A polyimide aerogel composite diaphragm with thermal shutdown function and its preparation method and application
By introducing polyethylene glycol into the lithium metal battery separator, it melts and blocks the pores at high temperatures, realizing the thermal shutdown function of the lithium metal battery, solving the problem of thermal runaway of the existing lithium metal battery separator at high temperatures, and improving the efficiency of the battery. security and performance.
Patent Information
- Application Number
- CN202410250711.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-03-05
AI Technical Summary
Existing lithium metal battery separators suffer from thermal runaway under high temperature conditions, resulting in safety risks, and cannot meet the separator requirements of high-performance lithium metal batteries, such as good thermal stability, high lithium ion mobility and high ion conductivity.
Design a polyimide airgel composite separator with thermal shutdown function. By adding polyethylene glycol to the polyimide pore structure, it melts and blocks the pores at 50-120°C, preventing lithium ion transmission. , thereby realizing the thermal shutdown function of the battery.
Significantly improve the use safety of lithium metal batteries and the thermal stability of the battery, avoid the risk of thermal runaway, and improve the electrolyte affinity and ionic conductivity.
Smart Images

Figure CN118173972B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of membrane materials and batteries, and relates to a polyimide aerogel composite diaphragm with a thermal shutdown function, and a preparation method and application thereof. Background Art
[0002] With the continuous development of industrial technology, energy storage devices such as secondary batteries (such as lithium-ion batteries and sodium-ion batteries) are being used in various fields. However, in order to meet the high demand for energy storage devices in various fields, such as fast-charging batteries for mobile electronic devices and long-life high-energy density batteries for new energy electric vehicles, lithium metal batteries (lithium metal as the negative electrode of the battery) are considered to be one of the candidates for the next generation of high-performance batteries due to their many advantages such as high theoretical capacity and high energy density, and have received extensive attention from researchers; however, in the application process of lithium metal batteries, the irregular dendrite growth on the surface of lithium metal and the rapid electrode reaction that releases a large amount of heat have seriously hindered the industrialization and commercialization of lithium metal batteries, leading to safety issues that cannot be ignored; based on this, researchers have taken many measures to improve the safety of lithium metal batteries.
[0003] Diaphragm engineering is one of the initiatives, which aims to improve the safety of lithium metal batteries through diaphragms with special properties. Currently, commercial battery diaphragms are polyolefin diaphragms, usually polyethylene and polypropylene. They have an uneven microporous structure obtained by stretching, which not only makes it difficult to deposit lithium metal evenly on the surface, but also fails to meet the requirements of high-performance lithium metal batteries for diaphragms: such as good thermal stability, high lithium ion mobility, high ionic conductivity, and stable cyclic charge and discharge capabilities. Using them as diaphragms to assemble lithium metal batteries will seriously affect the safety of lithium metal batteries. Poor thermal stability can easily cause thermal runaway of the battery and even explosion.
[0004] Therefore, whether it is possible to design a high-performance battery separator that can achieve the function of closing the pores when the temperature exceeds a certain level is of great significance for improving the safety of lithium-ion batteries. Summary of the invention
[0005] Purpose of the invention: In view of the problems and shortcomings of the prior art, the present invention provides a polyimide aerogel composite diaphragm with thermal shutdown function for lithium metal batteries and its preparation method and application, which has the advantages of thermal shutdown function, good electrolyte affinity, high ionic conductivity and low interface impedance.
[0006] In the first aspect, the present invention provides a polyimide aerogel composite diaphragm with a thermal shutdown function, in which polyethylene glycol is adhered to the polyimide pore structure in the form of an added phase to form the polyimide aerogel composite diaphragm with a thermal shutdown function, and the thermal shutdown function means that the polyimide aerogel composite diaphragm can achieve pore closure at 50-120°C. The polyimide aerogel composite diaphragm with a thermal shutdown function of the present invention introduces a polyethylene glycol phase into the polyimide aerogel, and the polyethylene glycol phase melts within 50-120°C and blocks the pores in the composite diaphragm, and no longer has ion-conducting properties, so that the composite diaphragm has a thermal shutdown characteristic at 50-120°C, so that when it is applied to a battery, the battery can stop running, and the assembled battery has higher safety.
[0007] In one implementation case, the average pore size of the polyimide aerogel composite membrane with thermal shutdown function is 50-150 nm.
[0008] In one implementation case, the polyimide aerogel composite diaphragm with heat-shutdown function has no obvious thermal shrinkage at 150°C and below, that is, the heat resistance of the polyimide aerogel composite diaphragm is 150°C.
[0009] In one implementation case, the thickness of the polyimide aerogel composite diaphragm with thermal shutdown function is 30-40 μm.
[0010] In one implementation case, the electrolyte contact angle of the polyimide aerogel composite membrane with thermal shutdown function is 0°.
[0011] In one embodiment, the ionic conductivity of the polyimide aerogel composite membrane with thermal shutdown function is greater than 0.40 mS / cm.
[0012] Furthermore, in one embodiment, the ionic conductivity of the polyimide aerogel composite membrane with thermal shutdown function is greater than 0.50 mS / cm.
[0013] Furthermore, in one embodiment, the ionic conductivity of the polyimide aerogel composite membrane with thermal shutdown function is greater than 0.60 mS / cm.
[0014] Furthermore, in one embodiment, the ionic conductivity of the polyimide aerogel composite membrane with thermal shutdown function is greater than 0.70 mS / cm.
[0015] Furthermore, in one embodiment, the ionic conductivity of the polyimide aerogel composite membrane with thermal shutdown function is greater than 0.80 mS / cm.
[0016] Furthermore, in one embodiment, the ionic conductivity of the polyimide aerogel composite membrane with thermal shutdown function is 0.84 mS / cm.
[0017] In one embodiment, the interfacial impedance of the polyimide aerogel composite membrane with thermal shutdown function is lower than 150Ω. Further, lower than 140Ω. Further, lower than 130Ω. Further, lower than 120Ω. Further, lower than 110Ω.
[0018] Furthermore, in one embodiment, the interface impedance of the polyimide aerogel composite membrane with thermal shutdown function is lower than 100Ω.
[0019] Furthermore, in one embodiment, the interface impedance of the polyimide aerogel composite membrane with thermal shutdown function is 95Ω.
[0020] In one embodiment, the charge transfer resistance of the polyimide aerogel composite membrane with thermal shutdown function is less than 70Ω.
[0021] Furthermore, the charge transfer resistance of the polyimide aerogel composite membrane with thermal shutdown function is lower than 60Ω.
[0022] Furthermore, the charge transfer resistance of the polyimide aerogel composite membrane with thermal shutdown function is lower than 50Ω.
[0023] Furthermore, in one embodiment, the charge transfer resistance of the polyimide aerogel composite membrane with thermal shutdown function is 46Ω.
