A composite catalyst for catalyzing cyclic ether polymerization and its preparation method and application
By combining the reactions of metal salts and functional silicon sources in catalyst preparation, a composite catalyst with suitable acidity is prepared, which solves the problems of corrosiveness and molecular weight distribution of existing catalysts in cyclic ether polymerization, and achieves high conversion rate and low color. No. 1 polymer production, suitable for high-end fabrics and medical care and other fields.
Patent Information
- Application Number
- CN202410592837.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-05-14
AI Technical Summary
Existing catalysts have problems in catalyzing the polymerization of cyclic ether compounds, such as strong corrosiveness, stringent equipment requirements, unreasonable acidity, high color number of the produced polymer, excessive molecular weight distribution, and low activity. It is difficult to meet the needs of products in the fields of high-end fabrics and medical care. Mass and molecular weight distribution requirements.
The first component containing a suitable metal salt is reacted with a functional silicon source in a solvent. After stirring, standing, drying and roasting steps, a composite catalyst with suitable acidity is prepared, which is combined with Lewis acid and Bronsted acidic sites. Catalyzes the ring-opening polymerization of cyclic ethers.
It achieves high conversion rate and narrow molecular weight distribution of the catalyst, reduces energy consumption and environmental pollution, simplifies the preparation process, avoids corrosive problems, and performs the catalytic reaction at a lower temperature, maintaining a low color number of the reaction solution.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalyst preparation, and specifically relates to a composite catalyst for catalyzing cyclic ether polymerization and a preparation method and application thereof. Background Art
[0002] Cyclic ether compounds are easy to polymerize, have rich structures and functional groups, are widely available, and are renewable. They are excellent monomers for synthesizing heterochain polymer materials. Using 3-8-membered rings such as ethylene oxide, propylene oxide, and tetrahydrofuran as monomers, various types of polymer materials can be obtained through ring-opening polymerization and copolymerization. Cyclic ether compounds can also be copolymerized with homologous cyclic ether monomers to obtain polymers with richer side group compositions. For example, they can be copolymerized with many non-epoxy compounds such as cyclic esters, cyclic anhydrides, carbon dioxide and its derivatives in random, alternating, and block reactions to generate polymers with main chain structures significantly different from side chains. With the development of industry and society, the functions and quality of various polymer materials have become more refined. Catalysts and process control are of great significance for accurately regulating and controlling the structure and properties of cyclic ether polymers. The catalytic polymerization of cyclic ether compounds is mainly divided into several catalytic systems such as ions, proton acids, and Lewis acids. Specific catalysts form complexes and ion pairs with initiators, thereby initiating the ring-opening polymerization of cyclic ethers.
[0003] Different catalysts can adjust the polymerization rate, molecular weight distribution, and the ratio and connection mode of the repeating blocks in the copolymerization product, so as to synthesize cyclic ether polymer materials that meet different needs. The catalysts currently used for catalyzing the polymerization of cyclic ether compounds have some problems, such as high corrosiveness, strict equipment requirements, and high color number of the product. Therefore, it is necessary to develop a new catalytic system.
[0004] The catalytic system of cyclic ether compounds can be divided into catalytic systems such as cationic ring-opening polymerization, anionic ring-opening polymerization and coordination ring-opening polymerization. Cationic ring-opening polymerization catalysts mainly include proton acids and Lewis acids. Alkali metal hydroxides and alcohol salts can be used to catalyze anionic ring-opening polymerization of cyclic ether compounds. Commonly used catalysts include potassium hydroxide, sodium hydroxide, potassium alcoholate and sodium alcoholate.
[0005] Acidic catalysts such as Lewis acid and fluorosulfonic acid have been used in the prior art to synthesize cyclic ether polymer materials. For example, US5180856A uses a boron trifluoride catalyst to polymerize tetrahydrofuran and glycerol ether in the presence of an alkanol. US4481123A discloses a method for polymerizing α-epoxyalkylenes having an alkyl group of 8 to 26 carbon atoms using a Lewis acid catalyst.
[0006] However, the acidic catalysts used in the prior art for catalyzing the polymerization of cyclic ether compounds have the following problems: (1) The catalysts are extremely corrosive and have strict requirements on equipment; (2) The acidity of the catalysts is unreasonable, resulting in a high color number and a wide molecular weight distribution of the generated polymer; (3) The activity of the catalysts is relatively low, resulting in low polymerization conversion rates or complex processing procedures during the manufacturing process. As downstream customers of polyethers (especially in the fields of high-end fabrics, medical care, etc.) continue to increase their requirements for product quality and molecular weight distribution, the field urgently needs to develop new catalytic systems to solve these problems. Summary of the invention
[0007] The purpose of the present invention is to provide a novel composite catalyst for catalyzing cyclic ether polymerization, and a preparation method and application thereof. The method of the present invention prepares the composite catalyst by selecting a first component containing a suitable metal salt and a functional silicon source, and by appropriate steps of dissolving, stirring, isothermal reaction, drying and calcining. The composite catalyst of the present invention has suitable acidity and has Lewis acid and Bronsted acid acid sites. The composite catalyst of the present invention can exhibit special performance in catalyzing cyclic ether ring-opening polymerization reaction through the combination of the two acid sites.
[0008] The first aspect of the present invention provides a method for preparing a composite catalyst, comprising the steps of:
[0009] (1) dissolving the metal salt in a solvent and stirring evenly to obtain a first component;
[0010] (2) adding a silicon source to the first component, allowing the silicon source to react with the metal salt, and allowing the reaction to stand;
[0011] (3) removing the solvent and drying to obtain dry powder;
[0012] (4) calcining the dried powder to obtain the composite catalyst;
[0013] The metal element in the metal salt is selected from one or more of Al, Zn, Sn, Fe, Ti, Zr and Hf; the anion in the metal salt is selected from one or more of halide ion, nitrate ion, sulfate ion, oxygen ion, carboxylate ion and alcohol ion;
[0014] The silicon source is selected from one or more of tetraethoxysilane, tetramethoxysilane, polysilane and silicon tetrachloride.
