A long-life catalyst for the hydrogenation of uranyl nitrate, its preparation method and application

By dispersing active metals in clusters on a mesoporous silica support, a long-life catalyst was prepared, solving the problems of easy catalyst aggregation and short lifespan. This enabled a highly efficient uranyl nitrate reduction reaction, meeting the long-term stability and activity requirements for industrial applications.

CN118179487BActive Publication Date: 2026-11-17DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202211585404.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-09
Publication Date
2026-11-17
Estimated Expiration
2042-12-09

AI Technical Summary

Technical Problem

Existing catalysts for the reduction of uranyl nitrate to uranium nitrate suffer from problems such as easy agglomeration of active metals, short lifespan, and poor stability, making it difficult to meet the long-term and high-efficiency operation requirements for industrial applications.

Method used

Mesoporous silica is used as a support, and active metals are highly dispersed in the pores in the form of clusters. Through preparation methods, active metals such as Pt, Rh, Pd or Ru are confined in the pores of mesoporous silica to form a long-life catalyst. Hydrogen is used as a reducing agent to carry out the hydrogenation reaction of uranyl nitrate at room temperature.

Benefits of technology

The catalyst achieved a uranyl nitrate conversion rate of over 99.5% after 2000 hours of continuous operation at room temperature, and still maintained a conversion rate of over 90% after 5000 hours, meeting the needs of industrial applications and extending the catalyst's service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118179487B_ABST
    Figure CN118179487B_ABST
Patent Text Reader

Abstract

This invention relates to a method for preparing a long-life catalyst for the hydrogenation of uranyl nitrate and its application. The catalyst consists of a support and an active metal. The support is mesoporous silica, and the active metal is one or a mixture of two elements selected from Ru, Rh, Pt, and Pd. The active metal comprises 0.2–5 wt% of the catalyst and is highly dispersed in clusters within the pores of the mesoporous silica, with cluster sizes ranging from 0.4 to 2.5 nm. The catalyst of this invention exhibits excellent catalytic activity at 10°C to 30°C. Using hydrogen as a reducing agent, it can reduce uranyl nitrate (VI) to uranyl nitrate (IV) at room temperature, achieving a uranyl nitrate conversion rate of over 99.5% after 2000 hours of continuous operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a method for preparing a long-life catalyst for the hydrogenation of uranyl nitrate and its application. Specifically, the active metal content is 0.2–5 wt% of the total catalyst mass, highly dispersed in clusters within the mesoporous silica channels of the support, with cluster sizes of 0.4–2.5 nm. Using hydrogen as a reducing agent, the catalyst of this invention exhibits excellent catalytic activity, capable of reducing uranyl nitrate (VI) to uranyl nitrate (IV) at room temperature. After 2000 hours of continuous operation, the conversion rate of uranyl nitrate reaches over 99.5%, and after 5000 hours of operation, the conversion rate still reaches over 90%, meeting the requirements for the industrial application of uranyl nitrate to uranyl nitrate through catalytic reduction. Background Technology

[0002] With the continuous surge in human energy consumption, traditional fossil fuels such as coal, oil, and natural gas are far from meeting the needs of social development. Furthermore, the processing and use of energy generate air pollutants such as carbon dioxide, sulfur dioxide, and nitrogen oxides, severely polluting the natural environment and posing a significant threat to human survival. Nuclear energy, as a green, environmentally friendly, clean, efficient, and safe energy source, is being adopted by an increasing number of countries. Uranium and its related compounds are the main raw materials for nuclear energy and are widely used in industry, agriculture, medicine, and the military. In the natural environment, uranium mainly exists as U(IV) and...

[0003] U(VI) exists in two oxidation states, with U(VI) often existing as uranyl ions (UO2). 2+ UO2 exists in the form of ) in aqueous solution 2+ With good solubility and easy migration, it can cause harm to the body through various routes such as skin and digestive tract absorption. As a reducing agent in the 1B process of the uranium-plutonium co-decontamination separation cycle, U(IV) can completely and rapidly reduce Pu(IV), achieving the separation of uranium and plutonium. Moreover, it does not introduce impurity ions into the system during the reaction, which conforms to the principle of waste minimization. It is an ideal choice for achieving the separation of uranium and plutonium in the uranium-plutonium co-decontamination separation cycle. Therefore, the preparation of U(IV) plays an important role in the implementation of the Purex process.