[0024] The second aspect of the present invention is to provide a method for preparing a polyimide aerogel composite diaphragm with a thermal shutdown function, the method comprising the following steps:
[0025] (1) dissolving a diamine monomer in a reaction solvent, introducing nitrogen, and adding a dianhydride monomer under stirring in an ice-water bath to prepare a polyamic acid solution;
[0026] (2) adding an ammonium phosphate crosslinking agent to the polyamic acid solution for crosslinking, then adding a heat-sensitive substance for blending, then adding a silane crosslinking agent for crosslinking, and finally adding an excess of an imidizing agent to obtain a polyimide solution;
[0027] (3) spraying the polyimide solution on the surface of the battery separator to obtain a wet gel composite separator, and then aging it;
[0028] (4) The aged wet gel composite membrane is placed in an organic solvent for solvent exchange, and then dried to obtain a polyimide aerogel composite membrane with a thermal shutdown function.
[0029] The inventive principle of the present invention is that polyethylene glycol adheres to the polyimide pore structure in the form of an additive phase, and the lithium-philic polyethylene glycol can improve multiple properties of the diaphragm (including but not limited to ionic conductivity and interface impedance); at the same time, the melting point of polyethylene glycol is 42-46°C, so the polyethylene glycol phase in the structure will melt within 50-120°C and block the pores in the composite diaphragm, making the composite diaphragm unable to complete the ion transmission required for the electrode reaction, thereby achieving the purpose of thermal shutdown of the battery. Polyethylene glycol will be thermally decomposed above 120°C, so the maximum thermal shutdown temperature is 120°C.
[0030] In one embodiment, in step (1), the diamine monomer is an aromatic diamine monomer, including at least one of p-phenylenediamine, benzidine, diaminodiphenyl ether or diaminobenzophenone, preferably diaminodiphenyl ether.
[0031] In one implementation case, the dianhydride monomer in step (1) is an aromatic dianhydride monomer, including at least one of pyromellitic anhydride, pyromellitic dianhydride, 4,4'-(hexafluoroisopropylene)phthalic anhydride, 4,4'-biphenyl ether dianhydride or benzophenonetetracarboxylic dianhydride, preferably pyromellitic dianhydride.
[0032] In one implementation case, the reaction solvent in step (1) is at least one of N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone, preferably N,N-dimethylacetamide.
[0033] In one implementation case, the molar ratio of the diamine monomer to the dianhydride monomer in step (1) is 1:1-1:1.30, preferably 1:1.10.
[0034] In one implementation case, the reaction time in step (1) is 2-8 hours, preferably 4 hours.
[0035] In one implementation case, the mass concentration of the polyamic acid solution in step (1) is 3wt%-15wt%, preferably 10wt%.
[0036] In one implementation case, in step (2), the ammonium phosphate cross-linking agent includes at least one of ammonium pyrophosphate, ammonium tripolyphosphate, ammonium orthophosphate, and ammonium polyphosphate cross-linking agent, preferably ammonium polyphosphate cross-linking agent.
[0037] In one implementation case, in step (2), the molar ratio of the ammonium phosphate crosslinking agent to the diamine monomer is 1:(0.5-3), preferably 1:1.1.
[0038] In one implementation case, in step (2), the cross-linking time after the addition of the ammonium phosphate cross-linking agent is 10-50 minutes, preferably 30 minutes.
[0039] In one implementation case, in step (2), the heat-sensitive substance is a polyol polymer, and the polyol polymer includes at least one of polyethylene glycol, polypropylene glycol, polypropylene glycol, polybutylene glycol, and polybutanetriol.
[0040] In one embodiment, the polyol polymer is polyethylene glycol.
[0041] Furthermore, in one embodiment, the average molecular weight of the polyethylene glycol is 1000-20000.
[0042] In one embodiment, in step (2), the heat-sensitive substance is dissolved in a second solvent, and the second solvent includes at least one of trifluoromethane, chloroform, and carbon tetrachloride, preferably chloroform.
[0043] In one implementation case, in step (2), the blending time after the heat-sensitive substance is added is 10-50 minutes, preferably 30 minutes.
[0044] In one implementation case, in the step (2), the mass ratio of the heat-sensitive substance to the diamine monomer is 1:(0.1-2), preferably 1:0.3.
[0045] In one embodiment, the silane crosslinking agent in step (2) includes at least one of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropylmethyldiethoxysilane, and 3-aminopropylmethyldimethoxysilane crosslinking agents, preferably 3-aminopropyltriethoxysilane.
[0046] In one implementation case, in step (2), the molar ratio of the silane crosslinking agent to the diamine monomer is 1:(0.5-3), preferably 1:1.1.
[0047] In one implementation case, in step (2), the crosslinking time after the addition of the silane crosslinking agent is 10-50 minutes, preferably 30 minutes.
[0048] In one embodiment, in the step (2), the imidization agent includes a catalyst and a dehydrating agent.
[0049] In one embodiment, the catalyst includes at least one of pyridine, picoline, and triethylamine, preferably triethylamine.
[0050] In one embodiment, the dehydrating agent includes at least one of acetic anhydride, acetyl chloride, thionyl chloride, phosphorus halides, organosilicon compounds, and dicyclohexylcarbocyanine, preferably acetic anhydride.
[0051] In one embodiment, the molar ratio of the dehydrating agent, the catalyst and the diamine monomer is (6-10):(6-10):1, preferably 8:8:1.
[0052] In one implementation case, the imidization time is 10-50 min, preferably 30 min.
[0053] In one embodiment, in step (3), the battery separator includes one of a Celgard membrane, a commercial electrospun polyimide fiber membrane, and a glass fiber membrane, preferably a Celgard membrane.
[0054] In one implementation case, in step (3), the aging condition is standing in air for 0.5-5 minutes, preferably 1 minute.
[0055] In one embodiment, in step (4), the exchange solvent is at least one of methanol, ethanol, acetone, cyclohexane, and n-hexane, preferably anhydrous ethanol and n-hexane;
[0056] In one implementation case, in step (4), the solvent exchange time is 4-24 hours, preferably 12 hours.
[0057] In one implementation case, in step (4), the drying conditions are normal pressure at 25-70°C, preferably 30°C, and the drying time is 1-12h, preferably 5h.
[0058] In a third aspect, the present invention provides a polyimide aerogel composite diaphragm with a thermal shutdown function prepared by the above technical method.
[0059] In one implementation case, the average pore size of the polyimide aerogel composite membrane with thermal shutdown function is 50-150 nm.
[0060] In one implementation case, the polyimide aerogel composite membrane with thermal shutdown function can achieve pore closure at 50-120°C.
[0061] In one implementation case, the polyimide aerogel composite diaphragm with heat-shutdown function has no obvious thermal shrinkage at 150°C and below, that is, the heat resistance of the polyimide aerogel composite diaphragm is 150°C.
[0062] In one implementation case, the thickness of the polyimide aerogel composite diaphragm with thermal shutdown function is 30-40 μm.
[0063] In one implementation case, the electrolyte contact angle of the polyimide aerogel composite membrane with thermal shutdown function is 0°.
[0064] In one embodiment, the ionic conductivity of the polyimide aerogel composite membrane with thermal shutdown function is greater than 0.40 mS / cm.
[0065] Furthermore, in one embodiment, the ionic conductivity of the polyimide aerogel composite membrane with thermal shutdown function is greater than 0.50 mS / cm.
[0066] Furthermore, in one embodiment, the ionic conductivity of the polyimide aerogel composite membrane with thermal shutdown function is greater than 0.60 mS / cm.
