A bifunctional coke oven gas hydrodesulfurization catalyst, its preparation method and application

The coke oven gas hydrodesulfurization catalyst prepared by the mixed precipitation method solves the problem of pore blockage in traditional methods, and achieves high efficiency and stability in hydrodesulfurization. It is suitable for the purification of coke oven gas, pyrolysis gas, converter gas and coal-to-syngas.

CN118179538BActive Publication Date: 2026-11-17北京启原新材科技有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410397634.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-03
Publication Date
2026-11-17
Estimated Expiration
2044-04-03

AI Technical Summary

Technical Problem

In existing coke oven gas purification technologies, catalysts prepared by traditional impregnation and wet mixing methods are easily blocked by large organic molecules, leading to a decline in catalyst performance. Furthermore, the problem of pore blockage has not been effectively solved, affecting the hydrodesulfurization effect of the catalyst.

Method used

The catalyst was prepared by a mixed precipitation method. Through the mixed precipitation reaction of active components and support precursors, a new pore structure was formed. By controlling conditions such as temperature, pH value and feeding sequence, the uniform distribution of active metal and the formation of large pore size were achieved, thereby enhancing the catalyst's ability to adsorb and accommodate large molecular organic matter.

Benefits of technology

The catalyst exhibits higher hydrodesulfurization performance and stability, can effectively adsorb and transform macromolecular organic matter, extend service life, reduce catalyst replacement frequency, and reduce industrial plant uptime and investment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118179538B_ABST
    Figure CN118179538B_ABST
Patent Text Reader

Abstract

This invention discloses a bifunctional coke oven gas hydrodesulfurization catalyst, its preparation method, and its application. The preparation method of the catalyst includes the following steps: dissolving the active component precursor in ammonia water to form a mixed solution, and kneading the support raw material with an acid solution to form a colloidal material; adding the mixed solution to the colloidal material for mixing and precipitation. The catalyst of this invention contains a large number of large-pore channels, which can absorb, accommodate, and partially convert large molecular organic matter, thereby improving the problem of unstable long-term production caused by increased bed differences in the coke oven gas purification section.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to catalyst synthesis processes, and more particularly to a bifunctional coke oven gas hydrodesulfurization catalyst, its preparation method, and its application. Background Technology

[0002] Since sulfides in coke oven gas are poisons to methanol synthesis catalysts, methane synthesis catalysts, and ammonia synthesis catalysts, and can deactivate these catalysts, thus affecting normal industrial production, coke oven gas must be purified before entering the synthesis tower to minimize the impact of sulfides on chemical synthesis catalysts.

[0003] The desulfurization and purification technology for coke oven gas first removes most of the hydrogen sulfide in the coking section through a wet desulfurization process. The concentration of hydrogen sulfide in the coke oven gas is approximately 50 mg / m³. 3 However, the total organic sulfur in coke oven gas, in various forms such as thiophene, carbonyl sulfide, sulfides, mercaptan, and carbon disulfide, still amounts to approximately 100–200 mg / m³. 3 It also needs to be converted into hydrogen sulfide through hydrogenation, and then removed using desulfurizing agents such as zinc oxide / iron oxide.

[0004] Traditional coke oven gas purification processes for removing organic sulfur consist of pre-hydrogenation, primary hydrodesulfurization, and secondary hydrodesulfurization. However, during actual industrial plant startup, the pre-hydrogenation catalyst often becomes clogged first due to the presence of high-molecular-weight organic compounds in the coke oven gas, such as anthracene, azobenzene, indene, monomethylnaphthalene, 1,6-dimethylnaphthalene, 2,7-dimethylnaphthalene, 2-methylbenzothiophene, dimethylbenzothiophene, and dibenzofuran, as well as colloidal and ash components. This clogs the catalyst bed, leading to increased pressure drop and disrupting normal production.

[0005] Chinese patent CN112742362B discloses a coke oven gas hydrodesulfurization catalyst and its preparation method. The catalyst is prepared by an impregnation method, wherein the active metal component of the catalyst includes molybdenum and Group VIII metals, and the support is raspberry-type oxide microspheres. Based on the oxides and the catalyst, the molybdenum content is 10–45 wt%; the Group VIII metal content is 1–16 wt%; and the support oxide content is 39–89 wt%.

