Aluminum-based composite material and preparation method thereof
By using modified reinforced fiber cloth and nano-reinforcements in aluminum-based composite materials, combined with multi-energy field treatment and heat treatment technology, the problems of insufficient thermal conductivity and low mechanical properties of traditional aluminum-based composite materials have been solved, and better performance has been achieved. Excellent wear resistance, corrosion resistance and thermal conductivity, suitable for industrial production.
Patent Information
- Application Number
- CN202410284735.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-03-13
AI Technical Summary
Traditional particle-reinforced aluminum matrix composites have problems such as poor wettability between reinforced particles and the matrix, difficult to control interface reactions, uneven distribution of reinforced particles, complex preparation processes, limited molding, insufficient thermal conductivity and mechanical and mechanical properties that need to be improved.
Using modified reinforced fiber cloth and nano-reinforcement components, through multi-energy field treatment and heat treatment technology, the matrix material including Si, Sr, Cu, Ga, V, Cr, Hf, Re, Os, Be, Te, rare earth elements is prepared and nano-reinforcements Aluminum-based composite material, the modifier is a mixture of sodium silicate and 1,3-bis[tris(hydroxymethyl)methylamino]propane, and the nano-reinforcement is nano-tantalum boride, nano-niobium silicide and nano-scandium nitride, which improves Reinforce the compatibility and interface bonding between the fiber cloth and the matrix material.
It significantly improves the mechanical properties, wear resistance and corrosion resistance of aluminum-based composite materials, while reducing preparation costs and energy consumption. It is suitable for industrial production and improves the thermal conductivity effect.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of metal-based composite materials, and in particular to an aluminum-based composite material and a preparation method thereof. Background Art
[0002] Aluminum-based composite materials have the advantages of high specific strength, high specific stiffness, heat resistance, wear resistance, low expansion, high thermal conductivity and large design freedom. It is an advanced structural and functional integrated material with excellent structural and functional performance. It has important application value and broad application prospects in the fields of aerospace, automobile, electronic packaging and sports industry, and has become one of the most commonly used and important materials in metal-based composite materials. In recent years, particle-reinforced aluminum-based composite materials have received widespread attention due to their excellent performance, with a large market demand and increasingly higher performance requirements.
[0003] Traditional particle-reinforced aluminum-based composites generally have defects such as poor wettability between the reinforcing particles and the matrix, difficult to control interfacial reactions, uneven distribution of reinforcing particles, easy appearance of micro-shrinkage holes and cracks, complex preparation process, limited molding, insufficient thermal conductivity and mechanical properties that need to be further improved.
[0004] In order to solve the above problems, the Chinese invention patent with the authorization announcement number CN105671387B discloses an aluminum-based composite material and its preparation method. The aluminum-based composite material is prepared by dispersing carbon materials, mixing aluminum materials, annealing treatment, etc. by weight ratio of aluminum 85%-99%, iron 0.1%-1%, zinc 0.2%-1%, copper 0.5%-4%, and carbon materials 0.2%-9%. The aluminum-based composite material described in the invention is obtained by adding carbon materials to the aluminum-based material through the process of dispersion-mixing drying-die casting-sintering-casting, and obtaining an aluminum-based composite material with high thermal conductivity and good thermal conductivity. The thermal conductivity of the aluminum-based composite material is as high as 285W / (m·℃) at room temperature. However, the mechanical properties, wear resistance and corrosion resistance of the material still need to be further improved. Summary of the invention
[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide an aluminum-based composite material having good mechanical properties, good wear resistance and corrosion resistance, and significant thermal conductivity, and a preparation method thereof.
[0006] To achieve the above object, the technical solution adopted by the present invention is: an aluminum-based composite material, comprising a matrix material and a modified reinforcing fiber cloth uniformly distributed in the matrix material, wherein the modified reinforcing fiber cloth accounts for 8-12% of the weight of the aluminum-based composite material; the matrix material comprises the following components in percentage by mass: Si 3%-5%, Sr 0.1%-0.3%, Cu1%-3%, Ga 0.01%-0.03%, V 0.05%-0.15%, Cr 0.3%-0.5%, Hf 0.1%-0.3%, Re 0.01%-0.03%, Os0.001%-0.005%, Be 0.001%-0.003%, Te 0.01%-0.03%, rare earth elements 0.1%-0.2%, Mo 0.1%-0.3% and nano reinforcement component 0.03%-0.05%, and the balance is Al.