[0067] Furthermore, in one embodiment, the ionic conductivity of the polyimide aerogel composite membrane with thermal shutdown function is greater than 0.70 mS / cm.
[0068] Furthermore, in one embodiment, the ionic conductivity of the polyimide aerogel composite membrane with thermal shutdown function is greater than 0.80 mS / cm.
[0069] Furthermore, in one embodiment, the ionic conductivity of the polyimide aerogel composite membrane with thermal shutdown function is 0.84 mS / cm.
[0070] In one embodiment, the interfacial impedance of the polyimide aerogel composite membrane with thermal shutdown function is lower than 150Ω. Further, lower than 140Ω. Further, lower than 130Ω. Further, lower than 120Ω. Further, lower than 110Ω.
[0071] Furthermore, in one embodiment, the interface impedance of the polyimide aerogel composite membrane with thermal shutdown function is lower than 100Ω.
[0072] Furthermore, in one embodiment, the interface impedance of the polyimide aerogel composite membrane with thermal shutdown function is 95Ω.
[0073] In one embodiment, the charge transfer resistance of the polyimide aerogel composite membrane with thermal shutdown function is less than 70Ω.
[0074] Furthermore, the charge transfer resistance of the polyimide aerogel composite membrane with thermal shutdown function is lower than 60Ω.
[0075] Furthermore, the charge transfer resistance of the polyimide aerogel composite membrane with thermal shutdown function is lower than 50Ω.
[0076] Furthermore, in one embodiment, the charge transfer resistance of the polyimide aerogel composite membrane with thermal shutdown function is 46Ω.
[0077] In a fourth aspect of the present invention, the present invention provides a battery separator, wherein the battery separator is the polyimide aerogel composite separator with thermal shutdown function as described in the above technical solution.
[0078] The fifth aspect of the present invention is to provide a use of the above-mentioned polyimide aerogel composite diaphragm with thermal shutdown function, or the use of the polyimide aerogel composite diaphragm with thermal shutdown function prepared by the above-mentioned technical method, and the use includes but is not limited to application in the field of battery diaphragms.
[0079] In one embodiment, the battery separator includes a lithium / sodium metal battery separator.
[0080] The sixth aspect of the present invention is to provide a battery, which comprises a polyimide aerogel composite diaphragm with a thermal shutdown function as described in any one of the above items, or a polyimide aerogel composite diaphragm with a thermal shutdown function prepared by the preparation method as described in any one of the above items.
[0081] In one embodiment, the battery separator includes a lithium / sodium metal battery.
[0082] Compared with the prior art, the present invention has the following beneficial effects:
[0083] 1. In the present invention, polyethylene glycol is added during the synthesis of the polyimide solution, so that the pores of the obtained battery separator are quickly closed under excessively high temperature conditions, thereby preventing lithium ions from continuing to migrate, avoiding dangerous consequences such as thermal runaway, and greatly improving the service life of the battery.
[0084] 2. Using polyimide aerogel as the skeleton and introducing polyethylene glycol into the surface of commercial battery separator can significantly improve the electrolyte affinity of the commercial separator. The preparation method of the composite separator in this patent is universal.
[0085] 3. This invention realizes the thermal shutdown function in the polyimide aerogel membrane. The polyethylene glycol thermal shutdown component introduced into the thermally stable polyimide aerogel framework can close the pore size of the membrane at 50-120°C while ensuring that the composite membrane as a whole has no thermal shrinkage, thereby greatly improving the safety of battery use. BRIEF DESCRIPTION OF THE DRAWINGS
[0086] Figure 1 This is a schematic diagram of the structure and principle of a polyimide aerogel composite diaphragm with thermal shutdown function prepared in an embodiment of the present invention.
[0087] Figure 2 The film thickness test results of the polyimide aerogel composite diaphragm with thermal shutdown function of Example 1, Celgard2500 film of Comparative Example 1 and the polyimide aerogel composite diaphragm without thermal shutdown function of Comparative Example 2 are shown.
[0088] Figure 3 The scanning electron microscope pictures of the polyimide aerogel composite diaphragm with heat shutdown function of Example 1 and the polyimide aerogel composite diaphragm without heat shutdown function of Comparative Example 2 before and after treatment at 120°C.
[0089] Figure 4 The Fourier transform infrared change spectra of the polyimide aerogel composite diaphragm with thermal shutdown function of Example 1, the Celgard2500 film of Comparative Example 1 and the polyimide aerogel composite diaphragm without thermal shutdown function of Comparative Example 2 are shown.
[0090] Figure 5 The Fourier transform infrared spectra of the polyimide aerogel composite diaphragm with heat-shutdown function of Example 1 and the polyimide aerogel composite diaphragm without heat-shutdown function of Comparative Example 2 before and after treatment at 120°C are shown.
[0091] Figure 6 The thermogravimetric test results of the polyimide aerogel composite diaphragm with thermal shutdown function of Example 1, Celgard 2500 membrane of Comparative Example 1, and the polyimide aerogel composite diaphragm without thermal shutdown function of Comparative Example 2 are shown.
[0092] Figure 7 This is a heat shrinkage test of the polyimide aerogel composite diaphragm with heat shutdown function of Example 1, the Celgard2500 film of Comparative Example 1, and the polyimide aerogel composite diaphragm without heat shutdown function of Comparative Example 2.
[0093] Figure 8 The electrolyte contact angle tests are performed on the polyimide aerogel composite diaphragm with thermal shutdown function of Example 1, the Celgard 2500 membrane of Comparative Example 1, and the polyimide aerogel composite diaphragm without thermal shutdown function of Comparative Example 2.
[0094] Fig. 9 Conductivity test of a stainless steel symmetrical battery assembled with the polyimide aerogel composite diaphragm with thermal shutdown function of Example 1, Celgard 2500 membrane of Comparative Example 1, and the polyimide aerogel composite diaphragm without thermal shutdown function of Comparative Example 2.
[0095] Fig.10 The interfacial impedance test of lithium symmetric batteries assembled with the polyimide aerogel composite separator with thermal shutdown function in Example 1, the Celgard 2500 membrane in Comparative Example 1, and the polyimide aerogel composite separator without thermal shutdown function in Comparative Example 2 was performed.
[0096] Fig.11 Charge transfer resistance test of lithium metal batteries assembled with the polyimide aerogel composite separator with thermal shutdown function of Example 1, Celgard 2500 membrane of Comparative Example 1 and the polyimide aerogel composite separator without thermal shutdown function of Comparative Example 2. DETAILED DESCRIPTION
[0097] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0098] Unless otherwise specified, the sources of the reagents used in the embodiments of the present invention can be purchased from the market.
[0099] The present invention provides a characterization test result diagram of Example 1, and other embodiments all adopt the same characterization test method. Those skilled in the art can directly and unambiguously determine the content of the embodiments of the present invention through the characterization test method provided by the present invention, which will not be elaborated here.