[0004] The reduction of radioactive uranyl (VI) nitrate to uranium (IV) nitrate is a primary process used in industrial nuclear fuel reprocessing plants. Currently, methods for preparing uranium nitrate from uranyl nitrate include electrolysis, photocatalysis, and heterogeneous catalysis. A pilot plant in my country uses electrolytic reduction in the presence of hydrazine nitrate to prepare uranium nitrate, producing a uranium (IV) content of 75% (total uranium concentration 200 g / L, uranium (IV) concentration 150 g / L). Compared to large-scale commercial reprocessing plants operating abroad, its uranium (IV) concentration and content are relatively low. Heterogeneous catalysis has lower requirements for conditions, simpler equipment, and is easier to industrialize. The Dalian Institute of Chemical Physics uses conventional Pt / SiO2 as a catalyst and hydrazine as a reducing agent to catalytically reduce uranyl nitrate to uranium nitrate, achieving a conversion rate of 100% at 60℃. The French National Nuclear Fuel Company (CNF) used a Pt / SiO2 catalyst with hydrogen as the reducing agent at a hydrogen pressure of 4 MPa to catalytically reduce uranyl nitrate to uranium nitrate, achieving a conversion rate of 96%. The catalyst needed to be replaced after 2000 hours of operation. The Indian Atomic Energy Research Centre (IAARC) conducted a comparative study on the reaction conditions for the catalytic reduction of uranyl nitrate to uranium nitrate using Pt / SiO2 and Pt / Al2O3 catalysts, respectively, with hydrogen and hydrazine nitrate as reducing agents.

[0005] In the reaction system for preparing uranium nitrate from uranyl nitrate, the catalyst is exposed to a strong acid environment for an extended period, thus placing extremely high demands on the catalyst. The catalyst must possess not only high activity and stability but also strong corrosion resistance. Furthermore, due to the significant difference in radii between the reactants uranyl ions and hydrogen ions, the diffusion rates of uranyl ions and hydrogen ions differ depending on the catalyst pore structure. Designing suitable catalyst pores to match the diffusion rates of uranyl ions and hydrogen ions can reduce the occurrence of catalyst poisoning caused by the direct hydrogenation of nitric acid to form nitrogen oxides. Active metal nanoparticles existing in clusters exhibit good catalytic performance in catalytic reactions; however, these particles are prone to aggregation, significantly reducing their catalytic activity. High dispersion of active metals can generate more active centers, increasing their contact area with reactants and thereby improving the reaction rate. Mesoporous silica, with its regular pore structure, narrow pore size distribution, and high specific surface area, can serve as a catalyst support to highly disperse and confine active metal particles within the pores, thereby preventing particle aggregation and enhancing catalyst activity and stability. Simultaneously, a suitable pore structure matches the diffusion rates of uranyl ions and hydrogen ions, suppressing side reactions and thus extending catalyst lifetime. This invention is the first to use mesoporous silica as a catalyst support, confining active metals in cluster form within the pores. At room temperature, long-term, high-efficiency hydrogenation of uranyl nitrate to uranium nitrate was achieved, with a catalyst lifetime exceeding 5000 hours, meeting the industrial application requirements for the reduction of uranyl nitrate to uranium nitrate. Summary of the Invention

[0006] This invention relates to a method for preparing a long-life catalyst for the hydrogenation of uranyl nitrate and its application.

[0007] To achieve the above objectives, the technical solution adopted by the present invention is as follows:

[0008] A long-life catalyst for the hydrogenation of uranyl nitrate comprises a support and an active metal. The support is mesoporous silica, and the active metal is one or a mixture of two elements selected from Pt, Rh, Pd, and Ru. The active metal has a mass percentage of 0.2–5 wt% in the catalyst and is highly dispersed in the pores of the mesoporous silica in the form of clusters with a cluster size of 0.4–2.5 nm.

[0009] The preparation method of the long-life catalyst for hydrogenation of uranyl nitrate is as follows: First, the active metal precursor and the support precursor are prepared into microemulsion solutions. The active metal precursor and silica precursor solutions are simultaneously added dropwise to an aqueous solution containing ammonia. After vigorous stirring, the active metal and silica in the microemulsion are co-precipitated. After static aging, the catalyst is obtained by filtration, washing, drying, and reduction.