[0006] Chinese patent CN201810684412.X discloses a low-load coke oven gas hydrodesulfurization catalyst. The catalyst uses γ-Al2O3 as a support and loads a certain amount of active components. The active components, by mass percentage of the catalyst, are 0.5-1.5% iron, 13.5% molybdenum, and 0.1-0.5% nickel. The catalyst is prepared by a wet kneading method: iron salt, molybdenum salt, and nickel salt are added to deionized water and stirred to obtain an iron-molybdenum-nickel mixed solution; boehmite and guar gum powder are mixed evenly and added to the iron-molybdenum-nickel mixed solution, kneaded and shaped, dried, and calcined to obtain the catalyst.

[0007] Chinese patent CN202011282489.8 discloses a magnesium-based coke oven gas hydrodesulfurization catalyst and its preparation method. The preparation method of the catalyst includes the following steps: in a hydrogen atmosphere, graphite, magnesium powder, polyurethane and N-doped titanium oxide are mixed and ball-milled to obtain the catalyst; wherein, the mass ratio of the graphite, magnesium powder, polyurethane and N-doped titanium oxide is 3:7:(15):(15); the weight average molecular weight of the polyurethane is 75,000 to 120,000; the N-doped titanium oxide is prepared by the following method: mixing and reacting titanium-containing raw materials and N-containing raw materials; the molar ratio of titanium element in the titanium-containing raw material and nitrogen element in the nitrogen-containing raw material is 1:2 to 2:1. The magnesium-based coke oven gas hydrodesulfurization catalyst of the present invention can achieve a thiophene conversion rate of ≥37% at 300℃, and the stability of the magnesium-based coke oven gas hydrodesulfurization catalyst is significantly improved.

[0008] Chinese patent CN202011227824.4 discloses a coke oven gas hydrodesulfurization catalyst and its preparation method. The catalyst comprises the following raw materials by mass percentage: TiO2 support: 75.0–95.0%, MoO3: 3.0–15.0%, NiO: 0.1–10.0%, and SiO2: 0.5–5.0%. The TiO2 support is prepared by suspending the Ti-containing raw material in a solvent to obtain a suspension, holding the suspension at a certain temperature, filtering to obtain a solid, and calcining the solid. The solvent is a mixture of glycerol, ethanol, and diethyl ether, with a volume ratio of glycerol, ethanol, and diethyl ether of (0.52):2:1. The holding temperature is 140–160°C, and the holding time is 12–48 hours. The coke oven gas hydrodesulfurization catalyst of this invention can achieve a thiophene conversion rate of ≥90% at 200°C and a thiophene conversion rate of ≥95% at 300°C.

[0009] The existing technologies mentioned above only focus on improving the hydrodesulfurization performance of the catalyst itself, ignoring the decline in catalyst performance caused by the blockage of pores by large molecular organic matter. There are no large-pore hydrodesulfurization catalysts suitable for coke oven gas purification. Moreover, the existing technologies all use impregnation methods, wet mixing methods and other methods to prepare hydrodesulfurizing agents. The catalysts prepared by these methods themselves have the above-mentioned shortcomings, resulting in the catalytic performance not reaching the ideal effect.

[0010] In view of this, the present invention is hereby proposed. Summary of the Invention

[0011] To address the problems existing in the prior art, the present invention aims to provide a method for preparing a dual-function coke oven gas hydrodesulfurization catalyst. By adopting the preparation method of the present invention, a new pore structure different from the original structure of the support can be formed inside the catalyst. It has dual functions, namely, the ability to adsorb and accommodate large organic molecules and high-efficiency hydrodesulfurization performance. The distribution of active metals is also more uniform, thus the catalytic performance is more stable.

[0012] To achieve the above objectives, the technical solution of the present invention is as follows:

[0013] The present invention provides a method for preparing a bifunctional coke oven gas hydrodesulfurization catalyst, comprising the following steps: dissolving the active component precursor in ammonia water to form a mixed solution, and kneading the support raw material with an acid solution to form a colloidal material;

[0014] The mixed solution is added to the pectin material and mixed to precipitate.