[0007] Preferably, the preparation method of the modified reinforced fiber cloth comprises the following steps: dispersing the modifier in water, mixing evenly, soaking the reinforced fiber cloth therein for 10-20 hours, taking it out, and drying it at 105-110° C. to constant weight to obtain the modified reinforced fiber cloth.
[0008] Preferably, the modifier is a mixture of sodium silicate and 1,3-bis[tris(hydroxymethyl)methylamino]propane in a mass ratio of (1-3):(0.3-0.5); the mass ratio of the modifier to water is 1:(5-8).
[0009] Preferably, the reinforcing fiber cloth is any one of Qinghai Guxiang GX-CF300 carbon fiber cloth and 06 alkali-free glass fiber cloth EWR600-100.
[0010] Preferably, the rare earth element is a mixture of Sc, Y and Nd in a mass ratio of (2-3):1:(0.1-0.2).
[0011] Preferably, the nano-reinforcement component is a mixture of nano-tantalum boride, nano-niobium silicide and nano-scandium nitride in a mass ratio of 1:(0.8-1.2):(0.1-0.3); the particle size of the nano-reinforcement component is 10-80nm.
[0012] Another object of the present invention is to provide a method for preparing the aluminum-based composite material, comprising the following steps:
[0013] Step S1: using aluminum ingots, Si-Al master alloys, Sr-Al master alloys, Cu-Al master alloys, Ga-Al master alloys, V-Al master alloys, Cr-Al master alloys, Hf-Al master alloys, Re-Al master alloys, Os-Al master alloys, Be-Al master alloys, Te-Al master alloys, rare earth element-Al master alloys and Mo-Al master alloys as raw materials, mixing them in proportion, and smelting them in a vacuum induction furnace to form an alloy melt; then adding a nano-reinforcement component preheated at 500-600° C. to the above alloy melt, and obtaining a matrix material melt after multi-energy field treatment;
[0014] Step S2: pouring the matrix material melt prepared in step S1 into a mold preheated at 430-470° C. and containing the modified reinforcing fiber cloth, and demoulding the mold after cooling and solidification;
[0015] Step S3: obtaining an aluminum-based composite material after heat treatment.
[0016] Preferably, the smelting temperature in step S1 is 700-770°C.
[0017] Preferably, the multi-energy field treatment in step S1 includes ultrasonic treatment and magnetic field treatment, the ultrasonic frequency of the ultrasonic treatment is 20-50KHZ, the power is 600-1100W, and the time is 8-15min; the magnetic field intensity of the magnetic field treatment is 5000-12000Gs, and the time is 5-10min.
[0018] Preferably, the heat treatment in step S3 includes solution treatment, aging treatment and annealing treatment; the temperature of the solution treatment is 490-510°C, the holding time is 1-3h, and the temperature is room temperature and water-cooled; the temperature of the aging treatment is 180-260°C, and the time is 8-10h; the temperature of the annealing treatment is 420-510°C, and the time is 3-5h.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] (1) The method for preparing the aluminum-based composite material disclosed in the present invention can be prepared using conventional equipment and production lines, with low capital investment, low energy consumption, simple process, convenient operation and control, high preparation efficiency and yield rate, and the prepared aluminum-based composite material is of good quality and suitable for industrial production.