[0015] In one or more embodiments, in step (1), the solvent is an organic solvent and / or water, and the organic solvent is preferably an alcohol solvent, such as a monohydric alcohol containing 1 to 4 carbon atoms.
[0016] In one or more embodiments, the solvent is a mixed solvent of an alcohol solvent and water, and in the mixed solvent, the volume ratio of the alcohol solvent to water is preferably (3-5): 1.
[0017] In one or more embodiments, the metal element in the metal salt is selected from one or more of Al, Ti and Zr, and the anion in the metal salt is selected from one or more of chloride ion, oxygen ion and nitrate ion.
[0018] In one or more embodiments, the metal salt is selected from one or more of zirconium oxynitrate, titanium tetrachloride, and aluminum nitrate.
[0019] In one or more embodiments, in step (2), the reaction is carried out for 4-48 hours, preferably 4-24 hours.
[0020] In one or more embodiments, the reaction is carried out at 40-80°C, preferably at 60-80°C.
[0021] In one or more embodiments, in step (2), the standing time is 12-48 hours, preferably 24-30 hours.
[0022] In one or more embodiments, in step (2), the concentration of the metal salt in the solvent is 0.05-1 mol / L, preferably 0.1-0.5 mol / L.
[0023] In one or more embodiments, in step (2), the concentration of the silicon source in the solvent is 0.2-4 mol / L, preferably 0.4-2 mol / L.
[0024] In one or more embodiments, in step (2), the molar ratio of the metal ions contained in the metal salt to the silicon atoms contained in the silicon source is 1: (3-10), preferably 1: (4-5).
[0025] In one or more embodiments, in step (3), the solvent is removed by centrifugation or gas stripping to obtain insoluble matter, and the insoluble matter is dried.
[0026] In one or more embodiments, in step (3), the drying temperature is 30-200°C.
[0027] In one or more embodiments, in step (3), the drying time is 1-12 hours.
[0028] In one or more embodiments, in step (4), the calcination temperature is 400-1500°C, preferably 600-1200°C.
[0029] In one or more embodiments, in step (4), the calcination time is 1-12 hours.
[0030] In one or more embodiments, the method further comprises the step of: (5) extruding and pelletizing the composite catalyst.
[0031] The second aspect of the present invention provides a composite catalyst prepared by the method described in the first aspect of the present invention.
[0032] In one or more embodiments, the specific surface area of the composite catalyst is ≥250 m 2 / g.
[0033] In one or more embodiments, the acidity of the composite catalyst is 0.02-0.2 mmol / g.
[0034] In one or more embodiments, the amount of acid on the surface of the composite catalyst is 0.40-0.70 mg.
[0035] In one or more embodiments, in the composite catalyst, the molar ratio of silicon to the metal is 3.5:1-4.5:1.
[0036] The third aspect of the present invention provides a use of the composite catalyst described in the second aspect of the present invention in catalyzing the ring-opening polymerization of cyclic ether compounds to produce polyether polymers.
[0037] In one or more embodiments, the cyclic ether compound is an optionally substituted 3-8 membered cyclic ether compound.
[0038] The present invention has the following beneficial effects:
[0039] 1. The composite catalyst synthesized by the present invention has suitable acidity, and has Lewis acid and Bronsted acid acid sites at the same time, and can show suitable acidity through the combination of the two acid sites, thereby showing a higher conversion rate and a narrower molecular weight distribution in the cyclic ether ring-opening polymerization reaction. The conversion rate of the polymerization reaction catalyzed by the composite catalyst of the present invention can reach more than 45%, for example, more than 48%, more than 50%, more than 55%, more than 60%, more than 65%, and the molecular weight distribution index of the obtained polymer can reach less than 2.3, for example, less than 2.25, less than 2.1, less than 2.0, less than 1.9, less than 1.8, less than 1.7.
[0040] 2. The composite catalyst preparation method of the present invention is simple and does not require the use of an acidic medium. The catalyst can be obtained by reacting the first component containing the metal salt with the functional silicon source in an organic solvent and then calcining it. The catalyst of the present invention is non-corrosive, avoiding the problems of the prior art in which the use of corrosive catalysts has stringent requirements on equipment and complicated processing procedures.
[0041] 3. The composite catalyst of the present invention can be used for the ring-opening polymerization of cyclic ether compounds to generate polyether polyesters or polyether polyols, and has a wide range of applications. Applicable cyclic ether compounds include cyclic ethers such as ethylene oxide, propylene oxide, THF, hexyl oxide, and derivatives of the above cyclic ethers containing side chains or substituents. The number average molecular weight of the obtained polyether polyester or polyether polyol product ranges from 50 to 10,000.
[0042] 4. The composite catalyst of the present invention can carry out catalytic reaction at a relatively low temperature, which is beneficial to reducing energy consumption and environmental pollution.
[0043] 5. The use of the composite catalyst of the present invention to catalyze the ring-opening polymerization of cyclic ethers can enable the reaction system to reach equilibrium in a shorter time. After the reaction reaches equilibrium, the reaction liquid can still maintain a lower color level after a long reaction time, thereby making the obtained polyether polyester or polyether polyol product have a lower color number.
[0044] In summary, the cyclic ether ring-opening polymerization reaction catalyzed by the composite catalyst of the present invention has a higher conversion rate than the prior art, and its polymerization product has a narrower molecular weight distribution. The preparation method of the composite catalyst of the present invention is simple, and its application range is wide. It has the advantages of low energy consumption and environmental pollution when used in catalytic reactions. DETAILED DESCRIPTION
[0045] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0046] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0047] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.
[0048] In this document, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible sub-ranges and individual values within the range (including integers and fractions).
[0049] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.
[0050] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.
[0051] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0052] The present invention provides a method for preparing a composite catalyst, comprising the steps of:
[0053] (1) dissolving the metal salt in a solvent and stirring evenly to obtain a first component;
[0054] (2) adding a silicon source to the first component, allowing the silicon source to react with the metal salt, and allowing the reaction to stand;
[0055] (3) removing the solvent and drying to obtain dry powder;
[0056] (4) Calcine the dried powder to obtain a composite catalyst.
