A catalyst for the hydrogenation of carbon dioxide to produce liquid solar methanol, its preparation method and application

CN118179530BActive Publication Date: 2026-11-17DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211590002.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-12
Publication Date
2026-11-17
Estimated Expiration
2042-12-12

AI Technical Summary

Technical Problem

[0003]对于二氧化碳加氢合成甲醇的催化剂研究最多的是CuZnO催化剂,铜基催化剂目前最大的挑战在于单程甲醇选择性不高及稳定性较差

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This application relates to a catalyst, preparation method, and application of carbon dioxide hydrogenation to produce liquid solar methanol. For liquid solar methanol, green hydrogen generated from renewable energy reacts with carbon dioxide to produce green methanol. A Si-ZnZrCuX (X = Mn, W, Re) five-membered catalyst prepared by a back-dropping precipitation-impregnation method exhibits high catalytic activity and stability. Cu enhances the ability to activate hydrogen; X (X = Mn, W, Re) partially replaces Zr, with XO... y It exists in a reducible form and is a variable-valence oxide, modulating the valence states of Cu and Zn. The impregnated Si exists in the form of SiO2, acting as a structural aid to protect the active sites of ZnO / Cu on the surface and improve thermal stability. Compared with ZnOZrO2 solid solutions, it improves the conversion rate and lowers the reaction temperature, achieving a methanol space-time yield of 636 mg / (g·h). It produces fewer byproducts and can be applied industrially.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application belongs to the field of catalysts for the synthesis of liquid solar methanol from carbon dioxide resource conversion, specifically involving a catalyst for the production of liquid solar methanol by carbon dioxide hydrogenation, its preparation method, and its application. Background Technology

[0002] Currently, industries such as chemical, metallurgical, cement, steelmaking, and thermal power emit huge amounts of CO2, and decarbonization is difficult in the short term. Hydrogen production using renewable energy and methanol production via CO2 hydrogenation can reduce CO2 emissions in these industries that are difficult to decarbonize. Utilizing renewable energy sources to achieve carbon resource utilization of CO2, and using renewable energy such as solar energy to produce hydrogen through photocatalysis, photoelectrocatalysis, or water electrolysis for CO2 hydrogenation to produce methanol and other fuels and chemicals, is the most feasible strategy for achieving CO2 emission reduction and sustainable carbon resource utilization. Methanol can replace traditional fossil fuels such as coal and oil in the power, transportation, and chemical industries. Large-scale development of methanol production via CO2 hydrogenation can strengthen my country's clean energy industry, enhance my country's energy diversification capabilities, and is an important way to ensure my country's energy security.

[0003] The most studied catalysts for the hydrogenation of carbon dioxide to methanol are CuZnO catalysts. The biggest challenge for copper-based catalysts currently lies in their low selectivity and poor stability in the single-pass methanol synthesis. Researchers typically add co-catalysts [Recent Advances in Carbon Dioxide Hydrogenation to Methanol via Heterogeneous Catalysis. Chem. Rev. 2020, 120, 7984-8034]. These co-catalysts include alkaline earth metals such as K and Ba, rare earth metals such as La and Ce, transition metal oxides such as TiO2 and ZrO2, and main group elements such as SiO2. Supports are usually metal oxides, such as Al2O3, ZrO2, and CeO2, and also include mesoporous SiO2 molecular sieves such as SBA-15, MCF, and KIT-6, and carbon nanotubes.

[0004] Dalian University of Technology's patent CN102302934A reports a novel additive-modified catalyst for the catalytic hydrogenation of carbon dioxide to methanol and its preparation method. The method involves dissolving copper, zinc, and aluminum nitrates in a mixed solution in water, then preparing a mixed solution of tetrabutyl titanate and n-butanol, along with a precipitant solution, and adding this solution dropwise to the copper, zinc, and aluminum nitrate solution to precipitate the catalyst, thus obtaining a silicon-titanium modified copper-zinc-aluminum catalyst, which improves the catalyst activity.