[0021] (2) The aluminum-based composite material disclosed in the present invention comprises a matrix material and a modified reinforcing fiber cloth uniformly distributed in the matrix material, wherein the modified reinforcing fiber cloth accounts for 8-12% of the weight of the aluminum-based composite material; the matrix material comprises the following components in percentage by mass: Si 3%-5%, Sr 0.1%-0.3%, Cu 1%-3%, Ga 0.01%-0.03%, V0.05%-0.15%, Cr0.3%-0.5%, Hf 0.1%-0.3%, Re 0.01%-0.03%, Os 0.001%-0.005%, Be 0.001%-0.003%, Te0.01%-0.03%, rare earth elements 0.1%-0.2%, Mo 0.1%-0.3% and nano-reinforcement component 0.03%-0.05%, and the balance is Al. The nano reinforcement component is a mixture of nano tantalum boride, nano niobium silicide and nano scandium nitride in a mass ratio of 1: (0.8-1.2): (0.1-0.3). Through the mutual cooperation between the raw materials, the aluminum-based composite material has good mechanical properties, good wear resistance and corrosion resistance, and significant thermal conductivity.
[0022] (3) The aluminum-based composite material disclosed in the present invention adopts a modified reinforcing fiber cloth, and the modifier is a mixture of sodium silicate and 1,3-bis[tris(hydroxymethyl)methylamino]propane in a mass ratio of (1-3):(0.3-0.5); through the mutual coordination between the modifier components, the compatibility between the reinforcing fiber cloth and the matrix material can be effectively improved, the wettability and interfacial bonding strength can be improved, thereby improving the density of the internal structure of the aluminum-based composite material, so that the mechanical properties, wear resistance and corrosion resistance of the prepared aluminum-based composite material are better, and the thermal conductivity effect is more significant.
[0023] (4) The aluminum-based composite material disclosed in the present invention has a dense structure, better mechanical properties and wear resistance, and a longer service life through the reasonable selection of the preparation process. DETAILED DESCRIPTION
[0024] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.
[0025] Embodiment 1
[0026] An aluminum-based composite material comprises a matrix material and a modified reinforcing fiber cloth uniformly distributed in the matrix material, wherein the modified reinforcing fiber cloth accounts for 8% of the weight of the aluminum-based composite material; the matrix material comprises the following components in percentage by mass: 3% Si, 0.1% Sr, 1% Cu, 0.01% Ga, 0.05% V, 0.3% Cr, 0.1% Hf, 0.01% Re, 0.001% Os, 0.001% Be, 0.01% Te, 0.1% rare earth element, 0.1% Mo and 0.03% nano-reinforcement component, and the balance is Al.
[0027] The preparation method of modified reinforced fiber cloth comprises the following steps: dispersing a modifier in water, mixing evenly, immersing the reinforced fiber cloth therein for 10 hours, taking it out, and drying it at 105°C to constant weight to obtain the modified reinforced fiber cloth; the modifier is a mixture of sodium silicate and 1,3-bis[tris(hydroxymethyl)methylamino]propane in a mass ratio of 1:0.3; the mass ratio of the modifier to water is 1:5; the reinforced fiber cloth is Qinghai Guxiang GX-CF300 carbon fiber cloth.
[0028] The rare earth elements are a mixture of Sc, Y and Nd in a mass ratio of 2:1:0.1; the nano-reinforcement component is a mixture of nano-tantalum boride, nano-niobium silicide and nano-scandium nitride in a mass ratio of 1:0.8:0.1; and the particle size of the nano-reinforcement component is 10 nm.
[0029] A method for preparing an aluminum-based composite material comprises the following steps:
[0030] Step S1: using aluminum ingots, Si-Al master alloys, Sr-Al master alloys, Cu-Al master alloys, Ga-Al master alloys, V-Al master alloys, Cr-Al master alloys, Hf-Al master alloys, Re-Al master alloys, Os-Al master alloys, Be-Al master alloys, Te-Al master alloys, rare earth element-Al master alloys and Mo-Al master alloys as raw materials, mixing them in proportion, and smelting them in a vacuum induction furnace to form an alloy melt; then adding the nano-reinforcement component preheated at 500° C. to the above alloy melt, and obtaining a matrix material melt after multi-energy field treatment;
[0031] Step S2: pouring the matrix material melt prepared in step S1 into a mold preheated at 430° C. and containing the modified reinforcing fiber cloth, and demoulding the mold after cooling and solidification;
[0032] Step S3: obtaining an aluminum-based composite material after heat treatment.