[0057] In step (1), the metal element in the metal salt can be selected from one or more of Al, Zn, Sn, Fe, Ti, Zr and Hf. In some embodiments, the metal element in the metal salt is selected from one or more of Al, Ti and Zr. The anion in the metal salt can be selected from one or more of halide ions, nitrate ions, sulfate ions, oxygen ions, carboxylate ions and alcohol ions. Herein, halide ions include fluoride ions, chloride ions, bromide ions, iodide ions, preferably chloride ions. Herein, oxygen ions refer to O 2-. Herein, carboxylate ion refers to an anion formed by a carboxylic acid molecule losing hydrogen from a carboxyl group. Carboxylate ions may be C1-C6 carboxylate ions, such as C1 carboxylate ions, C2 carboxylate ions, C3 carboxylate ions, C4 carboxylate ions, C5 carboxylate ions, and C6 carboxylate ions. In the text, the carbon number before an ion or compound indicates the number of carbon atoms contained in the ion or compound, such as C1 carboxylate ion indicates a carboxylate ion containing 1 carbon atom (i.e., formate ion). Herein, alcoholate ion refers to an anion formed by an alcohol molecule losing hydrogen from a hydroxyl group. Alcoholate ions may be C1-C6 alcoholate ions, such as C1 alcoholate ions, C2 alcoholate ions, C3 alcoholate ions, C4 alcoholate ions, C5 alcoholate ions, and C6 alcoholate ions. In some embodiments, the anion in the metal salt is selected from one or more of chloride ions, oxygen ions, and nitrate ions. In some embodiments, the metal salt is selected from one or more of chlorides, nitrates, oxynitrates, and alcoholates. Herein, nitrate refers to a metal salt whose anion is a nitrate ion, oxynitrate refers to a metal salt whose anion is a nitrate ion and an oxygen ion, and alkoxide refers to a compound in which the hydrogen in the hydroxyl group in the alcohol molecule is replaced by one or more metals selected from Al, Zn, Sn, Fe, Ti, Zr and Hf. Herein, alkoxide may be a salt formed by replacing the hydroxyl hydrogen of C1-C6 alcohol (e.g., C1 alcohol, C2 alcohol, C3 alcohol, C4 alcohol, C5 alcohol, C6 alcohol) with the metal described herein, including but not limited to methoxide, ethoxide, propoxide, aluminum alcohol, titanium alcohol, zirconium alcohol. Preferably, the metal salt is selected from one or more of chloride, nitrate and oxynitrate, such as zirconium nitrate, titanium tetrachloride, aluminum nitrate. The solvent may be an organic solvent and / or water. Preferably, the solvent is a mixed solvent of an organic solvent and water. The organic solvent may be an alcohol solvent, for example, a monohydric alcohol containing 1-4 carbon atoms, including but not limited to methanol, ethanol, propanol, butanol. In some embodiments, the solvent is a mixed solvent of an alcohol solvent and water. In the mixed solvent, the volume ratio of the alcohol solvent to water can be (3-5): 1, for example 4:1.
[0058] In step (2), the silicon source may be selected from one or more of tetraethoxysilane, tetramethoxysilane, polysilane and silicon tetrachloride. Preferably, the silicon source is tetraethoxysilane. The reaction may be carried out for 4-48 hours, for example, 8 hours, 12 hours, 18 hours, 24 hours, 30 hours, 36 hours, 40 hours. The reaction is preferably carried out for 4-24 hours. The reaction may be carried out at 40-80°C, for example, 40°C, 50°C, 60°C, 70°C, 80°C. The reaction is preferably carried out at 60-80°C. The standing time may be 12-48 hours, for example, 12 hours, 18 hours, 24 hours, 30 hours, 36 hours, 40 hours. The standing time is preferably 24-30 hours, 24-48 hours. After the reaction in step (2) generates a gel compound, stirring is stopped and the mixture is kept standing at a constant temperature, which is conducive to the structural stability of the gel compound.
[0059] The concentration of the metal salt in the solvent may be 0.05-1 mol / L, for example, 0.08 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, 0.5 mol / L, 0.7 mol / L, 0.9 mol / L. The concentration of the metal salt in the solvent is preferably 0.1-0.5 mol / L. The concentration of the silicon source in the solvent may be 0.2-4 mol / L, for example, 0.4 mol / L, 0.6 mol / L, 0.8 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L. The concentration of the silicon source in the solvent is preferably 0.4-2 mol / L. The molar ratio of the metal ions contained in the metal salt to the silicon atoms contained in the silicon source may be 1: (3-10), for example, 1: 3, 1: 4, 1: 5, 1: 6, 1: 8. The molar ratio of the metal ions contained in the metal salt to the silicon atoms contained in the silicon source is preferably 1: (4-5).
[0060] In step (3), the solvent is removed by centrifugation or gas stripping to obtain insoluble matter, and the insoluble matter is dried. The gas stripping method is preferably carried out using an inert gas, such as nitrogen or argon. The drying temperature may be 30-200°C, for example, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 150°C, 180°C. The drying time may be 1-12 hours, for example, 2 hours, 3 hours, 5 hours, 8 hours, 10 hours.
[0061] In step (4), the calcination temperature may be 400-1500°C, for example, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1200°C, 1300°C. The calcination temperature is preferably 600-1200°C. The calcination time may be 1-12 hours, for example, 2 hours, 3 hours, 5 hours, 8 hours, 10 hours. The calcination may be carried out in an air atmosphere or under the protection of an inert gas (for example, nitrogen or argon).
[0062] The method of the present invention further comprises the step of: (5) extruding and granulating the composite catalyst. The composite catalyst prepared by extrusion and granulation is shaped to be cylindrical, strip, capsule, spherical or other special shapes.