[0005] Kunming University of Science and Technology's patent CN 103230801 A reports the preparation of a mixed solution of copper nitrate, zinc nitrate, and zirconium nitrate. Then, lanthanum nitrate, cerium nitrate, praseodymium nitrate, rubidium nitrate, and tungsten nitrate are dissolved in the copper-zinc-zirconium mixed solution and then co-precipitated with carbonates. This catalyst improves the synergistic effect between catalyst components by adding rare earth additives, thereby enhancing the catalyst's activity. Summary of the Invention

[0006] This application presents a Si-ZnZrCuX (X = Mn, W, Re) pentagonal catalyst prepared by a reverse-dropping precipitation-impregnation method. This catalyst exhibits high catalytic activity and stability. Cu primarily enhances the activation of hydrogen gas; X (X = Mn, W, Re) partially replaces Zr, and XO is the active ingredient in the catalyst. y XO exists in form. y It is a reducible, variable-valence oxide that allows for the adjustment of the valence states of Cu and Zn. The impregnated Si exists in the form of SiO2, which acts as a structural aid, protecting the ZnO / Cu active sites on the catalyst surface and improving catalyst stability. Compared to ZnOZrO2 solid solutions, this catalyst significantly improves carbon dioxide conversion and lowers the reaction temperature, achieving a methanol space-time yield of 636 mg / (g·h) for 1% Si-CuZnZrMn. Furthermore, it produces fewer byproducts, has a simple preparation process, and is suitable for large-scale applications.

[0007] According to one aspect of this application, a catalyst for the synthesis of liquid solar methanol by carbon dioxide hydrogenation is provided, said catalyst comprising an active component and an auxiliary agent;

[0008] The active components include zinc and zirconium.

[0009] The additives include silicon, copper, and other metallic elements;

[0010] The other metals are selected from manganese, tungsten, and rhenium.

[0011] In the catalyst, the molar content of silicon dioxide is 0.1-5%, preferably 0.5-3%, and optionally one of 0.5, 1, 1.5, 2.0, or 3.0%.

[0012] The catalyst contains zinc oxide in a molar amount of 10-45% of the total molar amount, optionally 25%, 27%, or 30%.

[0013] In the catalyst, the molar content of zirconium oxide is 5-30%, optionally 10, 12, 14, or 15%.

[0014] In the catalyst, the molar content of copper oxide is 30-70%, optionally 45%, 50%, 60%, or 65%.

[0015] In the catalyst, the molar content of the other metal oxides is 0.1% to 20%, optionally one of 2%, 4%, 6%, or 8%;

[0016] In the catalyst, the total molar content of zinc oxide and zirconium oxide is 35-50%;

[0017] In the catalyst described above, the molar ratio of the other metal oxides to the zirconium oxide is 1:3 to 3:1.

[0018] The catalyst has a specific surface area of ​​120–180 m². 2 / g;

[0019] The catalyst has a pore size of 9–20 nm;

[0020] The catalyst has a pore volume of 0.4–0.8 cm³. 3 / g.

[0021] According to another aspect of this application, a method for preparing a catalyst for the synthesis of liquid solar methanol by carbon dioxide hydrogenation is provided, the method being a reverse precipitation-impregnation method, comprising the following steps:

[0022] (1) Mix the raw materials containing zinc source and zirconium source with deionized water to obtain mixed solution I;

[0023] (2) Mix and stir the raw materials containing copper source and other metal source with solvent to obtain mixed solution II;

[0024] (3) Add the precipitant to deionized water and stir to obtain a precipitant solution;

[0025] (4) The mixed solution I obtained in (1) and the mixed solution II obtained in (2) are added dropwise to the precipitant solution at a certain temperature and stirring speed to cause a precipitation reaction, and then the precursor is aged and washed with water.

[0026] (5) The precursor is washed with water, dried and calcined to obtain calcined product III.

[0027] (6) Add deionized water to the roasted product III and stir to make a slurry. Add the ethanol solution IV of organosilicon source to cause a hydrolysis reaction. Filter to obtain the impregnated product V.

[0028] (7) The product V is dried to obtain the catalyst used for the synthesis of liquid solar methanol by carbon dioxide hydrogenation.

[0029] The silicon source is selected from at least one of methyl orthosilicate or ethyl orthosilicate;

[0030] The zinc source is selected from at least one of zinc nitrate or acetate;

[0031] The zirconium source is selected from at least one of zirconium nitrate or zirconium oxynitrate;

[0032] The copper source is selected from at least one of copper nitrate or acetate;

[0033] The other metal element sources include one of manganese, tungsten, or rhenium;

[0034] The manganese source is selected from at least one of manganese nitrate, sulfate or acetate;

[0035] The tungsten source is selected from at least one of the high-valent acid salts and halides of tungsten.

[0036] The rhenium source is selected from at least one of the high-valence acid salts and halides of rhenium.