[0033] The smelting temperature in step S1 is 700°C; the multi-energy field treatment in step S1 includes ultrasonic treatment and magnetic field treatment, the ultrasonic frequency of the ultrasonic treatment is 20KHZ, the power is 600W, and the time is 8min; the magnetic field intensity of the magnetic field treatment is 5000Gs, and the time is 5min.
[0034] The heat treatment in step S3 includes solution treatment, aging treatment and annealing treatment; the temperature of the solution treatment is 490°C, the holding time is 1 hour, and the room temperature is water-cooled; the temperature of the aging treatment is 180°C, the time is 8 hours; the temperature of the annealing treatment is 420°C, and the time is 3 hours.
[0035] Embodiment 2
[0036] An aluminum-based composite material comprises a matrix material and a modified reinforcing fiber cloth uniformly distributed in the matrix material, wherein the modified reinforcing fiber cloth accounts for 9% of the weight of the aluminum-based composite material; the matrix material comprises the following components in percentage by mass: 3.5% Si, 0.15% Sr, 1.5% Cu, 0.015% Ga, 0.07% V, 0.35% Cr, 0.15% Hf, 0.015% Re, 0.002% Os, 0.0015% Be, 0.015% Te, 0.13% rare earth element, 0.15% Mo and 0.035% nano-reinforcement component, and the balance is Al.
[0037] The preparation method of modified reinforced fiber cloth comprises the following steps: dispersing a modifier in water, mixing uniformly, immersing the reinforced fiber cloth in the water for 12 hours, taking out, and drying at 107°C to constant weight to obtain the modified reinforced fiber cloth; the modifier is a mixture of sodium silicate and 1,3-bis[tris(hydroxymethyl)methylamino]propane in a mass ratio of 1.5:0.35; the mass ratio of the modifier to water is 1:6; the reinforced fiber cloth is 06 alkali-free glass fiber cloth EWR600-100.
[0038] The rare earth elements are a mixture of Sc, Y and Nd in a mass ratio of 2.3:1:0.13; the nano-reinforcement component is a mixture of nano-tantalum boride, nano-niobium silicide and nano-scandium nitride in a mass ratio of 1:0.9:0.15; and the particle size of the nano-reinforcement component is 30nm.
[0039] A method for preparing an aluminum-based composite material comprises the following steps:
[0040] Step S1: using aluminum ingots, Si-Al master alloys, Sr-Al master alloys, Cu-Al master alloys, Ga-Al master alloys, V-Al master alloys, Cr-Al master alloys, Hf-Al master alloys, Re-Al master alloys, Os-Al master alloys, Be-Al master alloys, Te-Al master alloys, rare earth element-Al master alloys and Mo-Al master alloys as raw materials, mixing them in proportion, and smelting them in a vacuum induction furnace to form an alloy melt; then adding the nano-reinforcement component preheated at 530° C. to the above alloy melt, and obtaining a matrix material melt after multi-energy field treatment;
[0041] Step S2: pouring the matrix material melt prepared in step S1 into a mold preheated at 440° C. and containing the modified reinforcing fiber cloth, and demoulding the mold after cooling and solidification;
[0042] Step S3: obtaining an aluminum-based composite material after heat treatment.
[0043] The smelting temperature in step S1 is 720°C; the multi-energy field treatment in step S1 includes ultrasonic treatment and magnetic field treatment, the ultrasonic frequency of the ultrasonic treatment is 35KHZ, the power is 800W, and the time is 10min; the magnetic field intensity of the magnetic field treatment is 7000Gs, and the time is 6.5min; the heat treatment in step S3 includes solution treatment, aging treatment and annealing treatment; the temperature of the solution treatment is 495°C, the holding time is 1.5h, and the room temperature is water-cooled; the temperature of the aging treatment is 210°C, and the time is 8.5h; the temperature of the annealing treatment is 440°C, and the time is 3.5h.