[0063] The present invention provides a composite catalyst prepared by the method of the present invention. The specific surface area of the composite catalyst of the present invention is ≥250m 2 / g, for example ≥260m 2 / g, ≥270m 2 / g, ≥280m 2 / g, ≥290m 2 / g, ≥300m 2 / g, ≥310m 2 / g, ≥320m 2 / g, ≥325m 2 / g. The specific surface area of the composite catalyst of the present invention is measured by the BET method. The amount of acid on the surface of the composite catalyst is 0.40-0.70mg. The amount of acid of the composite catalyst of the present invention can be measured by an ion exchange method. The suitable acidity of the composite catalyst is 0.02-0.2mmol / g, for example, 0.02 mmol / g, 0.04 mmol / g, 0.05 mmol / g, 0.06 mmol / g, 0.08mmol / g, 0.1 mmol / g, 0.13 mmol / g, 0.15 mmol / g, 0.18 mmol / g. In some embodiments, the acidity of the composite catalyst is 0.02-0.05 mmol / g. In the composite catalyst, the molar ratio of silicon to metal is 3.5:1-4.5:1. In some embodiments, in the composite catalyst, the molar ratio of silicon to metal is 4:1.
[0064] The present invention provides an application of the catalyst of the present invention in catalyzing the ring-opening polymerization of a cyclic ether compound to generate a polyether polymer.
[0065] The cyclic ether compound is an optionally substituted 3- to 8-membered cyclic ether compound, for example, ethylene oxide, propylene oxide, tetrahydrofuran (THF), hexyl oxide.
[0066] As used herein, "optionally" or "optionally" means that the event or situation described subsequently may or may not occur, and the description includes both the occurrence and non-occurrence of the event or situation. For example, "optionally substituted 3-8 membered cyclic ether compound" means that the cyclic ether compound is substituted or unsubstituted, and the description includes both substituted cyclic ether compounds and unsubstituted cyclic ether compounds. The "optional" substituents described in the present invention are selected from alkyl, alkenyl, alkynyl, alkoxy, halogen, haloalkyl, haloalkenyl, haloalkynyl, cyano, carboxyl, hydroxyl, nitro, triphenylphosphino, azido, aldehyde, optionally substituted aryl, optionally substituted heteroaryl, optionally substituted cycloalkyl, and optionally substituted heterocyclic.
[0067] As used herein, the term "substituted", whether or not preceded by the term "optionally" (i.e., equivalent to substituted or unsubstituted), refers to the replacement of one or more hydrogens of a specified group or part by a "suitable substituent". Herein, the number of substituents may be one or more, i.e., 1, 2, 3, 4, 5, or 6 or more, depending on the substituted group and the nature of the substituent. For example, when the substituent of an ethyl group is a halogen, the group may be substituted by 1, 2, 3, 4, or 5 substituents, such as trifluoroethyl, pentafluoroethyl, etc., depending on the structure of the substituted group. In some embodiments, the number of the substituents is 1, 2, or 3. In some embodiments, the number of the substituents is 1 or 2. In some embodiments, the number of the substituents is 1. It will be understood that "substituted" or "substituted by..." includes implicit conditions, i.e., such substitutions are carried out according to the allowed valence of the substituted atom, and the substitution produces a stable or chemically feasible compound, such as a compound that does not spontaneously transform, such as by rearrangement, cyclization, elimination, etc. Unless otherwise indicated, an "optionally substituted" group may have a suitable substituent at each substitutable position of the group, and when more than one position in any given structure may be substituted by more than one substituent selected from a specified group, the substituent may be the same or different at each position. It will be understood by those skilled in the art that the substituent itself may be substituted if appropriate. Unless specifically indicated as "unsubstituted", chemical moieties referred to herein should be understood to include substituted variants. For example, reference to a "cyclic ether compound" or moiety implicitly includes unsubstituted cyclic ether compounds and substituted derivatives.
[0068] For the entire context of the present invention, the above-mentioned "suitable substituents" should be understood to include, but are not limited to, the alkyl, alkenyl, alkynyl, halogen, haloalkyl, haloalkenyl, haloalkynyl, alkoxy, cyano, hydroxy, amino, monoalkylamino, dialkylamino, nitro, aryl, heteroaryl, cycloalkyl (e.g., cycloalkyl, cycloalkenyl, etc.), carboxyl, triphenylphosphino, azido, aldehyde, heterocyclyl, etc. described herein; these groups as substituents, including alkyl, alkenyl, alkynyl, alkyl in haloalkyl, alkenyl in haloalkenyl, alkynyl in haloalkynyl, alkoxy, alkyl in monoalkylamino, alkyl in dialkylamino, aryl, heteroaryl, cycloalkyl and heterocyclyl themselves are also optionally substituted, for example, they may also be optionally substituted by one or more groups selected from alkyl, halogen, haloalkyl, alkoxy, hydroxy, amino, monoalkylamino, dialkylamino, nitro, carboxyl, triphenylphosphino, azido, aryl, heteroaryl, cycloalkyl and heterocyclyl.
[0069] In the present invention, polyether polymers are polymers polymerized from the main monomers of cyclic ether compounds, wherein the mass of cyclic ether compounds can account for more than 80% of the total mass of monomers, such as more than 90%, more than 95%, more than 98%, more than 99%. In addition to cyclic ether compounds, the monomers of polyether polymers may also include one or more selected from anhydrides, cyclic anhydrides, cyclic esters, carbon dioxide, polyols and polycarboxylic acids. In some embodiments, in addition to cyclic ether compounds, the monomers of polyether polymers may also include one or more selected from anhydrides, cyclic anhydrides, polyols and polycarboxylic acids. In some embodiments, the monomers of polyether polymers are composed of cyclic ether compounds and one or more monomers optionally selected from anhydrides, cyclic anhydrides, cyclic esters, carbon dioxide, polyols and polycarboxylic acids. In some embodiments, the monomers of polyether polymers are composed of cyclic ether compounds and one or more monomers optionally selected from anhydrides, cyclic anhydrides, polyols and polycarboxylic acids. Examples of polyether polymers include, but are not limited to, polyether polyesters, polyether polyols, etc.