[0010] The preparation method of the long-life catalyst is as follows: First, an aqueous solution of the active metal precursor, hexadecyltrimethylammonium bromide (CTAB), and n-hexanol are prepared in a mass ratio of 0.8–1:4–5:5–6 to form a microemulsion solution A containing the active metal, wherein the mass content of the active metal precursor in the solution is (0.1–2.8 wt%); then, an aqueous solution of the silica precursor, CTAB, and n-hexanol are prepared in a mass ratio of 13.5–15:3.6–4: A microemulsion solution B containing a silica support is prepared at a ratio of 0.9–1, wherein the mass content of silica in the solution is (10–20 wt%). Solutions A and B are simultaneously and slowly added dropwise to an ammonia solution, wherein the mass content of the ammonia solution is 5–10 wt%. The mixture is stirred vigorously at 80–100 °C for 2–5 h, allowed to stand overnight, filtered and washed, dried at 80–120 °C for 12–24 h, and reduced with hydrogen at 400–750 °C for 2–4 h to obtain the target catalyst.

[0011] A method for preparing a long-life catalyst, wherein the active metal precursor is one or more of chloroplatinic acid hexahydrate, rhodium trichloride, palladium chloride, or ruthenium trichloride trihydrate; and the silica precursor is one or more of vinyltrimethoxysilane (VTMS) or vinyltriethoxysilane (VTES).

[0012] The preparation method of long-life catalysts involves a mass ratio of solution A to ammonia solution of 1:12.5 to 1:8.

[0013] The application of long-life catalysts for the hydrogenation of uranyl nitrate involves using hydrogen as a reducing agent. Uranyl nitrate begins to undergo a hydrogenation reaction to produce uranium nitrate under the action of the catalyst; the hydrogen pressure is 4-5 MPa.

[0014] Compared with existing technologies, the essential features of this invention are:

[0015] (1) The catalyst prepared by the method of the present invention has active metals dispersed in uniform size clusters, which is beneficial to improving the catalytic activity of the catalyst and reducing the amount of active metals used.

[0016] (2) The support used in the preparation of the catalyst in this invention is mesoporous silica, which has a large specific surface area, which is conducive to the dispersion of active metals and confines the active metals in the channels, preventing the agglomeration of active metal particles to improve the activity and stability of the catalyst, thereby extending the life of the catalyst.

[0017] (3) Compared with the same Pt-based catalyst prepared by the traditional impregnation method, using hydrogen as a reducing agent, it can reduce uranyl nitrate (VI) to uranyl nitrate (IV) at room temperature. After 2000 hours of continuous operation, the conversion rate of uranyl nitrate reaches more than 99.5%, and after 5000 hours of operation, the conversion rate of uranyl nitrate can still reach more than 90%. It meets the requirements for industrial application of uranyl nitrate to prepare uranyl nitrate by catalytic reduction. It can replace the electrolytic reduction of uranyl nitrate to prepare uranyl nitrate currently used in pilot plants. The technical advantages are very significant. Attached Figure Description

[0018] Figure 1 Electron micrograph of the catalyst prepared in Example 1;

[0019] Figure 2 The wide-angle XRD pattern of the catalyst prepared in Example 1;

[0020] Figure 3 The small-angle XRD pattern of the catalyst prepared in Example 1;

[0021] Figure 4 The physical adsorption-desorption curves of the catalyst prepared in Example 5 are shown.

[0022] Figure 5 The pore size distribution diagram is shown for the catalyst prepared in Example 6.

[0023] Figure 6 Electron micrographs of the catalyst prepared in Comparative Example 1;

[0024] Figure 7 The graph shows the experimental results of uranyl nitrate conversion rate in the hydrogenation test of uranyl nitrate in Example 12;

[0025] Figure 8The graph shows the experimental results of uranyl nitrate conversion rate in the hydrogenation test of uranyl nitrate in Example 1 for comparison. Detailed Implementation

[0026] The following examples are provided to illustrate the invention in more detail, but the invention is not limited thereto.