[0100] Example 1: Preparation of polyimide aerogel composite membrane with thermal shutdown function
[0101] (1) Place a three-necked flask in an ice-water bath, introduce inert argon gas into the three-necked flask, discharge water and oxygen in the three-necked flask, then add 0.58 g (2.896 mmol) of 4,4'-diaminodiphenyl ether, and then add 23.20 g (0.266 mol) of N,N-dimethylacetamide as a reaction solvent, turn on the stirring device, set the speed to 330 r / min and start stirring, wait for it to dissolve, then add 1.43 g (3.219 mmol) of dianhydride monomer 4,4'-(hexafluoroisopropylene) diphthalic anhydride in three batches, the three batches are 0.50 g, 0.50 g, and 0.43 g respectively. At this time, the solution is yellow. After fully reacting for 4 hours, a transparent polyamide solution with a solid content of 7 wt% is obtained.
[0102] (2) dissolving 0.50 g (0.003 mol) of ammonium polyphosphate in 3.75 g (0.043 mol) of N,N-dimethylacetamide in a small test tube, shaking the test tube to fully dissolve it, adding it to the polyamic acid solution obtained in step (1), stirring at low temperature for 30 min, and performing chemical crosslinking;
[0103] 2.0 g (0.100 mmol) of polyethylene glycol (average molecular weight 20,000) was placed in a small test tube and then 7.4 g (0.062 mol) of chloroform was added. The small test tube was then placed in an ultrasonic machine for ultrasonic treatment to dissolve the polyethylene glycol. The mixture was then added to the reaction system and stirred at low temperature for 30 min to uniformly mix the polyethylene glycol in the polyamide solution.
[0104] Then, 0.65 g (2.92 mmol) of 3-aminopropyltriethoxysilane was added to the solution, and the mixture was stirred at low temperature for 30 min to carry out chemical crosslinking. Then, 2.34 g (0.023 mol) of acetic anhydride was added as a dehydrating agent and 2.36 g (0.023 mol) of triethylamine was added as a catalyst. The speed of the stirring equipment was increased to 380 r / min, and stirring was continued at low temperature for 20 min to obtain a light yellow modified polyimide solution.
[0105] (3) The polyimide solution obtained in step (2) is evenly sprayed on both sides of the Celgard diaphragm with a spray gun, and after aging for 30 seconds, it is immersed in ethanol for 12 hours, and then transferred to n-hexane and immersed for 12 hours to perform solvent exchange.
[0106] (4) Drying the wet gel composite diaphragm obtained in step (3) at room temperature, and after the solvent on the composite diaphragm is completely evaporated, a polyimide aerogel composite diaphragm with a thermal shutdown function can be obtained.
[0107] Example 2: Preparation of polyimide aerogel composite membrane with thermal shutdown function
[0108] The difference from Comparative Example 1 is that the average molecular weight of the polyethylene glycol is 1000.
[0109] (1) Place a three-necked flask in an ice-water bath, introduce inert argon gas into the three-necked flask, discharge water and oxygen in the three-necked flask, then add 0.58 g (2.896 mmol) of 4,4'-diaminodiphenyl ether, and then add 23.20 g (0.266 mol) of N,N-dimethylacetamide as a reaction solvent, turn on the stirring device, set the speed to 330 r / min and start stirring, wait for it to dissolve, then add 1.43 g (3.219 mmol) of dianhydride monomer 4,4'-(hexafluoroisopropylene) diphthalic anhydride in three batches, the three batches are 0.50 g, 0.50 g, and 0.43 g respectively. At this time, the solution is yellow. After fully reacting for 4 hours, a transparent polyamide solution with a solid content of 7 wt% is obtained.
[0110] (2) dissolving 0.50 g (0.003 mol) of ammonium polyphosphate in 3.75 g (0.043 mol) of N,N-dimethylacetamide in a small test tube, shaking the test tube to fully dissolve it, adding it to the polyamic acid solution obtained in step (1), stirring at low temperature for 30 min, and performing chemical crosslinking;
[0111] 2.0 g (0.002 mol) of polyethylene glycol (average molecular weight 1000) was placed in a small test tube and then 7.4 g (0.062 mol) of chloroform was added. The small test tube was then placed in an ultrasonic machine for ultrasonic treatment to dissolve the polyethylene glycol. The mixture was then added to the reaction system and stirred at low temperature for 30 min to uniformly mix the polyethylene glycol in the polyamide solution.
[0112] Then, 0.65 g (2.92 mmol) of 3-aminopropyltriethoxysilane was added to the solution, and the mixture was stirred at low temperature for 30 min to carry out chemical crosslinking. Then, 2.34 g (0.023 mol) of acetic anhydride was added as a dehydrating agent and 2.36 g (0.023 mol) of triethylamine was added as a catalyst. The speed of the stirring equipment was increased to 380 r / min, and stirring was continued at low temperature for 20 min to obtain a light yellow modified polyimide solution.
[0113] (3) The polyimide solution obtained in step (2) is evenly sprayed on both sides of the Celgard diaphragm with a spray gun, and after aging for 30 seconds, it is immersed in ethanol for 12 hours, and then transferred to n-hexane and immersed for 12 hours to perform solvent exchange.
[0114] (4) Drying the wet gel composite diaphragm obtained in step (3) at room temperature, and after the solvent on the composite diaphragm is completely evaporated, a polyimide aerogel composite diaphragm with a thermal shutdown function can be obtained.
[0115] Example 3: Preparation of polyimide aerogel composite diaphragm with thermal shutdown function
[0116] The difference from Comparative Example 1 is that the added amount of the thermosensitive substance polyethylene glycol (average molecular weight 20000) is 1.0 g, and the mass ratio of polyethylene glycol to the diamine monomer is 1:0.58.
[0117] (1) Place a three-necked flask in an ice-water bath, introduce inert argon gas into the three-necked flask, discharge water and oxygen in the three-necked flask, then add 0.58 g (2.896 mmol) of 4,4'-diaminodiphenyl ether, and then add 23.20 g (0.266 mol) of N,N-dimethylacetamide as a reaction solvent, turn on the stirring device, set the speed to 330 r / min and start stirring, after it is dissolved, add 1.43 g (3.219 mmol) of dianhydride monomer into it in three batches, the three batches are 0.50 g, 0.50 g, and 0.43 g respectively. At this time, the solution is yellow. After fully reacting for 4 hours, a yellow polyamide solution is obtained with a solid content of 7 wt%.
[0118] (2) dissolving 0.50 g (0.003 mol) of ammonium polyphosphate in 3.75 g (0.043 mol) of N,N-dimethylacetamide in a small test tube, shaking the test tube to fully dissolve it, adding it to the polyamic acid solution obtained in step (1), stirring at low temperature for 30 min, and performing chemical crosslinking;
[0119] 1.0 g (0.050 mmol) of polyethylene glycol (average molecular weight 20,000) was placed in a small test tube and then 7.4 g (0.062 mol) of chloroform was added. The small test tube was then placed in an ultrasonic machine for ultrasonic treatment to dissolve the polyethylene glycol. The mixture was then added to the reaction system and stirred at low temperature for 30 min to uniformly mix the polyethylene glycol in the polyamide solution.
[0120] Then, 0.65 g (2.92 mmol) of 3-aminopropyltriethoxysilane was added to the solution, and the mixture was stirred at low temperature for 30 min to carry out chemical crosslinking. Then, 2.34 g (0.023 mol) of acetic anhydride was added as a dehydrating agent and 2.36 g (0.023 mol) of triethylamine was added as a catalyst. The speed of the stirring equipment was increased to 380 r / min, and stirring was continued at low temperature for 20 min to obtain a light yellow modified polyimide solution.