[0015] In the above preparation method, a mixed precipitation method is used instead of the previously used impregnation and wet kneading methods. This is because the pore structure of catalysts prepared by the impregnation and wet kneading methods mainly depends on the pore structure of the support, while the catalyst prepared by the mixed precipitation method of this invention essentially generates new pores. In the preparation method of this invention, the active component solution and the support precursor undergo a mixed precipitation reaction, generating active metal oxide-support-active metal oxide chemical bonds. Through crystal nucleation, primary particle and secondary particle growth, a new pore structure different from the original structure of the support is formed. Subsequently, by reasonably controlling specific preparation conditions such as temperature, pH, and feeding sequence, the desired catalyst pore structure distribution can be controlled and obtained.

[0016] When preparing catalysts using impregnation and wet mixing methods, the varying adsorption capacities of the support for different active components, along with the varying diffusion and desorption rates of different components on the support, make it difficult to achieve a uniform distribution of multiple components on the support. In the mixed precipitation method of this invention, the active components are bound to the support in the form of metal oxides or hydroxides, eliminating problems such as competitive adsorption. Therefore, the distribution of active metals is more uniform, and the catalytic performance is more stable. This is the advantage of the preparation method of this invention compared to traditional methods.

[0017] Specifically, in the process of preparing the mixed solution, preferably, as a further feasible option, the active component precursor includes at least one of nickel nitrate, ferric nitrate, cobalt nitrate, ammonium heptamolybdate, and ammonium metatungstate.

[0018] Preferably, the sulfur content in the active component precursor is 0-3 wt%, more preferably 1-2 wt%.

[0019] The precursor of the active component can be any one or a mixture of several of the above-mentioned molybdenum salt, nickel salt, cobalt salt, iron salt and tungsten salt.

[0020] Preferably, as a further feasible option, the concentration of the ammonia water is 4-18 wt%, more preferably 6-15 wt%.

[0021] The reason why ammonia water needs to be controlled within a suitable concentration range is that its concentration directly affects the stability of the active metal solution and the pore size of the catalyst.

[0022] Ammonia water promotes the dissolution of ammonium molybdate. The ammonium hydroxide (NH4OH) in ammonia water can combine with molybdate ions (MoO4) to form a cyclic complex (NH4)2[MoO4(OH)2], thus ensuring the stable dissolution of ammonium molybdate in ammonia water. When the ammonia water concentration is below 4 wt%, a stable coexisting active metal mixture solution is not easily formed, leading to uneven dispersion of the active metal in the catalyst. When the ammonia water concentration is above 18 wt%, the precipitate particles formed when the active metal mixes with the support are relatively fine, which is not conducive to the formation of larger pores. Therefore, it is necessary to control the concentration within a suitable range.

[0023] Preferably, as a further feasible option, the temperature for dissolving ammonia is controlled between 30 and 80°C, more preferably between 40 and 65°C.

[0024] The dissolution temperature is also a very important parameter because the solubility of the active metal is directly related to the dissolution temperature. When the dissolution temperature is below 30℃, the solubility of the active metal is low, and the content of the active component in the catalyst is limited. When the dissolution temperature is above 65℃ or even above 80℃, a large amount of free ammonia escapes, which is not conducive to the precise control of pH in the subsequent mixing and precipitation steps, and will seriously affect the operating environment for catalyst preparation.

[0025] Preferably, as a further feasible option, the pH of the mixed solution is controlled at 8.0 to 11.0, more preferably 8.5 to 10.5.

[0026] The pH of the mixed solution affects the state of the active components in the solution, and ultimately affects the uniform distribution of the active components in the subsequent mixing and precipitation steps. When pH > 8.0, especially pH > 8.5, Mo(VI) ions mainly exist as MoO4. 2- The presence of this form avoids the mixing and precipitation process of Mo7O. 24 6- Rapid formation of molybdate precipitates is crucial to prevent uneven distribution of active metal components; therefore, the pH value needs to be controlled within a suitable range. Preferably, as a further feasible option, the carrier material in the preparation of the colloidal material is at least one selected from alumina, titanium dioxide, and silicon dioxide, along with a pore-expanding agent and a binder.