[0027] Example 1

[0028] Preparation of 2Pt / m-SiO2 (Pt mass content is 2wt%)

[0029] First, prepare a microemulsion A containing chloroplatinic acid hexahydrate by mixing 1g of an aqueous solution containing 0.11g of CTAB and 5g of n-hexanol; prepare a microemulsion B containing silica precursor by mixing 15g of an aqueous solution containing 6.33g of VTES, 4g of CTAB and 1g of n-hexanol; prepare an ammonia solution C by dissolving 25g of 25-28wt% ammonia in 100g of water; slowly add solutions A and B dropwise to solution C, react at 80℃ for 3h, let stand overnight, filter and wash, dry at 100℃ for 24h, and reduce at 550℃ for 2h to obtain 2Pt / m-SiO2. Figure 1 The images show electron micrographs and particle size distribution of the catalyst 2Pt / m-SiO2. The figures reveal that Pt is dispersed in clusters within a support with regular channels, exhibiting a narrow and relatively uniform size distribution, ranging from 1.3 to 1.7 nm in diameter, with an average particle size of 1.5 nm. Figure 2 The wide-angle XRD pattern of the catalyst 2Pt / m-SiO2 shows only diffraction peaks of SiO2 and no diffraction peaks of Pt species, indicating that Pt species are highly dispersed on SiO2. Figure 3 The small-angle XRD pattern of the catalyst 2Pt / m-SiO2 shows characteristic diffraction peaks in the 2-6° range, indicating that the support is mesoporous silica. Figure 4 , Figure 5 The physical adsorption-desorption curves and pore size distribution diagrams of the 2Pt / m-SiO2 catalyst are shown, further verifying that the support is mesoporous silica. The pore size distribution diagram shows that the silica channels range from 3.9 to 4.2 nm, with an average pore size of 4.0 nm. Catalyst-related information is shown in Table 1.

[0030] Example 2

[0031] Preparation of 2Rh / m-SiO2 (Rh mass content is 2wt%)

[0032] The difference from Example 1 is that 1g of an aqueous solution containing 0.08g of rhodium trichloride was added instead of the aqueous solution of chloroplatinic acid hexahydrate. The amounts of other materials and operating conditions were the same as in Example 1, resulting in a 2Rh / m-SiO2 catalyst. Electron micrographs show that Rh is dispersed in clusters within the pores of the support, with relatively uniform particle size ranging from 1.6 to 2.1 nm, and an average particle size of 1.8 nm. Catalyst-related parameters are shown in Table 1.

[0033] Example 3

[0034] Preparation of 2Pd / m-SiO2 (Pd mass content 2wt%)

[0035] The difference from Example 1 is that 1g of an aqueous solution containing 0.07g of palladium dichloride was added instead of the aqueous solution of chloroplatinic acid hexahydrate. The amounts of other materials and operating conditions were the same as in Example 1, resulting in a 2Pd / m-SiO2 catalyst. Electron micrographs show that Pd is dispersed in clusters within the pores of the support, with relatively uniform particle size ranging from 1.9 to 2.3 nm, and an average particle size of 2.1 nm. Catalyst-related parameters are shown in Table 1.

[0036] Example 4

[0037] Preparation of 2Ru / m-SiO2 (Ru content 2wt%)

[0038] The difference from Example 1 is that 1g of an aqueous solution containing 0.11g of rhodium trichloride was added instead of an aqueous solution of chloroplatinic acid hexahydrate. The amounts of other materials and operating conditions were the same as in Example 1, resulting in a 2Ru / m-SiO2 catalyst. Electron micrographs show that Rh is dispersed in clusters within the pores of the support, with relatively uniform particle size ranging from 1.6 to 2.0 nm, and an average particle size of 1.7 nm. Catalyst-related parameters are shown in Table 1.

[0039] Example 5

[0040] Preparation of 0.2Pt / m-SiO2 (Pt mass content is 0.2wt%)

[0041] The difference from Example 1 is the addition of 1g of an aqueous solution containing 0.01g of chloroplatinic acid hexahydrate, followed by reduction with hydrogen at 400°C for 4 hours. Other material amounts and operating conditions remained the same as in Example 1, yielding a 0.2Pt / m-SiO2 catalyst. Electron micrographs show that Pt is dispersed in clusters within the pores of the support, with relatively uniform particle size ranging from 0.4 to 1.0 nm, and an average particle size of 0.8 nm. Catalyst-related parameters are shown in Table 1.

[0042] Example 6

[0043] Preparation of 5Pt / m-SiO2 (Pt mass content is 5wt%)

[0044] The difference from Example 1 is the addition of 1g of an aqueous solution containing 0.28g of chloroplatinic acid hexahydrate. Other material amounts and operating conditions remained the same as in Example 1, yielding a 5Pt / m-SiO2 catalyst. Electron micrographs show that Pt is dispersed in clusters within the pores of the support, with relatively uniform particle size ranging from 2.3 to 2.5 nm, and an average particle size of 2.4 nm. Catalyst-related parameters are shown in Table 1.