[0121] (3) The polyimide solution obtained in step (2) is evenly sprayed on both sides of the Celgard diaphragm with a spray gun, and after aging for 30 seconds, it is immersed in ethanol for 12 hours, and then transferred to n-hexane and immersed for 12 hours to perform solvent exchange.
[0122] (4) Drying the wet gel composite diaphragm obtained in step (3) at room temperature, and after the solvent on the composite diaphragm is completely evaporated, a polyimide aerogel composite diaphragm with a thermal shutdown function can be obtained.
[0123] Example 4: Preparation of polyimide aerogel composite diaphragm with thermal shutdown function
[0124] The difference from Comparative Example 1 is that the reaction solvent is 33.41 g (0.384 mol) of N,N-dimethylacetamide, and step (1) obtains a transparent polyamide solution with a solid content of 5 wt%.
[0125] (1) Place a three-necked flask in an ice-water bath, introduce inert argon gas into the three-necked flask, discharge water and oxygen in the three-necked flask, then add 0.58 g (2.896 mmol) of 4,4'-diaminodiphenyl ether, and then add 33.41 g (0.384 mol) of N,N-dimethylacetamide as a reaction solvent, turn on the stirring device, set the speed to 330 r / min and start stirring, wait for it to dissolve, then add 1.43 g (3.219 mmol) of dianhydride monomer 4,4'-(hexafluoroisopropylene) diphthalic anhydride in three batches, the three batches are 0.50 g, 0.50 g, and 0.43 g respectively. At this time, the solution is yellow. After fully reacting for 4 hours, a transparent polyamide solution with a solid content of 5 wt% is obtained.
[0126] (2) dissolving 0.50 g (0.003 mol) of ammonium polyphosphate in 4.69 g (0.054 mol) of N,N-dimethylacetamide in a small test tube, shaking the test tube to fully dissolve it, adding it to the polyamic acid solution obtained in step (1), stirring at low temperature for 30 min, and performing chemical crosslinking;
[0127] 2 g (0.100 mmol) of polyethylene glycol (average molecular weight 20,000) was placed in a small test tube and then 7.4 g (0.062 mol) of chloroform was added. The small test tube was then placed in an ultrasonic machine for ultrasonic treatment to dissolve the polyethylene glycol. The mixture was then added to the reaction system and stirred at low temperature for 30 min to uniformly mix the polyethylene glycol in the polyamide solution.
[0128] Then, 0.65 g (2.92 mmol) of 3-aminopropyltriethoxysilane was added to the solution, and the mixture was stirred at low temperature for 30 min to carry out chemical crosslinking. Then, 2.34 g (0.023 mol) of acetic anhydride was added as a dehydrating agent and 2.36 g (0.023 mol) of triethylamine was added as a catalyst. The speed of the stirring equipment was increased to 380 r / min, and stirring was continued at low temperature for 20 min to obtain a light yellow modified polyimide solution.
[0129] (3) The polyimide solution obtained in step (2) is evenly sprayed on both sides of the Celgard diaphragm with a spray gun, and after aging for 30 seconds, it is immersed in ethanol for 12 hours, and then transferred to n-hexane and immersed for 12 hours to perform solvent exchange.
[0130] (4) Drying the wet gel composite diaphragm obtained in step (3) at room temperature, and after the solvent on the composite diaphragm is completely evaporated, a polyimide aerogel composite diaphragm with a thermal shutdown function can be obtained.
[0131] Example 5: Preparation of polyimide aerogel composite membrane with thermal shutdown function
[0132] The difference from Comparative Example 1 is that the reaction solvent is 23.20 g (0.234 mol) of N-methyl-2-pyrrolidone, and the step (1) obtains a transparent polyamide solution with a solid content of 7 wt%.
[0133] (1) Place a three-necked flask in an ice-water bath, introduce inert argon gas into the three-necked flask, discharge water and oxygen in the three-necked flask, then add 0.58 g (2.896 mmol) of 4,4'-diaminodiphenyl ether, and then add 23.20 g (0.234 mol) of N-methyl-2-pyrrolidone as a reaction solvent, turn on the stirring device, set the speed to 330 r / min and start stirring, wait for it to dissolve, then add 1.43 g (3.219 mmol) of dianhydride monomer 4,4'-(hexafluoroisopropylene) diphthalic anhydride in three batches, the three batches are 0.50 g, 0.50 g, and 0.43 g respectively. At this time, the solution is yellow. After fully reacting for 4 hours, a transparent polyamide solution with a solid content of 7 wt% is obtained.
[0134] (2) dissolving 0.50 g (0.003 mol) of ammonium polyphosphate in 6.00 g (0.061 mol) of N-methyl-2-pyrrolidone in a small test tube, shaking the test tube to fully dissolve it, adding it to the polyamic acid solution obtained in step (1), stirring at low temperature for 30 min, and performing chemical crosslinking;
[0135] 2 g (0.100 mmol) of polyethylene glycol (average molecular weight 20,000) was placed in a small test tube and then 7.4 g (0.062 mol) of chloroform was added. The small test tube was then placed in an ultrasonic machine for ultrasonic treatment to dissolve the polyethylene glycol. The mixture was then added to the reaction system and stirred at low temperature for 30 min to uniformly mix the polyethylene glycol in the polyamide solution.
[0136] Then, 0.65 g (2.92 mmol) of 3-aminopropyltriethoxysilane was added to the solution, and the mixture was stirred at low temperature for 30 min to carry out chemical crosslinking. Then, 2.34 g (0.023 mol) of acetic anhydride was added as a dehydrating agent and 2.36 g (0.023 mol) of triethylamine was added as a catalyst. The speed of the stirring equipment was increased to 380 r / min, and stirring was continued at low temperature for 20 min to obtain a light yellow modified polyimide solution.
[0137] (3) The polyimide solution obtained in step (2) is evenly sprayed on both sides of the Celgard diaphragm with a spray gun, and after aging for 30 seconds, it is immersed in ethanol for 12 hours, and then transferred to n-hexane and immersed for 12 hours to perform solvent exchange.
[0138] (4) Drying the wet gel composite diaphragm obtained in step (3) at room temperature, and after the solvent on the composite diaphragm is completely evaporated, a polyimide aerogel composite diaphragm with a thermal shutdown function can be obtained.
[0139] Example 6: Preparation of polyimide aerogel composite membrane with thermal shutdown function
[0140] The difference from Comparative Example 1 is that the spin-coated base film is a polyimide fiber film, and the polyimide aerogel composite diaphragm with thermal shutdown function obtained in step (4) is a polyimide aerogel / fiber / aerogel composite diaphragm.
[0141] (1) Place a three-necked flask in an ice-water bath, introduce inert argon gas into the three-necked flask, discharge water and oxygen in the three-necked flask, then add 0.58 g (2.896 mmol) of 4,4'-diaminodiphenyl ether, and then add 23.20 g (0.266 mol) of N,N-dimethylacetamide as a reaction solvent, turn on the stirring device, set the speed to 330 r / min and start stirring, wait for it to dissolve, then add 1.43 g (3.219 mmol) of dianhydride monomer 4,4'-(hexafluoroisopropylene) diphthalic anhydride in three batches, the three batches are 0.50 g, 0.50 g, and 0.43 g respectively. At this time, the solution is yellow. After fully reacting for 4 hours, a transparent polyamide solution with a solid content of 7 wt% is obtained.