[0037] The total metal ion concentration in the aqueous solution containing zinc, zirconium, copper and other metal element sources is 0.2–1.2 mol / L, preferably 0.5–0.8 mol / L, and optionally one of 0.5, 0.6, 0.7 and 0.8%.

[0038] In solution IV, the concentration of the organosilicon source ethanol solution is 0.1–0.8 mol / L, preferably 0.2–0.4 mol / L, and optionally one of 0.2, 0.3, or 0.4 mol / L.

[0039] The precipitant is selected from at least one of sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, sodium hydroxide, or potassium hydroxide.

[0040] The concentration of the precipitant in the aqueous solution is 0.3–1.5 mol / L, optionally one of 0.5, 0.8, or 1.0 mol / L.

[0041] The ratio of the mixed salt solution I to the precipitant solution is 1:1 to 1:1.2, and optionally one of 1:1, 1:1.1, or 1:1.2.

[0042] Reverse precipitation involves adding a mixed solution of metal salts dropwise to a precipitant solution to react.

[0043] The dripping rate is 2 to 12 ml / min, and optionally one of 5, 8, or 10 ml / min;

[0044] The criterion for determining the endpoint of the dropping is that the pH of the precipitant solution is 5 to 9, and optionally one of 6, 7, or 8;

[0045] The precipitation reaction is carried out at a temperature of 50–100°C, optionally 60, 70, or 80°C.

[0046] The precipitation reaction time is 1 to 10 hours, optionally 2, 3, 4, or 5 hours.

[0047] The aging time after the precipitation reaction is 2 to 16 hours, optionally 4, 6, or 8 hours.

[0048] The hydrolysis reaction time is 2 to 16 hours, and optionally one of 4, 6, or 8 hours.

[0049] The drying process employs a constant temperature forced-air drying oven to remove the solvent, with a drying temperature of 50–150°C, optionally one of 60, 80, 100, or 120°C.

[0050] The drying time is 4 to 24 hours, and optionally 8 to 15 hours.

[0051] The calcination is selected from static calcination or flowing atmosphere calcination, and the calcination atmosphere is selected from at least one of air, oxygen, nitrogen, and argon.

[0052] The roasting temperature is 200-500℃, and optionally one of 300, 350, 400, or 450℃;

[0053] The roasting time is 2 to 12 hours, and can be selected from 3, 4, 5, or 6 hours.

[0054] According to another aspect of this application, a catalyst for the synthesis of liquid solar methanol by hydrogenation of carbon dioxide is provided, the catalyst being selected from the above-described catalysts for the synthesis of liquid solar methanol by hydrogenation of carbon dioxide or the catalysts for the synthesis of liquid solar methanol by hydrogenation of carbon dioxide prepared by the above-described preparation method.

[0055] The catalyst undergoes pretreatment before use;

[0056] The preprocessing procedure includes at least the following steps:

[0057] The catalyst is treated in an activating atmosphere at a temperature of 150–350°C, preferably 220–300°C;

[0058] The catalyst is treated in an activating atmosphere for 2 to 24 hours, preferably 2 to 8 hours; optionally, one of 2, 5, or 8 hours.

[0059] The pressure of the activating atmosphere is 0.1 to 1 MPa, preferably 0.1 to 0.5 MPa; optionally, it is one of 0.1, 0.3, or 0.5 MPa.

[0060] The activating atmosphere is selected from a mixture of hydrogen and inactive gases;

[0061] The inactive gas is selected from at least one of helium, argon or nitrogen;

[0062] The volume concentration of hydrogen in the activation atmosphere is 2-99.999%, preferably 5%-10%. Optionally, it can be one of 5%, 8%, or 10%.

[0063] According to another aspect of this application, a method for synthesizing liquid solar methanol by hydrogenation of carbon dioxide is provided, comprising the following steps:

[0064] A catalyst is loaded into a fixed-bed reactor and activated; then a mixture of carbon dioxide and hydrogen is introduced, and the catalyst is brought into contact with the mixture under certain temperature and pressure to undergo a catalytic reaction; finally, a product containing methanol is obtained.

[0065] The catalyst is selected from the above-mentioned catalysts for the synthesis of liquid solar methanol by hydrogenation of carbon dioxide.

[0066] The molar ratio of hydrogen to carbon dioxide is 1 to 6, preferably 2 to 4; alternatively, it is one of 2, 3, or 4.