[0045] Example 7

[0046] Preparation of 1Pt-1Pd / m-SiO2 (Pt and Pd content are 1wt%)

[0047] The difference from Example 1 is that 1g of an aqueous solution containing 0.055g of chloroplatinic acid hexahydrate and 0.034g of palladium dichloride was added instead of the aqueous solution of chloroplatinic acid hexahydrate. Reduction was performed under hydrogen at 750°C for 4 hours. The amounts of other materials and operating conditions were the same as in Example 1, yielding a 1Pt-1Pd / m-SiO2 catalyst. Electron micrographs show that Pt and Pd are dispersed in clusters within the pores of the support, with relatively uniform particle size ranging from 1.7 to 2.2 nm, and an average particle size of 2.0 nm. Catalyst-related parameters are shown in Table 1.

[0048] Example 8

[0049] Preparation of 2Pt-0.5Ru / m-SiO2 (Pt and Ru mass contents of 2wt% and 0.5wt%, respectively)

[0050] The difference from Example 1 is that 1g of an aqueous solution containing 0.11g of chloroplatinic acid hexahydrate and 0.028g of ruthenium trichloride trihydrate was added instead of the aqueous solution of chloroplatinic acid hexahydrate. The amounts of other materials and operating conditions were the same as in Example 1, resulting in a 2Pt-0.5Ru / m-SiO2 catalyst. Electron micrographs show that Pt and Ru are dispersed in clusters on the support, with relatively uniform particle size ranging from 1.4 to 1.7 nm, and an average particle size of 1.6 nm. Catalyst-related parameters are shown in Table 1.

[0051] Example 9

[0052] Preparation of 1Pt / m-SiO2 (Pt mass content is 1wt%)

[0053] Unlike Example 1, 15g of an aqueous solution containing 12.66g of VTES was added, while the amounts of other materials and other operating conditions remained the same as in Example 1, yielding a 1Pt / m-SiO2 catalyst. Electron microscopy images show that Pt and Ru are dispersed in clusters within the pores of the support, with relatively uniform particle size ranging from 1.2 to 1.6 nm, and an average particle size of 1.4 nm. Catalyst-related parameters are shown in Table 1.

[0054] Example 10

[0055] 15g of an aqueous solution containing 4.93g of VTMS was added, with other material amounts and operating conditions remaining the same as in Example 1, to obtain a 2Pt / m-SiO2 catalyst. Electron micrographs show that Pt and Ru are dispersed in clusters within the pores of the support, with relatively uniform particle size ranging from 1.6 to 1.9 nm, and an average particle size of 1.7 nm. Catalyst-related parameters are shown in Table 1.

[0056] Example 11

[0057] The difference from Example 1 is that the reaction temperature was changed from 80℃ to 100℃, and the drying was carried out at 120℃ for 12 hours. Other material amounts and operating conditions remained the same as in Example 1, resulting in a 2Pt / m-SiO2 catalyst. Electron micrographs show that Pt is dispersed in clusters on the support, with relatively uniform particle size ranging from 1.6 to 2.0 nm, and an average particle size of 1.8 nm. Catalyst-related parameters are shown in Table 1.

[0058] Comparative Example 1

[0059] The difference in Example 1 is that a 2Pt / SiO2 catalyst (Pt content of 2wt%) was prepared using the conventional impregnation method. Electron micrographs are shown below. Figure 6 As can be seen from the figure, the catalyst particles are unevenly distributed and relatively large, mostly above 3 nm, with a particle size range of 4–10 nm. Catalyst-related parameters are shown in Table 1.

[0060] Comparative Example 2

[0061] The difference in Example 1 is that P123 (polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer) replaced CTAB, while the amounts of other materials and other operating conditions were the same as in Example 1, resulting in a 2Pt / m-SiO2 catalyst. Electron micrographs show that the support lacks pores, the Pt particles are relatively large and unevenly distributed, with a particle size range of 4–9 nm and an average particle size of 4.5 nm. Catalyst-related parameters are shown in Table 1.

[0062] Comparative Example 3

[0063] The difference in Example 1 is that n-hexylamine replaces n-hexanol, while the amounts of other materials and other operating conditions are the same as in Example 1, resulting in a 2Pt / m-SiO2 catalyst. Electron micrographs show that the Pt support lacks pores, the Pt particles are large and unevenly distributed, with a particle size range of 4–8 nm and an average particle size of 4.8 nm. Catalyst-related parameters are shown in Table 1.