[0070] Herein, anhydride refers to a compound formed by dehydration condensation of carboxyl groups between multiple (e.g., two) carboxylic acid molecules into anhydride groups. Herein, multiple refers to two or more, such as two, three, four, five, six. Anhydride can be C2-C10 anhydride, such as C2 anhydride, C3 anhydride, C4 anhydride, C5 anhydride, C6 anhydride, C7 anhydride, C8 anhydride, C9 anhydride, C10 anhydride. Available anhydrides include, but are not limited to, acetic anhydride, propionic anhydride, etc.
[0071] Herein, a cyclic anhydride refers to a compound formed by dehydration condensation of a carboxyl group in a single carboxylic acid molecule containing multiple (e.g., two) carboxyl groups into an anhydride group. The cyclic anhydride may be a 4-8 membered cyclic anhydride, such as a 4-membered cyclic anhydride, a 5-membered cyclic anhydride, a 6-membered cyclic anhydride, a 7-membered cyclic anhydride, and an 8-membered cyclic anhydride. Herein, an n-membered cyclic compound means that the number of ring atoms of the cyclic compound is n.
[0072] Herein, cyclic ester refers to a compound having an ester bond on the ring. The cyclic ester may be a 4-8 membered cyclic ester, such as a 4-membered cyclic ester, a 5-membered cyclic ester, a 6-membered cyclic anhydride, a 7-membered cyclic ester, or an 8-membered cyclic ester.
[0073] Herein, polyol refers to an alcohol containing multiple hydroxyls, including but not limited to diols, triols, etc. n-hydric alcohol means that the alcohol contains n hydroxyls. The polyol can be a C2-C10 polyol, such as a C2 polyol, a C3 polyol, a C4 polyol, a C5 polyol, a C6 polyol, a C7 polyol, a C8 polyol, a C9 polyol, a C10 polyol. Available polyols include but are not limited to ethylene glycol, propylene glycol, glycerol, etc.
[0074] Herein, polycarboxylic acid refers to a carboxylic acid containing multiple carboxyl groups, including but not limited to dicarboxylic acids, tricarboxylic acids, etc. An n-carboxylic acid means that the carboxylic acid contains n carboxyl groups. The polycarboxylic acid can be a C2-C10 polycarboxylic acid, such as a C2 polycarboxylic acid, a C3 polycarboxylic acid, a C4 polycarboxylic acid, a C5 polycarboxylic acid, a C6 polycarboxylic acid, a C7 polycarboxylic acid, a C8 polycarboxylic acid, a C9 polycarboxylic acid, and a C10 polycarboxylic acid.
[0075] Since the composite catalyst of the present invention has suitable acidity, it can show relatively excellent performance (higher conversion rate and narrower molecular weight distribution) in the cyclic ether ring-opening polymerization reaction. Therefore, the composite catalyst has broad application prospects in the following application fields.
[0076] 1. High-end fabrics: The composite catalyst of the present invention can be used for the ring-opening polymerization of cyclic ether compounds to generate polyether polyesters or polyether polyols. Such polymers have good elasticity and durability and can be used in the manufacture of high-end fabrics, such as high-elastic fibers, high-strength fabrics, etc.
[0077] 2. Medical care: Polyether polyester materials are biocompatible and degradable, and are suitable for medical devices, medical dressings and other fields. The composite catalyst of the present invention can be used to synthesize polyether polyester materials to meet the requirements of material performance and quality in the field of medical care.
[0078] 3. Functional coatings: Polyether polyester materials have good adhesion, flexibility and wear resistance in coatings and can be used in automotive paints, architectural coatings and other fields. The composite catalyst of the present invention can catalyze the polymerization reaction to obtain polyether polyester materials with narrow molecular weight distribution at a high conversion rate, which can improve the performance and quality of coatings.
[0079] 4. Electronic materials: Polyether polyester materials have good electrical insulation and heat resistance and can be used in packaging and insulation of electronic devices. The composite catalyst of the present invention can be used to catalyze the synthesis of polyether polyester materials with specific performance requirements to meet the needs of the electronic materials field.
[0080] 5. Degradable materials: Polyether polyester materials are degradable and can be used in the manufacture of environmentally friendly products, such as degradable plastics, degradable packaging materials, etc. The preparation method of the polyether polyester material catalyzed by the composite catalyst of the present invention is simple and efficient, which helps to improve the production efficiency and quality of polyether polyester degradable materials.
[0081] In summary, the composite catalyst of the present invention has broad application prospects in application fields such as high-end fabrics, medical care, functional coatings, electronic materials and degradable materials. As the market's requirements for product performance and quality increase, it is imperative to develop new catalytic systems, so the present invention has good technical application prospects and market demand.
[0082] The present invention also provides a method for generating polyether polyester by catalyzing the polymerization of cyclic ether compounds and anhydride analogs using the composite catalyst of the present invention. In the present invention, polyether polyester refers to a polyether polymer whose monomers include cyclic ether compounds and anhydride analogs. In the method, the anhydride analog can be selected from one or more of C2-C10 anhydrides, 4-8-membered cyclic anhydrides and C2-C10 polycarboxylic acids. The polycarboxylic acid can be an aliphatic polycarboxylic acid or an aromatic polycarboxylic acid. The polycarboxylic acid is preferably selected from dicarboxylic acids and tricarboxylic acids, such as oxalic acid, malonic acid, and phthalic acid. In some embodiments, the anhydride analog is acetic anhydride. The mass ratio of the cyclic ether compound to the anhydride analog can be 80-240:1, such as 100:1, 120:1, 130:1, 150:1, 180:1, 200:1, 220:1, preferably 100-200:1. In some embodiments, the monomer of the polyether polyester also includes a polyol, such as a diol. The mass ratio of polyol to anhydride analogue can be 80-240:1, for example 100:1, 120:1, 130:1, 150:1, 180:1, 200:1, 220:1. In some embodiments, the monomer of polyether polyester is composed of cyclic ether compound, anhydride analogue and optional polyol. The consumption of composite catalyst of the present invention can be 0.001-0.1wt% of cyclic ether compound, for example 0.005wt%, 0.008wt%, 0.01wt%, 0.02wt%, 0.03wt%, 0.04wt%, 0.05wt%, 0.06wt%, 0.07wt%, 0.08wt%, 0.09wt%, preferably 0.01-0.02wt%. Reaction pressure can be ≤1MPaG, for example, ≤0.2MPaG, ≤0.4MPaG, ≤0.6MPaG, ≤0.8MPaG. The reaction temperature may be 50-120°C, for example, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, preferably 60-100°C. The reaction time may be 2-48h, for example, 3h, 5h, 8h, 12h, 15h, 18h, 24h, 30h, 36h. The number average molecular weight range of the polyether polyester prepared by the method of the present invention is 450-10000, preferably 1600-1700. The molecular weight distribution index of the polyether polyester prepared by the method of the present invention is 1.60-2.00, preferably 1.70-1.90. In some embodiments, the molecular weight distribution index of the polyether polyester prepared by the method of the present invention is 1.75-1.88.