[0067] The pressure of the mixed gas is 2-10 MPa, preferably 4-6 MPa; optionally, it is 4, 5, or 6 MPa.

[0068] The feed space velocity of the mixed gas is 4000-24000 mL / (gh), preferably 8000-16000 mL / (gh); optionally, it is one of 8000, 12000, or 16000 mL / (gh).

[0069] The temperature of the catalytic reaction is 160–280°C, preferably 210–260°C. Optionally, it can be any one of 210, 230, 250, or 260°C.

[0070] The beneficial effects of this application are as follows:

[0071] The Si-ZnZrCuX (X = Mn, W, Re) pentagonal catalyst prepared by the reverse-dropping precipitation-impregnation method exhibits high catalytic activity and stability. Compared to ZnOZrO2 solid solutions, this catalyst significantly improves carbon dioxide conversion and lowers the reaction temperature. The methanol space-time yield of 1% Si-CuZnZrMn catalyst reaches 636 mg / (g·h). Furthermore, it produces fewer byproducts, has a simple preparation process, and can be applied to the industrial-scale synthesis of liquid methanol from carbon dioxide resources. Detailed Implementation

[0072] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.

[0073] Unless otherwise specified, all raw materials used in the embodiments of this application were purchased through commercial channels.

[0074] In the following examples, the activity evaluation of the catalyst for the synthesis of methanol from carbon dioxide by hydrogenation was conducted in a pressurized fixed-bed continuous flow reactor-GC combined system. The reaction was carried out under the following conditions: 2–10 MPa, 180–280 °C, a syngas composition of n(H2):n(CO2) molar ratio of 1–6, and a space velocity (GHSV) of 4000–24000 mL / (hg). Before the reaction, the oxidized precursor catalyst was reduced at 250 °C for 2 h in atmospheric pressure, pure hydrogen, nitrogen, argon, or nitrogen and argon diluted hydrogen (flow rate of 20 mL / min). The reaction tail gas was discharged to atmospheric pressure via a back pressure valve, and samples were taken at 150 °C via a 10-port gas chromatograph. The samples were analyzed online using a thermal conductivity detector (TCD) and a flame ionization detector (FID) of an Agilent GC-8890 gas chromatograph. The former uses a 5A molecular sieve coupled with Propark Q (Agilent), with a column length of 3 m, H2 as the carrier gas, and operates at 90 °C, for the separation and detection of CO2, Ar, and CO. The latter uses an HP-PLOT Q capillary column, with dimensions of 30 m × 0.32 mm × 20 μm, N2 as the carrier gas, for the separation and detection of low-carbon hydrocarbons and alcohols. CO2 conversion and the C-based selectivity and space-time yield of carbon-containing products such as CO, alcohols, and hydrocarbons were calculated using the C-based normalization method.

[0075] The formula for calculating the CO2 conversion rate is as follows:

[0076]

[0077] The molecules represent the total amount of each product in the gaseous state after the reaction, including CO, CH4, CH3OH, C2H4, C2H6, CH3OCH3, C3 and C4 products;

[0078] The denominator is the total amount of carbon-containing substances in the gas after the reaction, including unreacted CO2 and products CO, CH4, CH3OH, C2H4, C2H6, CH3OCH3, C3 and C4 substances.

[0079] The formula for calculating methanol selectivity is:

[0080]

[0081] The formula for calculating CO selectivity is:

[0082]

[0083] The formula for calculating methanol yield is:

[0084]

[0085] Where GHSV represents the mass hourly space velocity of the reaction, with units of mL / (g·h), V%(CO2) represents the volume fraction of CO2 in the reaction gas, and X CO2 S represents the CO2 conversion rate. CH3OH This represents the selectivity of methanol.

[0086] Example 1

[0087] Weigh 0.5 mmol Mn(NO3)2·4H2O, 12 mmol Zn(NO3)2·6H2O, 7.5 mmol Zr(NO3)4·5H2O, and 30 mmol Cu(NO3)2·3H2O to prepare a 100 mL salt solution; weigh 60 mmol Na2CO3 to prepare a 120 mL Na2CO3 aqueous solution and place it in a 500 mL four-necked beaker; insert a pH meter and a thermometer, and at 60 °C, add the metal salt solution dropwise in the Na2CO3 aqueous solution to precipitate; stir at 600 r / min, precipitate at 6 mL / min, and control the pH to 7.0; age at 60 °C for 2 h; after aging, filter and wash 5 times with deionized water until no sodium ions are present in the filtrate; dry the filter cake at 80 °C and calcine in air at 350 °C for 4 h to obtain the calcined sample.