[0044] Embodiment 3
[0045] An aluminum-based composite material comprises a matrix material and a modified reinforcing fiber cloth uniformly distributed in the matrix material, wherein the modified reinforcing fiber cloth accounts for 10% of the weight of the aluminum-based composite material; the matrix material comprises the following components in percentage by mass: 4% Si, 0.2% Sr, 2% Cu, 0.02% Ga, 0.1% V, 0.4% Cr, 0.2% Hf, 0.02% Re, 0.0035% Os, 0.002% Be, 0.02% Te, 0.15% rare earth element, 0.2% Mo and 0.04% nano-reinforcement component, and the balance is Al.
[0046] The preparation method of modified reinforced fiber cloth comprises the following steps: dispersing a modifier in water, mixing evenly, immersing the reinforced fiber cloth therein for 15 hours, taking it out, and drying it at 107°C to constant weight to obtain the modified reinforced fiber cloth; the modifier is a mixture of sodium silicate and 1,3-bis[tris(hydroxymethyl)methylamino]propane in a mass ratio of 2:0.4; the mass ratio of the modifier to water is 1:6.5; and the reinforced fiber cloth is Qinghai Guxiang GX-CF300 carbon fiber cloth.
[0047] The rare earth elements are a mixture of Sc, Y and Nd in a mass ratio of 2.5:1:0.15; the nano-reinforcement component is a mixture of nano-tantalum boride, nano-niobium silicide and nano-scandium nitride in a mass ratio of 1:1:0.2; and the particle size of the nano-reinforcement component is 40nm.
[0048] A method for preparing an aluminum-based composite material comprises the following steps:
[0049] Step S1: using aluminum ingots, Si-Al master alloys, Sr-Al master alloys, Cu-Al master alloys, Ga-Al master alloys, V-Al master alloys, Cr-Al master alloys, Hf-Al master alloys, Re-Al master alloys, Os-Al master alloys, Be-Al master alloys, Te-Al master alloys, rare earth element-Al master alloys and Mo-Al master alloys as raw materials, mixing them in proportion, and smelting them in a vacuum induction furnace to form an alloy melt; then adding the nano-reinforcement component preheated at 550° C. to the above alloy melt, and obtaining a matrix material melt after multi-energy field treatment;
[0050] Step S2: pouring the matrix material melt prepared in step S1 into a mold preheated at 450° C. and containing the modified reinforcing fiber cloth, and demoulding the mold after cooling and solidification;
[0051] Step S3: obtaining an aluminum-based composite material after heat treatment.
[0052] The smelting temperature in step S1 is 740°C; the multi-energy field treatment in step S1 includes ultrasonic treatment and magnetic field treatment, the ultrasonic frequency of the ultrasonic treatment is 35KHZ, the power is 900W, and the time is 12min; the magnetic field intensity of the magnetic field treatment is 9000Gs, and the time is 7min; the heat treatment in step S3 includes solution treatment, aging treatment and annealing treatment; the temperature of the solution treatment is 500°C, the holding time is 2h, and the room temperature is water-cooled; the temperature of the aging treatment is 230°C, and the time is 9h; the temperature of the annealing treatment is 480°C, and the time is 4h.
[0053] Embodiment 4
[0054] An aluminum-based composite material comprises a matrix material and a modified reinforcing fiber cloth uniformly distributed in the matrix material, wherein the modified reinforcing fiber cloth accounts for 11% of the weight of the aluminum-based composite material; the matrix material comprises the following components in percentage by mass: 4.5% Si, 0.25% Sr, 2.5% Cu, 0.025% Ga, 0.13% V, 0.45% Cr, 0.25% Hf, 0.025% Re, 0.004% Os, 0.0025% Be, 0.025% Te, 0.18% rare earth element, 0.25% Mo and 0.045% nano-reinforcement component, and the balance is Al.
[0055] The preparation method of modified reinforced fiber cloth comprises the following steps: dispersing a modifier in water, mixing evenly, immersing the reinforced fiber cloth therein for 18 hours, taking it out, and drying it at 109° C. to constant weight to obtain the modified reinforced fiber cloth; the modifier is a mixture of sodium silicate and 1,3-bis[tris(hydroxymethyl)methylamino]propane in a mass ratio of 2.5:0.45; the mass ratio of the modifier to water is 1:7.5; and the reinforced fiber cloth is Qinghai Guxiang GX-CF300 carbon fiber cloth.