[0064] Table 1. Relevant information for Examples 1-11 and Comparative Example 1

[0065]

[0066] Example 12

[0067] First, the 2Pt / m-SiO2 catalyst prepared in Example 1 was loaded into a uranyl nitrate fixed-bed reactor. Then, at room temperature, a uranyl nitrate solution with a uranium content of 200 g / L and a nitric acid concentration of 2.0 M was mixed with high-pressure hydrogen gas at 4 MPa at the upper end of the fixed bed using a liquid high-pressure pump and added to the fixed-bed reactor. Under the action of the catalyst, uranyl nitrate began to undergo a hydrogenation reaction to produce uranium nitrate. After 40 minutes, the liquid after the reaction was completed flowed out through the lower end outlet of the fixed bed and entered a gas-liquid high-pressure separator for separation. The gas phase flowed out through the back pressure valve and was discharged into the air, while the liquid phase was released through the intermittent valve. Samples were taken every 24 hours to analyze the uranyl nitrate conversion rate. Figure 7 The graph shows the conversion rate of uranyl nitrate versus time. As can be seen from the graph, the conversion rate of uranyl nitrate reaches over 99.5% after 2000 hours of continuous operation, 99.8% after 2016 hours, and still over 91.6% after 5112 hours. The experimental results are shown in Table 2.

[0068] Example 13

[0069] The difference from Example 12 is that the 2Rh / m-SiO2 catalyst prepared in Example 2 was loaded into the uranyl nitrate fixed-bed reactor, while the amounts of other materials and other operating conditions were the same as in Example 1. The experimental results showed that the uranyl nitrate conversion rate reached over 99.5% after 2000 hours of continuous operation, 99.7% after 2016 hours, and still over 90.7% after 5112 hours. The experimental results are shown in Table 2.

[0070] Example 14

[0071] Unlike Example 12, the 2Pd / m-SiO2 catalyst prepared in Example 3 was loaded into the uranyl nitrate fixed-bed reactor, while the amounts of other materials and other operating conditions were the same as in Example 1. The experimental results showed that the uranyl nitrate conversion rate reached over 99.5% after 2000 hours of continuous operation, 99.7% after 2016 hours, and still over 90.5% after 5112 hours. The experimental results are shown in Table 2.

[0072] Example 15

[0073] Unlike Example 12, the 2Ru / m-SiO2 catalyst prepared in Example 4 was loaded into the uranyl nitrate fixed-bed reactor, while the amounts of other materials and other operating conditions were the same as in Example 1. The experimental results showed that the uranyl nitrate conversion rate reached over 99.5% after 2000 hours of continuous operation, 99.8% after 2016 hours, and still over 91.6% after 5112 hours. The experimental results are shown in Table 2.

[0074] Example 16

[0075] Unlike Example 12, the 0.2 Pt / m-SiO2 catalyst prepared in Example 5 was loaded into the uranyl nitrate fixed-bed reactor, while the amounts of other materials and other operating conditions were the same as in Example 1. The experimental results showed that the uranyl nitrate conversion rate reached over 99.5% after 2000 hours of continuous operation, 99.6% after 2016 hours, and still over 90.2% after 5112 hours. The experimental results are shown in Table 2.

[0076] Example 17

[0077] Unlike Example 12, the 5Pt / m-SiO2 catalyst prepared in Example 6 was loaded into the uranyl nitrate fixed-bed reactor, while the amounts of other materials and other operating conditions were the same as in Example 1. The experimental results showed that the uranyl nitrate conversion rate reached over 99.5% after 2000 hours of continuous operation, 99.8% after 2016 hours, and still over 91.5% after 5112 hours. The experimental results are shown in Table 2.

[0078] Example 18

[0079] Unlike Example 12, the 2Pt-0.5Ru / m-SiO2 catalyst prepared in Example 8 was loaded into the uranyl nitrate fixed-bed reactor, while the amounts of other materials and other operating conditions were the same as in Example 1. The experimental results showed that the uranyl nitrate conversion rate reached over 99.5% after 2000 hours of continuous operation, 99.8% after 2016 hours, and still over 91.7% after 5112 hours. The experimental results are shown in Table 2.