[0083] The present invention also provides a method for generating polyether polyols by catalyzing the polymerization of cyclic ether compounds and polyols by the composite catalyst of the present invention. In the present invention, polyether polyols refer to polyether polymers whose monomers include cyclic ether compounds and polyols, and the monomers of polyether polyols do not include anhydride analogs. In some embodiments, the monomers of polyether polyols are composed of cyclic ether compounds and polyols. Herein, the polyols may have 2, 3, 4, 5 or 6 hydroxyl groups. The polyols may be selected from C2-C20 polyols, C2-C10 polyols, C2-C6 polyols, C2-C4 polyols. In some embodiments, the polyols are selected from one or more of ethylene glycol, propylene glycol and glycerol. The mass ratio of cyclic ether compounds to polyols may be 80-240:1, for example, 100:1, 120:1, 130:1, 150:1, 180:1, 200:1, 220:1, preferably 100-200:1. The amount of the composite catalyst of the present invention can be 0.001-0.1wt% of the cyclic ether compound, such as 0.005wt%, 0.008wt%, 0.01wt%, 0.02wt%, 0.03wt%, 0.04wt%, 0.05wt%, 0.06wt%, 0.07wt%, 0.08wt%, 0.09wt%, preferably 0.01-0.05wt%, 0.02-0.03wt%. The reaction pressure can be ≤1MPaG, such as ≤0.2MPaG, ≤0.4MPaG, ≤0.6MPaG, ≤0.8MPaG. The reaction temperature can be 50-120°C, such as 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, preferably 60-100°C. The reaction time may be 2-48 hours, for example, 3 hours, 5 hours, 8 hours, 12 hours, 15 hours, 18 hours, 24 hours, 30 hours, 36 hours. The number average molecular weight of the polyether polyol prepared by the method of the present invention is in the range of 450-10000, preferably 1000-1500, more preferably 1100-1300. The molecular weight distribution index of the polyether polyol prepared by the method of the present invention is 2.00-2.35. In some embodiments, the molecular weight distribution index of the polyether polyol prepared by the method of the present invention is 2.10-2.30.
[0084] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually based on conventional conditions or the conditions recommended by the manufacturer. Unless otherwise stated, percentages and parts are calculated by weight.
[0085] Example 1
[0086] Preparation of Al-Si composite catalyst. Dissolve 21.30 g of aluminum nitrate powder in 500 mL of ethanol-water mixed solvent (the volume ratio of ethanol to water is 4:1), then add it to the reactor and stir it thoroughly. Subsequently, add 88.64 mL of tetraethoxysilane, react at a constant temperature at 60 ° C for 24 hours, and then let it stand for 24 hours. Using the nitrogen stripping method, pass nitrogen into the reactor at 20 mL / hr for 2 hours to evaporate the liquid in the reactant. The reactant is transferred to an evaporating dish, and the evaporating dish is placed in a dryer preheated to 120 ° C and dried for 3 hours. The dried solid is calcined at 900 ° C for 3 hours in an air atmosphere to obtain a composite catalyst powder containing an Al / Si molar ratio of 1:4. It is formed by extrusion. The specific surface area measured by the BET method is 282m 2 / g, the amount of acid on the catalyst surface measured by ion exchange method was 0.53mg, and the acidity was 0.026mmol / g.
[0087] Example 2
[0088] Preparation of Ti-Si composite catalyst. 18.97 g of titanium tetrachloride powder was dissolved in 500 mL of ethanol-water mixed solvent (the volume ratio of ethanol to water was 4:1), then added to the reactor and stirred thoroughly. Subsequently, 88.64 mL of tetraethoxysilane was added, and the reaction was carried out at a constant temperature of 60 ° C for 24 hours, and then allowed to stand for 24 hours. Using the nitrogen stripping method, 20 mL / hr of nitrogen was introduced into the reactor for 2 hours to evaporate the liquid in the reactant. The reactant was transferred to an evaporating dish, and the evaporating dish was placed in a dryer preheated to 120 ° C and dried for 3 hours. The dried solid was calcined at 900 ° C for 3 hours in an air atmosphere to obtain a composite catalyst powder containing a Ti / Si molar ratio of 1:4. It was formed by extrusion. The specific surface area measured by the BET method was 263 m 2 / g, the amount of acid on the catalyst surface measured by ion exchange method was 0.48 mg, and the acidity was 0.036 mmol / g.
[0089] Example 3
[0090] Preparation of Zr-Si composite catalyst. Dissolve 23.12 g of zirconium oxynitrate powder in 500 mL of ethanol-water mixed solvent (the volume ratio of ethanol to water is 4:1), then add it to the reactor and stir it thoroughly. Then add 88.64 mL of tetraethoxysilane, react at a constant temperature at 60 ° C for 24 hours, and then let it stand for 24 hours. After centrifuging the reactants, remove the sediment and move it to an evaporating dish, and place the evaporating dish in a dryer preheated to 120 ° C for 3 hours. The dried solid was calcined at 900 ° C for 3 hours in an air atmosphere to obtain a composite catalyst powder containing a Zr / Si molar ratio of 1:4. It was formed by extrusion. The specific surface area measured by the BET method is 327m 2 / g, the amount of acid on the catalyst surface measured by ion exchange method was 0.55mg, and the acidity was 0.046mmol / g.