[0056] The rare earth elements are a mixture of Sc, Y and Nd in a mass ratio of 2.8:1:0.18; the nano-reinforcement component is a mixture of nano-tantalum boride, nano-niobium silicide and nano-scandium nitride in a mass ratio of 1:1.1:0.25; and the particle size of the nano-reinforcement component is 70nm.
[0057] A method for preparing an aluminum-based composite material comprises the following steps:
[0058] Step S1: using aluminum ingots, Si-Al master alloys, Sr-Al master alloys, Cu-Al master alloys, Ga-Al master alloys, V-Al master alloys, Cr-Al master alloys, Hf-Al master alloys, Re-Al master alloys, Os-Al master alloys, Be-Al master alloys, Te-Al master alloys, rare earth element-Al master alloys and Mo-Al master alloys as raw materials, mixing them in proportion, and smelting them in a vacuum induction furnace to form an alloy melt; then adding the nano-reinforcement component preheated at 590° C. to the above alloy melt, and obtaining a matrix material melt after multi-energy field treatment;
[0059] Step S2: pouring the matrix material melt prepared in step S1 into a mold preheated at 460° C. and containing the modified reinforcing fiber cloth, and demoulding the mold after cooling and solidification;
[0060] Step S3: obtaining an aluminum-based composite material after heat treatment.
[0061] The smelting temperature in step S1 is 760°C; the multi-energy field treatment in step S1 includes ultrasonic treatment and magnetic field treatment, the ultrasonic frequency of the ultrasonic treatment is 45KHZ, the power is 1000W, and the time is 13min; the magnetic field intensity of the magnetic field treatment is 11000Gs, and the time is 9min.
[0062] The heat treatment in step S3 includes solution treatment, aging treatment and annealing treatment; the temperature of the solution treatment is 505°C, the holding time is 2.5h, and the room temperature is water-cooled; the temperature of the aging treatment is 250°C, the time is 9.5h; the temperature of the annealing treatment is 500°C, and the time is 4.5h.
[0063] Embodiment 5
[0064] An aluminum-based composite material comprises a matrix material and a modified reinforcing fiber cloth uniformly distributed in the matrix material, wherein the modified reinforcing fiber cloth accounts for 12% of the weight of the aluminum-based composite material; the matrix material comprises the following components in percentage by mass: 5% Si, 0.3% Sr, 3% Cu, 0.03% Ga, 0.15% V, 0.5% Cr, 0.3% Hf, 0.03% Re, 0.005% Os, 0.003% Be, 0.03% Te, 0.2% rare earth element, 0.3% Mo and 0.05% nano-reinforcement component, and the balance is Al.
[0065] The preparation method of modified reinforced fiber cloth comprises the following steps: dispersing a modifier in water, mixing evenly, immersing the reinforced fiber cloth in the water for 20 hours, taking out, and drying at 110°C to constant weight to obtain the modified reinforced fiber cloth; the modifier is a mixture of sodium silicate and 1,3-bis[tris(hydroxymethyl)methylamino]propane in a mass ratio of 3:0.5; the mass ratio of the modifier to water is 1:8; and the reinforced fiber cloth is 06 alkali-free glass fiber cloth EWR600-100.
[0066] The rare earth elements are a mixture of Sc, Y and Nd in a mass ratio of 3:1:0.2; the nano-reinforcement component is a mixture of nano-tantalum boride, nano-niobium silicide and nano-scandium nitride in a mass ratio of 1:1.2:0.3; and the particle size of the nano-reinforcement component is 80nm.