[0142] (2) dissolving 0.50 g (0.003 mol) of ammonium polyphosphate in 3.75 g (0.043 mol) of N,N-dimethylacetamide in a small test tube, shaking the test tube to fully dissolve it, adding it to the polyamic acid solution obtained in step (1), stirring at low temperature for 30 min, and performing chemical crosslinking;
[0143] 2.0 g (0.100 mmol) of polyethylene glycol (average molecular weight 20,000) was placed in a small test tube and then 7.4 g (0.062 mol) of chloroform was added. The small test tube was then placed in an ultrasonic machine for ultrasonic treatment to dissolve the polyethylene glycol. The mixture was then added to the reaction system and stirred at low temperature for 30 min to uniformly mix the polyethylene glycol in the polyamide solution.
[0144] Then, 0.65 g (2.92 mmol) of 3-aminopropyltriethoxysilane was added to the solution, and the mixture was stirred at low temperature for 30 min to carry out chemical crosslinking. Then, 2.34 g (0.023 mol) of acetic anhydride was added as a dehydrating agent and 2.36 g (0.023 mol) of triethylamine was added as a catalyst. The speed of the stirring equipment was increased to 380 r / min, and stirring was continued at low temperature for 20 min to obtain a light yellow modified polyimide solution.
[0145] (3) The polyimide solution obtained in step (2) is evenly sprayed on both sides of the polyimide fiber membrane using a spray gun, and after being aged for 30 seconds, it is immersed in ethanol for 12 hours, and then transferred to n-hexane and immersed for 12 hours to perform solvent exchange.
[0146] (4) Drying the wet gel composite diaphragm obtained in step (3) at room temperature, and after the solvent on the composite diaphragm is completely evaporated, a polyimide aerogel composite diaphragm with a thermal shutdown function can be obtained.
[0147] Comparative Example 1: Celgard 2500 Diaphragm
[0148] Comparative Example 2: Preparation of polyimide aerogel composite diaphragm without thermal shutdown function
[0149] The difference from Comparative Example 1 is that polyethylene glycol is not added in step (2).
[0150] (1) Place a three-necked flask in an ice-water bath, introduce inert argon gas into the three-necked flask, discharge water and oxygen in the three-necked flask, then add 0.58 g (2.896 mmol) of 4,4'-diaminodiphenyl ether, and then add 23.20 g (0.266 mol) of N,N-dimethylacetamide as a reaction solvent, turn on the stirring device, set the speed to 330 r / min and start stirring, wait for it to dissolve, then add 1.43 g (3.219 mmol) of dianhydride monomer 4,4'-(hexafluoroisopropylene) diphthalic anhydride in three batches, the three batches are 0.50 g, 0.50 g, and 0.43 g respectively. At this time, the solution is yellow. After fully reacting for 4 hours, a transparent polyamide solution with a solid content of 7 wt% is obtained.
[0151] (2) dissolving 0.50 g (0.003 mol) of ammonium polyphosphate in 3.75 g (0.043 mol) of N,N-dimethylacetamide in a small test tube, shaking the test tube to fully dissolve it, adding it to the polyamic acid solution obtained in step (1), stirring at low temperature for 30 min, and performing chemical crosslinking;
[0152] Then, 0.65 g (2.92 mmol) of 3-aminopropyltriethoxysilane was added to the solution, and the mixture was stirred at low temperature for 30 min to carry out chemical crosslinking. Then, 2.34 g (0.023 mol) of acetic anhydride was added as a dehydrating agent and 2.36 g (0.023 mol) of triethylamine was added as a catalyst. The speed of the stirring equipment was increased to 380 r / min, and stirring was continued at low temperature for 20 min to obtain a light yellow modified polyimide solution.
[0153] (3) The polyimide solution obtained in step (2) is evenly sprayed on both sides of the Celgard diaphragm with a spray gun, and after aging for 30 seconds, it is immersed in ethanol for 12 hours, and then transferred to n-hexane and immersed for 12 hours to perform solvent exchange.
[0154] (4) Drying the wet gel composite diaphragm obtained in step (3) at room temperature, and after the solvent on the composite diaphragm is completely evaporated, a polyimide aerogel composite diaphragm without a thermal shutdown function can be obtained.
[0155] Experimental example: Structural characterization and performance testing of polyimide aerogel composite membrane with thermal shutdown function
[0156] The assembly process of the button battery is as follows: the polyimide aerogel composite diaphragm with thermal shutdown function prepared in Example 1, the polyimide aerogel composite diaphragm without thermal shutdown function prepared in Comparative Example 2 and the Celgard 2500 diaphragm of Comparative Example 1 are cut into discs with a diameter of 19 mm as diaphragms, and then CR2032 button batteries (LiFePO4|diaphragm|Li) are respectively installed on the battery testing system. The battery performance of the zirconium coordinated polyimide aerogel composite diaphragm prepared in Example 1 is studied at 25°C and in the potential range of 2.4-4.2V; wherein the positive electrode is composed of an active material (LiFePO4), a conductive agent (carbon black) and a binder (polyvinylidene fluoride) in a mass ratio of 8:1:1, and the loading of the active material is about 2.2 mg / cm 2 ; The working electrolyte was LB-124; all cell assemblies were performed in an argon-filled glove box.
[0157] like Figure 2 The structure and principle diagram of the polyimide aerogel composite diaphragm with thermal shutdown function prepared in the embodiment of the present invention is shown. It can be seen from the figure that polyethylene glycol adheres to the polyimide pore structure in the form of an additive phase, and the lithium-philic polyethylene glycol can improve multiple properties of the embodiment diaphragm (including but not limited to ionic conductivity and interface impedance); at the same time, the melting point of polyethylene glycol is 42-46°C, so the polyethylene glycol phase in the structure will melt and block the pores in the composite diaphragm within 50-120°C, and no longer have ion-conducting properties, so that the composite diaphragm has a thermal shutdown characteristic at 50-120°C. Polyethylene glycol will be thermally decomposed above 120°C, so the maximum thermal shutdown temperature of the composite diaphragm is 120°C.
[0158] like Figure 2 The film thickness test results of the polyimide aerogel composite separator with thermal shutdown function of Example 1, the Celgard 2500 separator of Comparative Example 1, and the polyimide aerogel composite separator without thermal shutdown function of Comparative Example 2 are shown. It can be seen that due to the polyimide aerogel coating applied on the battery separator, the polyimide aerogel composite separator with thermal shutdown function of Example 1 and the polyimide aerogel composite separator without thermal shutdown function of Comparative Example 2 have an increased thickness (35 μm) compared with the Celgard 2500 membrane of Comparative Example 1 (27 μm).