[0088] The calcined sample was placed in a 100 ml flask, 50 ml of water was added and stirred to form a slurry, and then 0.25 mmol of (C2H5)4·SiO4 ethanol solution was added to initiate a hydrolysis reaction. The mixture was stirred at room temperature for 2 h; after filtration, it was dried at 120 °C for 6 h to obtain the catalyst 0.5% Si-CuZnZrMn-0.20 MPa was used to press the catalyst into tablets, crush them, and screen them through a 40-80 mesh for evaluation.

[0089] 1.0 g of the selected catalyst was weighed and loaded into a reaction tube with an inner diameter of 6 mm. Reduction was carried out at 250 °C for 2 h under normal pressure and pure H2 at a flow rate of 20 mL / min. Then, a feed gas with a ratio of n(H2):n(CO2) of 3:1 was introduced. The reaction was conducted at 5 MPa, 240 °C, and GHSV = 8000 mL / (hg). Detailed results are shown in Table 1.

[0090] Example 2

[0091] Weigh out 1.0 mmol Mn(NO3)2·4H2O, 12 mmol Zn(NO3)2·6H2O, 7 mmol Zr(NO3)4·5H2O, and 30 mmol Cu(NO3)2·3H2O to prepare a 100 mL salt solution; other steps are the same as in Example 1, to obtain the catalyst 0.5% Si-CuZnZrMn-1. Detailed results are shown in Table 1.

[0092] Example 3

[0093] Weigh out 1.5 mmol Mn(NO3)2·4H2O, 12 mmol Zn(NO3)2·6H2O, 6.5 mmol Zr(NO3)4·5H2O, and 30 mmol Cu(NO3)2·3H2O to prepare a 100 mL salt solution; other steps are the same as in Example 1, to obtain the catalyst 0.5% Si-CuZnZrMn-2. Detailed results are shown in Table 1.

[0094] Example 4

[0095] 2.0 mmol Mn(NO3)2·4H2O, 12 mmol Zn(NO3)2·6H2O, 6.0 mmol Zr(NO3)4·5H2O, and 30 mmol Cu(NO3)2·3H2O were weighed and prepared into a 100 mL salt solution; other steps were the same as in Example 1, to obtain the catalyst 0.5% Si-CuZnZrMn-3. Detailed results are shown in Table 1.

[0096] Example 5

[0097] 12 mmol Zn(NO3)2·6H2O, 7 mmol Zr(NO3)4·5H2O, and 30 mmol Cu(NO3)2·3H2O were weighed to prepare a 100 mL salt solution. 1 mmol WCl6 ethanol solution was added to the salt solution. Other steps were the same as in Example 1, yielding a 0.5% Si-CuZnZrW-1 catalyst. Detailed results are shown in Table 1.

[0098] Example 6

[0099] 12 mmol Zn(NO3)2·6H2O, 7 mmol Zr(NO3)4·5H2O, and 30 mmol Cu(NO3)2·3H2O were weighed to prepare a 100 mL salt solution. 1 mmol ReCl6 in ethanol was added to the salt solution. Other steps were the same as in Example 1, yielding a 0.5% Si-CuZnZrRe-1 catalyst. Detailed results are shown in Table 1.

[0100] Example 7

[0101] 1.0 mmol Mn(NO3)2·4H2O, 12 mmol Zn(NO3)2·6H2O, 7 mmol Zr(NO3)4·5H2O, and 30 mmol Cu(NO3)2·3H2O were weighed to prepare a 100 mL salt solution. During the second impregnation step, 0.5 mmol (C2H5)4·SiO4 was added, and the other steps were the same as in Example 1, yielding a 1.0% Si-CuZnZrMn-1 catalyst. Detailed results are shown in Table 1.

[0102] Example 8

[0103] 1.0 mmol Mn(NO3)2·4H2O, 12 mmol Zn(NO3)2·6H2O, 7 mmol Zr(NO3)4·5H2O, and 30 mmol Cu(NO3)2·3H2O were weighed to prepare a 100 mL salt solution. During the second impregnation step, 0.75 mmol (C2H5)4·SiO4 was added, and the other steps were the same as in Example 1, yielding a 1.5% Si-CuZnZrMn-1 catalyst. Detailed results are shown in Table 1.