[0080] Comparative Example 4

[0081] Unlike Example 12, the 2Pt / SiO2 catalyst prepared in Comparative Example 1 was loaded into the uranyl nitrate fixed-bed reactor, while the amounts of other materials and other operating conditions were the same as in Example 1. The experimental results showed that after 1000 hours of continuous operation, the uranyl nitrate conversion rate decreased to below 95%. After 1008 hours of operation, the uranyl nitrate conversion rate was 93.3%. With continued operation, the conversion rate gradually decreased, and the 2000-hour operation test could not be completed. The experimental results are shown in Table 2.

[0082] Comparative Example 5

[0083] Unlike Example 12, the 2Pt / SiO2 catalyst prepared in Comparative Example 2 was loaded into a uranyl nitrate fixed-bed reactor, while the amounts of other materials and other operating conditions were the same as in Example 1. The experimental results showed that after 1000 hours of continuous operation, the uranyl nitrate conversion rate decreased to below 95%. After 1008 hours of operation, the uranyl nitrate conversion rate was 90.5%. With continued operation, the conversion rate gradually decreased, and the 2000-hour operation test could not be completed. The experimental results are shown in Table 2.

[0084] Table 2. Test results of Examples 12-18 and Comparative Example 2

[0085]

[0086] Results Evaluation and Analysis: The table shows that the catalyst of this invention (Examples 12-18) exhibits good catalytic activity and lifetime. Using hydrogen as a reducing agent, it can reduce uranyl nitrate (VI) to uranyl nitrate (IV) at room temperature. After 2000 hours of continuous operation, the uranyl nitrate conversion rate reaches over 99.5%, and after 5000 hours of operation, the conversion rate still reaches over 90%. In contrast, catalysts prepared by other methods (Comparative Examples 4-6) have short lifetimes and failed to complete the 2000-hour operation test.

Claims

1. A process for the preparation of a long-lived catalyst for the hydro genation of uranyl nitrate characterized in that: The catalyst consists of two parts: a support and an active metal. The support is mesoporous silica, and the active metal is one or a mixture of two elements selected from Pt, Rh, Pd and Ru. The active metal has a mass percentage of 0.2 to 5 wt% in the catalyst and is highly dispersed in the pores of the mesoporous silica in the form of clusters with a cluster size of 0.4 to 1.0 nm. The specific process is as follows: First, an aqueous solution of the active metal precursor, hexadecyltrimethylammonium bromide, and n-hexanol were prepared in a mass ratio of 0.8~1:4~5:5~6 to form a microemulsion solution A containing the active metal, wherein the mass content of the active metal precursor in microemulsion solution A was 0.1~2.8 wt%. A microemulsion solution B containing a silica carrier was prepared by mixing an aqueous solution of a silica precursor, hexadecyltrimethylammonium bromide, and n-hexanol in a mass ratio of 13.5–15:3.6–4:0.9–1, wherein the silica content in microemulsion solution B was 10–20 wt%. Solution A and solution B are simultaneously and slowly added dropwise to an ammonia solution, wherein the ammonia content is 5-10 wt%. Vigorously stir at 80-100℃ for 2-5 hours, let stand overnight, filter and wash, dry at 80-120℃ for 12-24 hours, and reduce with hydrogen at 400-750℃ for 2-4 hours to obtain the target catalyst.

2. The method of claim 1, wherein the long-life catalyst is prepared by the steps of: The active metal precursor is one or more of chloroplatinic acid hexahydrate, rhodium trichloride, palladium chloride, or ruthenium trichloride trihydrate; The silica precursor is one or a combination of two or more of vinyltrimethoxysilane or vinyltriethoxysilane.

3. The method of claim 1, wherein the long-life catalyst is prepared by the steps of: The mass ratio of solution A to ammonia solution is 1:12.5 to 1:

8.

4. Use of the process according to claim 1 for the preparation of long-lived catalysts for the hydrogenation of uranyl nitrate, characterized in that, Using hydrogen as a reducing agent, uranyl nitrate undergoes a hydrogenation reaction to produce uranium nitrate under the action of a catalyst; the hydrogen pressure is 4~5 MPa.

Citation Information

Patent Citations

  • Spiral mesoporous silicon dioxide nanofiber with cracked surface and preparation method thereof

    CN102502660A

  • Method for loading nano-particles of metal or metallic oxide in mesoporous silica channel

    CN105084372A

  • Method for preparing uranium nitrate through catalytic hydrogenation reduction of uranyl nitrate