[0091] Comparative Example 1
[0092] Comparative catalyst D1 is a Ti-Si composite catalyst prepared by impregnation method. The Ti / Si molar ratio is 1:4. The specific surface area of catalyst D1 measured by BET method is 280 m 2 / g, and the acidity of the catalyst measured by ion exchange method was 0.01mmol / g. The catalyst was dried in a dryer at 120°C for 3 hours. The dried solid was calcined at 900°C for 3 hours in an air atmosphere.
[0093] Comparative Example 2
[0094] Zeolite molecular sieve is a typical high aluminum-silicon ratio composite compound with both Bronsted acid and Lewis acid acid sites, and is widely used in the petrochemical field. Comparative catalyst D2 is ZSM-5 (Al:Si molar ratio 1:50) produced by NKC direct synthesis method. The specific surface area of the catalyst measured by BET method is 340m 2 / g, and the acidity of the catalyst measured by ion exchange method was 0.3 mmol / g. The catalyst was dried in a dryer at 120°C for 3 hours. The dried solid was calcined at 900°C for 3 hours in an air atmosphere.
[0095] Comparative Example 3
[0096] The comparative catalyst D3 is SiO2 (Q-10) purchased from Fuji. The specific surface area of catalyst D3 measured by BET method is 290 m 2 / g, particle size 4mm, the acidity of the catalyst measured by ion exchange method is 0.01mmol / g. The catalyst is dried in a dryer at 120°C for 3 hours. The dried solid is calcined at 900°C for 3 hours in an air atmosphere.
[0097] Application Example 1
[0098] 20 mg of the catalyst prepared in Examples 1, 2, 3 and Comparative Examples 1, 2, 3 were taken and loaded into a 100 mL stainless steel reactor, 80 g of ethylene oxide and 0.8 g of ethylene glycol were added at a mass ratio of 100:1, the reactor was closed and replaced with nitrogen 5 times, the nitrogen kept the pressure in the reactor ≤ 0.4 MPaG, and the reaction was carried out at a constant temperature of 80°C for 8 hours, and the stirring speed was 300 rpm. The conversion rate, number average molecular weight and molecular weight distribution index of each reaction are shown in Table 1.
[0099] Table 1
[0100]
[0101] Application Example 2
[0102] 20 mg of the catalyst prepared in Examples 1, 2, 3 and Comparative Examples 1, 2, 3 were taken and loaded into a 100 mL stainless steel reactor. 160 g of tetrahydrofuran (THF), 80 g of propylene oxide and 1.6 g of acetic anhydride were added in a mass ratio of 100:50:1. The reactor was closed and replaced with nitrogen 5 times. The nitrogen kept the pressure in the reactor ≤ 0.4 MPaG. The reaction was carried out at a constant temperature of 80°C for 8 hours, and the stirring speed was 300 rpm. The conversion rate, number average molecular weight and molecular weight distribution index of each reaction are shown in Table 2.
[0103] Table 2
[0104]
[0105] Application Example 3
[0106] Take the mixture of the reaction solution and the catalyst in the above application examples 1 and 2, and test the initial color number of the reaction solution. Continue to maintain the corresponding reaction conditions, and perform conversion rate and color analysis every 4 hours until the conversion rate is stable and the fluctuation is less than 0.1%. It is considered that the reaction has reached equilibrium and the equilibrium conversion rate is measured. After maintaining the same reaction conditions and continuing to run for 60 days, the conversion rate and color number of the reactants are analyzed, and the final color number is measured. The results are shown in Table 3.
[0107]
[0108] Calculation of conversion rate = polymer mass in product / total amount of raw materials × 100%;
[0109] The polymer mass is the weight of the polymer obtained after rotary evaporation at -80 kPaG and 130°C. The rotary evaporator is Buchi Rotavapor R215 and the vacuum pump is VACUUBRAND GMBH +CO KG MD 1C +AK+EK.
[0110] In this article, the number average molecular weight of polyether polyester (Molecular Weight Average, abbreviated MW average The determination of the saponification value SN (unit: g / mol) requires first adding an excess of KOH for saponification reaction, and then acid titrating the remaining alkali to obtain the saponification value SN (abbreviated as SN, unit: mgKOH / g). The saponification value SN is the equivalent amount of KOH consumed in the saponification reaction of 1g of sample. The determination of the saponification value SN is based on the ASTM D94-07 (2017) method, and then the number average molecular weight is calculated according to the following formula: MW average =56105×2 / SN.
[0111] In this article, the number average molecular weight of polyether polyols (Molecular Weight Average, abbreviated MW average The determination of hydroxyl number (HN, unit: mgKOH / g) requires the addition of excess acetic anhydride to convert the hydroxyl groups of the sample into ester groups by esterification reaction, and then the unreacted acetic anhydride is fully hydrolyzed and then titrated with alkali to obtain the hydroxyl number (HN, unit: mgKOH / g). The determination of hydroxyl number HN is based on the ASTM D4274-05 (2010) method. The number average molecular weight is then calculated using the following formula: MW average =56105×2 / HN.
[0112] In this paper, the titrator used is the automatic potentiometer T7 produced by METTLER TOLEDO.
[0113] The molecular weight distribution index was measured by Agilent 1260 Infinity II gel permeation chromatography (GPC) with THF as the mobile phase.
[0114] The color number was determined using the British Lovibond automatic colorimeter PFX195, and the chromaticity value was based on the platinum-cobalt standard of ASTM D1209.
[0115] The polymerization of cyclic ethers is carried out in a fully automated laboratory reactor RC1 from METTLER TOLEDO.
[0116] Comparison between Example 2 and Comparative Example 1 shows that the acidity of the catalyst D1 obtained in Comparative Example 1 is lower due to the difference in the preparation method. Catalyst D1 is used to catalyze the ring-opening polymerization of cyclic ether compounds. As shown in Tables 1 and 2, the conversion rate and molecular weight distribution of the polymerized product measured are poor. Catalyst D2 obtained in Comparative Example 2 has a high specific surface area and acidity and is used to catalyze the ring-opening polymerization of cyclic ether compounds. Although the conversion rate is high, the molecular weight distribution of the polymerized product is wide because the preparation method of the catalyst is different from that of the present invention. Catalyst D3 obtained in Comparative Example 3 cannot catalyze the ring-opening polymerization of cyclic ether compounds.