[0104] Example 9

[0105] 1.0 mmol Mn(NO3)2·4H2O, 12 mmol Zn(NO3)2·6H2O, 7 mmol Zr(NO3)4·5H2O, and 30 mmol Cu(NO3)2·3H2O were weighed to prepare a 100 mL salt solution. During the second impregnation step, 1.0 mmol (C2H5)4·SiO4 was added, and the other steps were the same as in Example 1, yielding a 2.0% Si-CuZnZrMn-1 catalyst. Detailed results are shown in Table 1.

[0106] Comparative Example 1

[0107] The ZnZrO solid solution catalyst was evaluated at 5 MPa, 320 °C, and GHSV = 8000 mL / (hg). The detailed results are shown in Table 1.

[0108] Detailed results are shown in Table 1.

[0109] Table 1. Catalyst activity evaluation results for the examples and comparative examples.

[0110]

[0111]

[0112] Characterization example

[0113] Table 2. Microstructure of catalytic properties in the examples and comparative examples.

[0114] Comparative Example <![CDATA[Specific surface area (m 2 / g)]]> <![CDATA[Pore volume (cm 3 / g)]]> Aperture (nm) 1.0% Si-CuZnZrMn-1 161 0.52 15.7 ZnZrO catalyst 32 0.06 3.8

[0115] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A method for preparing a catalyst for the hydrogenation of carbon dioxide to methanol, characterized in that, The catalyst contains active components and additives; The active components include zinc and zirconium. The additives include silicon, copper, and other metallic elements; The other metallic elements are selected from at least one of manganese, tungsten, and rhenium; The active components and additives exist in the form of oxides; In the catalyst, the molar content of silicon dioxide is 0.1-5%; In the catalyst, the molar content of zinc oxide is 10-45%; The catalyst contains 5-30% zirconium oxide in molar concentration. The catalyst contains 30-70% copper oxide in molar concentration. In the catalyst, the molar content of other metal oxides is 0.1-20%; In the catalyst, the molar content of zinc oxide and zirconium oxide is 35-50%; The molar ratio of the other metal oxides to the zirconium oxide is 1:3 to 3:1; Its preparation method is a reverse precipitation-impregnation method, which includes the following steps: (1) Mix the raw materials containing zinc source and zirconium source with deionized water to obtain mixed solution I; (2) Mix and stir the raw materials containing copper source and other metal source with solvent to obtain mixed solution II; (3) Add the precipitant to deionized water and stir to obtain an aqueous solution of the precipitant; (4) The mixed solution I obtained in (1) and the mixed solution II obtained in (2) are added dropwise to the precipitant solution at a certain temperature and stirring speed to cause a precipitation reaction, and then the precursor is aged and washed with water. (5) The precursor is washed with water, dried and calcined to obtain calcined product III; (6) Add deionized water to the roasted product III, stir and slurry, add ethanol solution IV of organosilicon source to cause hydrolysis reaction, and filter to obtain the impregnated product V; (7) The product V is dried to obtain the catalyst for the synthesis of methanol by hydrogenation of carbon dioxide.

2. The preparation method according to claim 1, characterized in that, In the catalyst, the molar content of silicon dioxide is 0.5% to 3%; In the catalyst, the molar content of zinc oxide is 25-30%; In the catalyst, the molar content of zirconium oxide is 10-15%; In the catalyst, the molar content of copper oxide is 45-65%; In the catalyst, the molar content of the other metal oxides is 2-8%; The catalyst has a specific surface area of ​​120~180 m². 2 / g, pore size 9~20nm, pore volume 0.4~0.8cm³ 3 / g.

3. The preparation method according to claim 1, characterized in that, The silicon source is selected from at least one of methyl orthosilicate or ethyl orthosilicate; The zinc source is selected from at least one of zinc nitrate or acetate; The zirconium source is selected from at least one of zirconium nitrate or zirconium oxynitrate. The copper source is selected from at least one of copper nitrate or acetate; The other metal element sources include one of manganese, tungsten, or rhenium; The manganese source is selected from at least one of manganese nitrate, sulfate or acetate; The tungsten source is selected from at least one of the high-valent acid salts and halides of tungsten. The rhenium source is selected from at least one of the high-valence acid salts and halides of rhenium. In solution I or II, the concentration of metal ions is 0.2~1.2 mol / L.