[0159] like Figure 3The scanning electron microscope images of the polyimide aerogel composite diaphragm with thermal shutdown function of Example 1 and the polyimide aerogel composite diaphragm without thermal shutdown function of Comparative Example 2 are shown. As can be seen from the figure: the surfaces of both Example 1 and Comparative Example 2 are typical aerogel porous structures with an average pore size of 50-150nm, and the interconnected pore structure helps to improve the porosity of the composite diaphragm. At the same time, the uniformly distributed pore structure can reduce the irregular dendrite growth on the surface of the lithium metal electrode during the operation of the lithium metal battery, thereby improving the safety of the lithium metal battery. In addition, after the polyimide aerogel composite diaphragm with a thermal shutdown function in Example 1 and the polyimide aerogel composite diaphragm without a thermal shutdown in Comparative Example 2 were heated at 120°C, it was found through scanning electron microscopy that the pores allowing ion transmission in the polyimide aerogel composite diaphragm with a thermal shutdown function in Example 1 were completely closed, showing a smooth surface, and the thermal shutdown safety function of the battery at 50-120°C could be achieved. The polyimide aerogel composite diaphragms obtained in Examples 2-6 were subjected to the same experimental method and obtained the same results as in Example 1, that is, after being heated at 120°C, the pores allowing ion transmission in the polyimide aerogel composite diaphragm were completely closed, showing a smooth surface, and the thermal shutdown safety function of the battery at 50-120°C could be achieved. The transport pores are completely closed, showing a smooth surface, and can achieve the thermal shutdown safety function of the battery at 120°C (the thermal shutdown function specifically refers to the slow melting of polyethylene glycol adhered to the polyimide pore structure when the temperature rises to 50-120°C, blocking the pore size of the diaphragm used for ion transport, thereby blocking the electrode reaction; the setting of the thermal shutdown temperature comes from the properties of the thermosensitive substance polyethylene glycol itself that plays a blocking role, and the temperature range should be above the melting point of polyethylene glycol: 42-46°C, and the thermal decomposition temperature starts to be below 120°C, that is, 50-120°C); while the polyimide aerogel composite diaphragm without thermal shutdown function in Comparative Example 2 still maintains the original pore structure.
[0160] like Figure 4 The Fourier transform infrared spectra of the polyimide aerogel composite diaphragm with thermal shutdown function of Example 1, Celgard 2500 diaphragm of Comparative Example 1 and the polyimide aerogel composite diaphragm without thermal shutdown function of Comparative Example 2 are shown. It can be seen that: Comparative Example 1 is at 2838 cm -1 -CH2- symmetric stretching vibration, 2866cm -1 -CH3 symmetric stretching vibration, 2918cm -1 -CH2- asymmetric stretching vibration and 2950cm -1 The -CH3 asymmetric stretching vibration is attributed to the characteristic peak of polypropylene. The infrared spectrum of the polyimide aerogel composite diaphragm without thermal shutdown function in comparative example 2 is located at 1782cm -1 The C=O vibration at 1723 cm-1 is attributed to the imine bond. -1 Belongs to the benzene ring, located at 1342cm -1The CN vibrations attributable to the imide bond represent the successful synthesis of polyimide. The polyimide aerogel composite membrane of Example 1 also has characteristic peaks of polyimide, representing the successful synthesis of polyimide materials, and the peaks appearing at 2880 cm -1 The vibration at is attributed to the -OH vibration from the presence of polyethylene glycol, which represents the successful introduction of polyethylene glycol into the polyimide aerogel composite membrane of Example 1;
[0161] like Figure 5 The Fourier infrared change spectra of the polyimide aerogel composite diaphragm with a thermal shutdown function in Example 1 and the polyimide aerogel composite diaphragm without a thermal shutdown function in Comparative Example 2 before and after heat treatment at 120°C are shown. It can be seen that after the heat treatment, the characteristic peaks of Comparative Example 2 have no obvious changes, indicating that the polyimide has good thermal stability; at the same time, after the polyimide aerogel composite diaphragm with a thermal shutdown function in Example 1 is heat treated at 120°C, the corresponding characteristic peaks of polyimide and polyethylene glycol have no obvious changes. Analysis shows that the structure of the polyimide aerogel prepared in Example 1 of the present invention has strong thermal stability, and the thermal shutdown function is achieved through the phase change of polyethylene glycol, that is, the polyethylene glycol in the diaphragm pores melts to block the ion transport channel, and finally the battery reaction is stopped.
[0162] like Figure 6 The thermogravimetric test results of the polyimide aerogel composite diaphragm with thermal shutdown function in Example 1, the Celgard2500 diaphragm in Comparative Example 1, and the polyimide aerogel composite diaphragm without thermal shutdown function in Comparative Example 2 show that the thermal decomposition of the Celgard 2500 membrane in Comparative Example 1 is mainly the decomposition of the polypropylene material at 250°C; in the thermogravimetric results of the polyimide aerogel composite diaphragm with thermal shutdown function in Example 1, the polyethylene glycol component begins to melt and thermally decompose at 120°C, and actually accounts for 9.6% of the total weight. At 250°C, the middle layer Celgard membrane, that is, the thermal decomposition of the polyolefin material, begins; the main thermal decomposition is at 350°C, which is attributed to the thermal decomposition of the polyimide aerogel material; compared with the polyimide aerogel composite diaphragm without polyethylene glycol added in Comparative Example 2, the polyimide aerogel composite diaphragm with thermal shutdown function in Example 1 has obvious thermal decomposition hysteresis.
[0163] like Figure 7The thermal shrinkage test of the polyimide aerogel composite diaphragm with thermal shutdown function in Example 1, the Celgard2500 diaphragm in Comparative Example 1 and the polyimide aerogel composite diaphragm without thermal shutdown function in Comparative Example 2 is shown in the figure. The thermal stability of the polyimide aerogel composite diaphragm with thermal shutdown function in Example 1 up to 150°C is intuitively shown; on the contrary, the Celgard 2500 film in Comparative Example 1 and the polyimide aerogel composite diaphragm without thermal shutdown function in Comparative Example 2 both show different degrees of thermal shrinkage at 150°C. A large degree of thermal shrinkage can cause a short circuit in the battery, greatly affecting the safety of the battery. The enhanced thermal stability of the polyimide aerogel composite diaphragm with thermal shutdown function in Example 1 comes from the fact that the molten polyethylene glycol strengthens the skeleton strength of the overall diaphragm, thereby obtaining more excellent thermal stability.
[0164] like Figure 8 The figure shows the electrolyte contact angle test of the polyimide aerogel composite diaphragm with a thermal shutdown function of Example 1, the Celgard 2500 diaphragm of Comparative Example 1 and the polyimide aerogel composite diaphragm without a thermal shutdown function of Comparative Example 2. It can be seen that: the polyimide aerogel composite diaphragm with a thermal shutdown function of Example 1 has excellent electrolyte affinity, and the contact angle with the liquid electrolyte is 0°, while the Celgard 2500 diaphragm of Comparative Example 1 has a contact angle of up to 90.1° due to the poor affinity between the non-polar polyolefin material and the electrolyte; the polyimide aerogel composite diaphragm without a thermal shutdown function of Comparative Example 2 has good affinity with the electrolyte due to the polarity of its polyimide material, and the contact angle is 13.8°. In addition, the interconnecting pore structure of the polyimide aerogel coating can quickly absorb the electrolyte, and the electrolyte contact angle of Comparative Example 2 becomes 0° after 1 minute.