[0067] A method for preparing an aluminum-based composite material comprises the following steps:
[0068] Step S1: using aluminum ingots, Si-Al master alloys, Sr-Al master alloys, Cu-Al master alloys, Ga-Al master alloys, V-Al master alloys, Cr-Al master alloys, Hf-Al master alloys, Re-Al master alloys, Os-Al master alloys, Be-Al master alloys, Te-Al master alloys, rare earth element-Al master alloys and Mo-Al master alloys as raw materials, mixing them in proportion, and smelting them in a vacuum induction furnace to form an alloy melt; then adding the nano-reinforcement component preheated at 600° C. to the above alloy melt, and obtaining a matrix material melt after multi-energy field treatment;
[0069] Step S2: pouring the matrix material melt prepared in step S1 into a mold preheated at 470° C. and containing the modified reinforcing fiber cloth, and demoulding the mold after cooling and solidification;
[0070] Step S3: obtaining an aluminum-based composite material after heat treatment.
[0071] The smelting temperature in step S1 is 770°C; the multi-energy field treatment in step S1 includes ultrasonic treatment and magnetic field treatment, the ultrasonic frequency of the ultrasonic treatment is 50KHZ, the power is 1100W, and the time is 15min; the magnetic field intensity of the magnetic field treatment is 12000Gs, and the time is 10min.
[0072] The heat treatment in step S3 includes solution treatment, aging treatment and annealing treatment; the temperature of the solution treatment is 510°C, the holding time is 3 hours, and the temperature is water-cooled at room temperature; the temperature of the aging treatment is 260°C, the time is 10 hours; the temperature of the annealing treatment is 510°C, and the time is 5 hours.
[0073] Comparative Example 1
[0074] An aluminum-based composite material and a preparation method thereof are basically the same as those of the first embodiment, except that Hf, Re and nano-niobium silicide are not added.
[0075] Comparative Example 2
[0076] An aluminum-based composite material and a preparation method thereof are basically the same as those of the first embodiment, except that Be, Te and nano-tantalum boride are not added.
[0077] In order to further illustrate the beneficial technical effects of the aluminum-based composite materials involved in each embodiment of the present invention, relevant performance tests were performed on the aluminum-based composite materials involved in Example 1-5 and Comparative Example 1-2. The test results are shown in Table 1. The test method is as follows:
[0078] (1) Thermal conductivity: The thermal conductivity of each composite material was tested in accordance with GB / T 3651-2008 at a test temperature of 100°C.
[0079] (2) Tensile strength: A room temperature tensile test was performed according to GB / T228.1-2010 to measure the tensile strength of each aluminum-based composite material product.
[0080] (3) Corrosion resistance: The room temperature (25°C) immersion corrosion test was conducted, the corrosive medium was a 5wt% NaCl solution, the corrosion specimen was a disc-shaped aluminum-based composite material specimen with a size of Φ15mm×3mm, and the corrosion time was 24h. The weight loss of the aluminum-based composite material specimen before and after corrosion was measured, and the annual corrosion rate (unit: mm / a) of the aluminum-based composite material specimen was calculated based on the surface area of the aluminum-based composite material specimen.
[0081] (4) Wear resistance: The friction and wear of each aluminum-based composite material sample was tested using a MFT-R4000 high-speed reciprocating friction and wear tester. The test load was 30 N, the test time was 5 min, and the friction length was 5 × 10 -3 m, the friction ball is φ4mm Al2O3 material, and the wear volume of the material after friction and wear is measured by a three-dimensional topography instrument to obtain the wear rate; the wear rate W is calculated using the following formula: W=m / N·L, where W is the wear rate (g / N·m); m is the wear mass (g); N is the load (N); and L is the total stroke (m).
[0082] Table 1
[0083] Test items tensile strength Thermal conductivity Wear rate Corrosion resistance unit MPa W / m·K <![CDATA[×10 -10 g / N·m]]> mm / a Embodiment 1 823.2 305 0.07 0.138 Embodiment 2 825.5 309 0.05 0.123 Embodiment 3 828.0 315 0.04 0.116 Embodiment 4 830.1 318 0.02 0.105 Embodiment 5 831.6 323 0.01 0.097 Comparative Example 1 809.8 289 0.23 0.353 Comparative Example 2 805.6 293 0.30 0.479
[0084] It can be seen from the data in Table 1 that the aluminum-based composite materials involved in the embodiments of the present invention have better thermal conductivity, mechanical properties, corrosion resistance and wear resistance than the comparative example products; the addition of Hf, Re, nano-niobium silicide, Be, Te and nano-tantalum boride helps to improve the above properties.