4. The preparation method according to claim 1, characterized in that, In solution I or II, the concentration of metal ions is 0.5~0.8 mol / L; In the ethanol solution IV, the concentration of the organosilicon source is 0.1~0.8 mol / L.

5. The preparation method according to claim 1, characterized in that, In the ethanol solution IV, the concentration of the organosilicon source is 0.2~0.4 mol / L.

6. The preparation method according to claim 1, characterized in that, The precipitant is selected from at least one of sodium carbonate, potassium carbonate, sodium bicarbonate, potassium bicarbonate, sodium hydroxide, or potassium hydroxide. The concentration of the precipitant in the aqueous solution is 0.3~1.5 mol / L.

7. The preparation method according to claim 1, characterized in that, The precipitation reaction is carried out at a temperature of 50~100℃; The precipitation reaction takes 1 to 10 hours. The hydrolysis reaction takes 2 to 16 hours. The drying process uses a constant temperature forced-air drying oven to remove the solvent, and the drying temperature is 50~150℃. The drying time is 4~24 hours; The calcination is selected from static calcination or flowing atmosphere calcination, and the calcination atmosphere is selected from at least one of air, oxygen, nitrogen, and argon. The roasting temperature is 200~500℃; The roasting time is 2 to 12 hours.

8. The preparation method according to claim 1, characterized in that, The concentration of the precipitant in the aqueous solution is 0.5~1.0 mol / L; The precipitation reaction is carried out at a temperature of 60~80℃; The precipitation reaction takes 2-5 hours. The hydrolysis reaction takes 4-8 hours. The drying temperature is 60~120℃; The drying time is 8-15 hours; The roasting temperature is 300~450℃; The roasting time is 3 to 6 hours.

9. A catalyst for the hydrogenation of carbon dioxide to methanol, characterized in that, The catalyst is selected from the catalyst for the synthesis of methanol from carbon dioxide hydrogenation according to any one of claims 1 to 8.

10. The catalyst according to claim 9, characterized in that, The catalyst undergoes pretreatment before use; The preprocessing procedure includes at least the following steps: The catalyst is treated in an activation atmosphere at a temperature of 150~350℃; The catalyst is treated in an activating atmosphere for 2-24 hours. The pressure of the activating atmosphere is 0.1~1 MPa; The activating atmosphere is selected from a mixture of hydrogen and inactive gases; The inactive gas is selected from at least one of helium, argon or nitrogen; The volume concentration of hydrogen in the activation atmosphere is 2~99.999%.

11. The catalyst according to claim 9, characterized in that, The catalyst is treated in an activating atmosphere at a temperature of 220~300℃; The catalyst is treated in an activating atmosphere for 2-8 hours. The pressure of the activating atmosphere is 0.1~0.5MPa; The volume concentration of hydrogen in the activation atmosphere is 5% to 10%.

12. A method for synthesizing methanol by hydrogenation of carbon dioxide, characterized in that, Includes the following steps: A catalyst is loaded into a fixed-bed reactor and activated; then a mixture of carbon dioxide and hydrogen is introduced, and the catalyst is brought into contact at a temperature of 160~280℃ and a pressure of 2~10MPa to undergo a catalytic reaction; finally, a product containing methanol is obtained. The catalyst is selected from the catalysts for the synthesis of methanol by hydrogenation of carbon dioxide according to any one of claims 9 to 11.

13. The method according to claim 12, characterized in that, In the mixed gas, the molar ratio of hydrogen to carbon dioxide is 1 to 6; The pressure of the mixed gas is 4~6MPa; The feed space velocity of the mixed gas is 4000–24000 mL / (gh); The temperature of the catalytic reaction is 210~260℃.

14. The method according to claim 12, characterized in that, In the mixed gas, the molar ratio of hydrogen to carbon dioxide is 2 to 4; The feed space velocity of the mixed gas is 8000–16000 mL / (gh).

Citation Information

Patent Citations

  • Novel auxiliary-modified catalyst for preparing methanol by catalytic hydrogenation of carbon dioxide and preparation method of catalyst

    CN102302934A

  • Preparation method for modified CuZnZr used for catalysis of CO2 to synthesize methanol

    CN103230801A

  • Catalyst applicable to synthesis of methanol by multi-component mixed gas as well as preparation method and application of methanol catalyst

    CN104722305A

  • Catalyst for synthesizing methanol by carbon dioxide hydrogenation and preparation and application thereof

    CN107008332A

  • Hydrophobic copper-based catalyst, preparation method and application

    CN107519883A