[0165] like Fig. 9 The figure shows the conductivity test of the polyimide aerogel composite diaphragm with thermal shutdown function of Example 1, the Celgard 2500 diaphragm of Comparative Example 1 and the polyimide aerogel composite diaphragm without thermal shutdown function of Comparative Example 2. It can be seen that the polyimide aerogel composite diaphragm with thermal shutdown function of Example 1 has a higher ionic conductivity than the Celgard 2500 diaphragm of Comparative Example 1 (0.37 mS / cm) and the polyimide aerogel composite diaphragm without thermal shutdown function of Comparative Example 2 (0.40 mS / cm), and the ionic conductivity is 0.84 mS / cm.
[0166] like Fig.10The interface impedance test of the polyimide aerogel composite diaphragm with thermal shutdown function of Example 1, Celgard 2500 diaphragm of Comparative Example 1 and polyimide aerogel composite diaphragm without thermal shutdown function of Comparative Example 2 is shown. It can be seen that the polyimide aerogel composite diaphragm with thermal shutdown function of Example 1 has a lower interface impedance (95Ω) than the Celgard 2500 diaphragm of Comparative Example 1 (907Ω) and the polyimide aerogel composite diaphragm without thermal shutdown function of Comparative Example 2 (297Ω).
[0167] like Fig.11 The charge transfer resistance test of the polyimide aerogel composite membrane with thermal shutdown function of Example 1, the Celgard 2500 membrane of Comparative Example 1, and the polyimide aerogel composite membrane without thermal shutdown function of Comparative Example 2 is shown. It can be seen that the polyimide aerogel composite membrane with thermal shutdown function of Example 1 has a lower charge transfer resistance (46Ω) than the Celgard 2500 membrane of Comparative Example 1 (553Ω) and the polyimide aerogel composite membrane without thermal shutdown function of Comparative Example 2 (72Ω).
[0168] It should be noted that Examples 2-6 can also use the same method as Example 1 to perform product performance testing, and also obtain similar technical effects as Example 1, which will not be repeated in this application.
[0169] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A polyimide aerogel composite diaphragm with thermal shutdown function, characterized in that: Polyethylene glycol adheres to the polyimide pore structure in the form of an additive phase to form the polyimide aerogel composite diaphragm with a thermal shutdown function, wherein the thermal shutdown function means that the pores of the composite diaphragm are closed at 50-120°C and no longer have ion-conducting properties; The method for preparing the polyimide aerogel composite diaphragm with thermal shutdown function comprises the following steps: (1) dissolving a diamine monomer in a reaction solvent, introducing nitrogen, and adding a dianhydride monomer under stirring in an ice-water bath to prepare a polyamic acid solution; (2) adding an ammonium phosphate crosslinking agent to the polyamic acid solution for crosslinking, then adding a heat-sensitive substance for blending, then adding a silane crosslinking agent for crosslinking, and finally adding an excess of an imidizing agent to obtain a polyimide solution; the heat-sensitive substance is polyethylene glycol, the average molecular weight of the polyethylene glycol is 1000-20000, and the mass ratio of the heat-sensitive substance to the diamine monomer is 1:(0.1-2); (3) spraying the polyimide solution on the surface of the battery separator to obtain a wet gel composite separator, and then aging it; (4) The aged wet gel composite membrane is placed in an organic solvent for solvent exchange and then dried to obtain a polyimide aerogel composite membrane with a thermal shutdown function.
2. The polyimide aerogel composite diaphragm with thermal shutdown function according to claim 1, characterized in that: The electrolyte contact angle of the polyimide aerogel composite diaphragm is 0°. The polyimide aerogel composite diaphragm with thermal shutdown function has an ion conductivity greater than 0.40 mS / cm, an interface impedance less than 150 Ω, and a charge transfer resistance less than 70 Ω.
3. The polyimide aerogel composite diaphragm with thermal shutdown function according to claim 1, characterized in that: The diamine monomer in step (1) is an aromatic diamine monomer, including at least one of p-phenylenediamine, benzidine, diaminodiphenyl ether or diaminobenzophenone; The dianhydride monomer in step (1) is an aromatic dianhydride monomer, including at least one of pyromellitic anhydride, pyromellitic dianhydride, 4,4'-(hexafluoroisopropylene) diphthalic anhydride, 4,4'-biphenyl ether dianhydride or benzophenone tetracarboxylic dianhydride; The reaction solvent in step (1) is at least one of N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone; In the step (1), the molar ratio of the diamine monomer to the dianhydride monomer is 1:1-1:1.30; The reaction time in step (1) is 2-8 h; The mass concentration of the polyamic acid solution in step (1) is 3 wt%-15 wt%.
4. The polyimide aerogel composite diaphragm with thermal shutdown function according to claim 1, characterized in that: In the step (2), the heat-sensitive substance is dissolved in a second solvent, and the second solvent includes at least one of trifluoromethane, chloroform, and carbon tetrachloride; The blending time after the heat-sensitive substance is added is 10-50 min.
5. The polyimide aerogel composite diaphragm with thermal shutdown function according to claim 1, characterized in that: In the step (2), the ammonium phosphate cross-linking agent includes at least one of ammonium pyrophosphate, ammonium tripolyphosphate, ammonium orthophosphate, and ammonium polyphosphate cross-linking agents. The molar ratio of the ammonium phosphate crosslinking agent to the diamine monomer is 1:(0.5-3); The cross-linking time after the addition of the ammonium phosphate cross-linking agent is 10-50 min; In the step (2), the silane crosslinking agent includes at least one of 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropylmethyldiethoxysilane, and 3-aminopropylmethyldimethoxysilane crosslinking agent, and the molar ratio of the silane crosslinking agent to the diamine monomer is 1:(0.5-3); The crosslinking time after the addition of the silane crosslinking agent is 10-50 min; In the step (2), the imidization agent includes a catalyst and a dehydrating agent; The catalyst comprises at least one of pyridine, picoline and triethylamine; The dehydrating agent includes at least one of acetic anhydride, acetyl chloride, thionyl chloride, phosphorus halides, organosilicon compounds, and dicyclohexylcarbodiimide; The molar ratio of the dehydrating agent, the catalyst and the diamine monomer is (6-10):(6-10):1; The imidization time is 10-50 min.
6. The polyimide aerogel composite diaphragm with thermal shutdown function according to claim 1, characterized in that: In step (3), the battery separator includes one of Celgard membrane, commercial electrospun polyimide fiber membrane, and glass fiber membrane; The aging condition is to stand in air for 0.5-5 min.
7. The polyimide aerogel composite diaphragm with thermal shutdown function according to claim 1, characterized in that: In step (4), the solvent is at least one of methanol, ethanol, acetone, cyclohexane, and n-hexane; The solvent exchange time is 4-24 h; The drying conditions are normal pressure, 25-70°C, and drying for 1-12 hours.
8. Use of the polyimide aerogel composite diaphragm with thermal shutdown function as claimed in any one of claims 1 to 7, in the field of battery diaphragms.
9. A battery, characterized in that: The battery comprises the polyimide aerogel composite separator with thermal shutdown function as described in any one of claims 1 to 7.