coarse aggregate and fine aggregate. In step (1), grinding is carried out by a grinding mill; the mineral powder for asphalt mixture specifically has the following characteristics: 100% pass rate for sieves with a particle size of <0.6mm, 90%~100% pass rate for sieves with a particle size of <0.15mm, and 75%~100% pass rate for sieves with a particle size of <0.075mm; In step (2), the mass ratio of distilled water to steel slag-based mineral powder is 3.4-3.6:
1.
2. The method for preparing asphalt mixture with carbon-reducing function according to claim 1, characterized in that, In step (3), the volume ratio of NH3·H2O solution to distilled water used in step (2) is 50:8-12; the number of times the distilled water is used for washing is 2; and the drying time after washing is 3 hours.
3. The method for preparing asphalt mixture with carbon-reducing function according to claim 2, characterized in that, In step (3), the loading ratio of Al(OH)3 to Mg(OH)2 is 1:
1.
4. The method for preparing asphalt mixture with carbon-reducing function according to claim 1, characterized in that, In step (4), the particle size requirement for coarse aggregate is: 4.75mm < particle size < 26.5mm; the particle size requirement for fine aggregate is: particle size < 4.75mm.
5. Carbon-reducing loaded Al(OH)3 / Mg(OH)2 steel slag-based mineral powder prepared by the method for preparing asphalt mixture with carbon-reducing function according to any one of claims 1 to 4.
6. A method for preparing Al(OH)3 / Mg(OH)2 supported steel slag-based mineral powder with carbon reduction function, characterized in that, Includes the following steps: Step (1): Crush and screen the steel slag, and grind it into mineral powder for asphalt mixture to obtain steel slag-based mineral powder; Step (2): Take AlCl3·6H2O and MgCl2·6H2O, add them to distilled water to dissolve them and form a solution containing AlCl3 and MgCl2. Then add steel slag-based mineral powder to the solution to completely absorb the solution and stir until uniform to obtain wet steel slag-based mineral powder. Step (3): Dry the wet steel slag-based mineral powder at 105℃, and then cool it naturally to room temperature to obtain the cooled material; then add NH3·H2O solution with a mass fraction of 4%~6% to the cooled material, stir and react for 9min-11min, filter, take the filter residue, wash it with distilled water, and then dry it at 105℃ to obtain the loaded Al(OH)3 / Mg(OH)2 steel slag-based mineral powder with carbon reduction function.
Citation Information
Patent Citations
Application of magnesium hydroxide-loaded wood flour in asphalt carbon emission reduction
CN114231045A
Application of aluminum hydroxide-loaded wood flour in asphalt carbon emission reduction
CN114249983A
Asphalt mixture utilizing slag micropowder as filler
CN1891758A