[0117] Application Example 3 tested the time for the reactions in Application Examples 1 and 2 to reach equilibrium and the color number of the reaction liquid after long-term operation. By comparison, it was found that the time for the reaction system using the composite catalyst of the present invention to reach equilibrium was shorter than that of the reaction system using the comparative catalyst. Among them, the composite catalyst prepared in Example 3 has higher activity, can make the reaction system reach reaction equilibrium in the shortest time, has the highest equilibrium conversion rate, and after running for 60 days, the color number of the reaction liquid still remains at a low color number level. The reaction system using comparative catalyst D1 in Application Example 1 has a short time to reach equilibrium and a low final color number of the reaction liquid, which is caused by the low conversion rate of the reaction.
[0118] In summary, the present invention provides a composite catalyst, which exhibits excellent performance in a cyclic ether ring-opening polymerization reaction. The composite catalyst has suitable acidity, and its preparation method is simple, and is suitable for synthesizing polyether polyesters or polyether polyol materials with different number average molecular weights and performance requirements. Using the composite catalyst of the present invention to catalyze the cyclic ether ring-opening polymerization reaction can make the reaction system reach equilibrium in a relatively short time, and after the reaction system reaches equilibrium, the reaction solution can still be kept at a relatively low color level after a long reaction. Example 1, Example 2 and Example 3 provide specific preparation methods for reference and practical application.
Claims
1. A method for catalyzing the polymerization of a cyclic ether compound and an acid anhydride to produce a polyether polyester or catalyzing the polymerization of a cyclic ether compound and a polyol to produce a polyether polyol, characterized in that: The cyclic ether compound is selected from ethylene oxide, propylene oxide, tetrahydrofuran or hexyl oxide, and the conversion rate of the method reaches more than 55%; The preparation method of the composite catalyst is: (1) dissolving the metal salt in a solvent and stirring evenly to obtain a first component; (2) adding a silicon source to the first component, allowing the silicon source to react with the metal salt, and allowing the reaction to stand; (3) removing the solvent and drying to obtain dry powder; (4) calcining the dried powder to obtain the composite catalyst; The metal salt is selected from one or more of zirconium nitrate, titanium tetrachloride and aluminum nitrate; The silicon source is selected from one or more of tetraethoxysilane, tetramethoxysilane, polysilane and silicon tetrachloride; The molar ratio of the metal ions contained in the metal salt to the silicon atoms contained in the silicon source is 1:4; The solvent is an alcohol solvent and / or water; The specific surface area of the composite catalyst is ≥250m 2 / g; The acidity of the composite catalyst is 0.02-0.2 mmol / g; The amount of acid on the surface of the composite catalyst is 0.40-0.70 mg.
2. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with the composite catalyst as claimed in claim 1, characterized in that: In step (2), The reaction is carried out for 4-48 hours; and / or, The reaction is carried out at 40-80°C.
3. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with the composite catalyst as claimed in claim 1, characterized in that: In step (2), the standing time is 12-48 hours.
4. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with the composite catalyst as claimed in claim 1, characterized in that: The step (2) has one or more of the following features: The concentration of the metal salt in the solvent is 0.05-1 mol / L; The concentration of the silicon source in the solvent is 0.2-4 mol / L.
5. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with a composite catalyst as claimed in claim 1, characterized in that: The step (3) has one or more of the following features: removing the solvent by centrifugation or gas stripping to obtain insoluble matter, and drying the insoluble matter; The drying temperature is 30-200°C; The drying time is 1-12 hours.
6. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with a composite catalyst as claimed in claim 1, characterized in that: In step (4), The calcination temperature is 400-1500°C; and / or, The calcination time is 1-12 hours.
7. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with a composite catalyst as claimed in claim 1, characterized in that: The method for preparing the composite catalyst further comprises the step of: (5) extruding and granulating the composite catalyst.
8. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with a composite catalyst as claimed in claim 1, characterized in that: The acid anhydride is selected from C2-C10 acid anhydride.
9. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with a composite catalyst as claimed in claim 1, characterized in that: The acid anhydride is acetic anhydride.
10. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with a composite catalyst as claimed in claim 1, characterized in that: In the method for generating polyether polyester by polymerizing a cyclic ether compound and an acid anhydride using a composite catalyst, the mass ratio of the cyclic ether compound to the acid anhydride is 100-200:
1.
11. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with a composite catalyst as claimed in claim 1, characterized in that: In the method for generating polyether polyester by catalyzing the polymerization of cyclic ether compound and acid anhydride by composite catalyst, the amount of the composite catalyst used is 0.001-0.1wt% of the cyclic ether compound.
12. The method for producing polyether polyester by catalyzing the polymerization of cyclic ether compound and acid anhydride or producing polyether polyol by catalyzing the polymerization of cyclic ether compound and polyol as claimed in claim 1, characterized in that: The polyol is a C2-C6 polyol having 2, 3, 4, 5 or 6 hydroxyl groups.
13. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with a composite catalyst as claimed in claim 1, characterized in that: The polyol is selected from one or more of ethylene glycol, propylene glycol and glycerol.
14. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with a composite catalyst as claimed in claim 1, characterized in that: In the method for generating polyether polyol by polymerizing a cyclic ether compound and a polyol using a composite catalyst, the mass ratio of the cyclic ether compound to the polyol is 100-200:
1.
15. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with a composite catalyst as claimed in claim 1, characterized in that: In the method for generating polyether polyol by polymerizing a cyclic ether compound and a polyol using a composite catalyst, the amount of the composite catalyst used is 0.01-0.05wt% of the cyclic ether compound.
16. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with a composite catalyst as claimed in claim 1, characterized in that: Reaction pressure ≤1MpaG.
17. The method for producing polyether polyols by catalyzing the polymerization of a cyclic ether compound and an acid anhydride with a composite catalyst as claimed in claim 1, characterized in that: The reaction temperature is 50-120°C.