[0085] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. All equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
Claims
1. An aluminum-based composite material, It is characterized in that The invention comprises a matrix material and a modified reinforcing fiber cloth uniformly distributed in the matrix material, wherein the modified reinforcing fiber cloth accounts for 8-12% of the weight of the aluminum-based composite material; the matrix material comprises the following components in percentage by mass: Si 3%-5%, Sr 0.1%-0.3%, Cu 1%-3%, Ga 0.01%-0.03%, V0.05%-0.15%, Cr 0.3%-0.5%, Hf 0.1%-0.3%, Re 0.01%-0.03%, Os 0.001%-0.005%, Be0.001%-0.003%, Te 0.01%-0.03%, rare earth elements 0.1%-0.2%, Mo 0.1%-0.3%, nano-reinforcement components 0.03%-0.05%, and the balance is Al; The preparation method of the modified reinforced fiber cloth comprises the following steps: dispersing a modifier in water, mixing the modifier evenly, immersing the reinforced fiber cloth in the water for 10-20 hours, taking the modifier out, and drying the water at 105-110° C. to a constant weight to obtain the modified reinforced fiber cloth; the modifier is a mixture of sodium silicate and 1,3-bis[tris(hydroxymethyl)methylamino]propane in a mass ratio of (1-3):(0.3-0.5); the mass ratio of the modifier to water is 1:(5-8); the reinforced fiber cloth is any one of GX-CF300 carbon fiber cloth and 06 alkali-free glass fiber cloth EWR600-100; The method for preparing the aluminum-based composite material comprises the following steps: Step S1, using aluminum ingots, Si-Al master alloys, Sr-Al master alloys, Cu-Al master alloys, Ga-Al master alloys, V-Al master alloys, Cr-Al master alloys, Hf-Al master alloys, Re-Al master alloys, Os-Al master alloys, Be-Al master alloys, Te-Al master alloys, rare earth element-Al master alloys, and Mo-Al master alloys as raw materials, mixing the ingredients in proportion, and smelting them in a vacuum induction furnace to form an alloy melt; then adding the nano-reinforcement component preheated at 500-600° C. to the above alloy melt, and obtaining a matrix material melt after multi-energy field treatment; Step S2, pouring the matrix material melt prepared in step S1 into a mold preheated at 430-470° C. and containing the modified reinforcing fiber cloth, and demolding the mold after cooling and solidification; Step S3: obtaining an aluminum-based composite material after heat treatment.
2. The aluminum-based composite material according to claim 1, It is characterized in that The rare earth element is a mixture of Sc, Y and Nd in a mass ratio of (2-3):1:(0.1-0.2).
3. The aluminum-based composite material according to claim 1, It is characterized in that The nano reinforcement component is a mixture of nano tantalum boride, nano niobium silicide and nano scandium nitride in a mass ratio of 1: (0.8-1.2): (0.1-0.3); the particle size of the nano reinforcement component is 10-80nm.
4. The aluminum-based composite material according to claim 1, It is characterized in that The smelting temperature in step S1 is 700-770°C.
5. The aluminum-based composite material according to claim 1, It is characterized in that The multi-energy field treatment in step S1 includes ultrasonic treatment and magnetic field treatment. The ultrasonic frequency of the ultrasonic treatment is 20-50kHz, the power is 600-1100W, and the time is 8-15min; the magnetic field intensity of the magnetic field treatment is 5000-12000Gs, and the time is 5-10min.
6. The aluminum-based composite material according to claim 1, It is characterized in that The heat treatment in step S3 includes solution treatment, aging treatment and annealing treatment; the temperature of the solution treatment is 490-510°C, the holding time is 1-3h, and the temperature is room temperature and water-cooled; the temperature of the aging treatment is 180-260°C, the time is 8-10h; the temperature of the annealing treatment is 420-510°C, and the time is 3-5h.