[0027] The alumina precursor, which is a pseudoboehmite, has a pore volume greater than 0.80 mL / g, and more preferably a pseudoboehmite with a pore volume greater than 1.0 mL / g; the titanium dioxide precursor is one or more of metatitanic acid or titanium oxysulfate; and the silica precursor is selected from silica sol.

[0028] The pore-expanding agent can be selected from one or more of the following: guar gum powder, carbon black, methylcellulose, polyethylene glycol, polyethylene oxide, polyvinyl alcohol, and polyacrylamide.

[0029] Preferably, as a further feasible option, the pH of the colloid material is controlled at 4.0 to 8.0, more preferably 5.0 to 7.5.

[0030] Preferably, the acid solution is one or a mixture of two of nitric acid and acetic acid solutions;

[0031] Adding acid to boehmite causes some of it to dissolve through the following reaction:

[0032] AlO(OH)·nH2O+3H + →Al 3+ +(2+n)H2O

[0033] Al is formed by adding acid. 3+Ions can react with molybdenum, cobalt, nickel, iron and other ions in the active metal solution under specific pH conditions to form a uniformly mixed precipitate at the atomic level, and generate new primary and secondary particles. In other words, the active components truly participate in the formation of the catalyst structural phase, which is conducive to the formation of more channels and increases the specific pore volume of the catalyst. This is the fundamental reason for the advantages of the mixed precipitation method of this invention.

[0034] More preferably, the acid solution is a mixture of nitric acid and acetic acid solutions, wherein the concentration of nitric acid is 1-8 wt%, preferably 2-5 wt%; and the concentration of acetic acid is 3-15 wt%, preferably 5-10 wt%.

[0035] Preferably, based on the solute, the mass ratio of nitric acid to acetic acid is (1-2):1;

[0036] However, the concentration of nitric acid cannot be increased indiscriminately. When the concentration exceeds 8 wt%, the colloidal process penetrates deep into the pseudoboehmite particles, disrupting the primary particle packing and reducing the number of macropores. Therefore, to obtain a suitable catalyst pore structure, the nitric acid concentration should not be too high, and should not exceed 8.0 wt%.

[0037] Acetic acid is weaker than nitric acid. It can not only improve the distribution of hydroxyl groups on the support surface and promote the formation of octahedral Mo, but also weaken the interaction between the support and the metal components, making it easier for the active components to disperse and sulfide. At the same time, when the concentration of acetic acid exceeds 15 wt%, the colloidal effect has a destructive effect on the pore structure of the catalyst.

[0038] For the purposes of this invention, the best combination of acids is to form a mixed acid of nitric acid and acetic acid in a specific ratio. This fully utilizes both the good colloidal effect of nitric acid and the role of acetic acid in improving the distribution of active components. Therefore, a good combination of the two can improve the emergence of new pore structures in the mixed precipitation method and also improve the pore distribution.

[0039] Preferably, as a further feasible option, the pH of the mixture after precipitation is measured to be 7.0–9.0, more preferably 7.5–8.5.

[0040] The pH is controlled within the above range because if the pH is too low, the active metal will not precipitate completely and will easily form crystalline precipitates, affecting the dispersion of the metal; if the pH is too high, the precipitate particles formed by the active metal will be finer, which is not conducive to the formation of larger pores.

[0041] Preferably, after mixing and precipitating, the mixture needs to be kneaded or rolled into a plastic body, and then processed, dried, and calcined to obtain the final catalyst product.

[0042] Preferably, the mixing and settling temperature and the kneading / rolling temperature are 30-80℃, more preferably 40-70℃; the drying temperature after molding is 110-150℃, more preferably 120-140℃; and the calcination temperature is 400-600℃, more preferably 450-550℃.

[0043] Preferably, the mixing and settling time is 10-30 min, more preferably 15-25 min; the kneading / rolling time is 1-4 h, more preferably 2-3 h; the drying time is 8-24 h, more preferably 12-16 h; and the calcination time is 1-7 h, more preferably 3-6 h.

[0044] Preferably, the plastic body is adjusted according to different processing techniques to adapt to different molding processes. The molding can be one or more of the following: Raschig ring, cloverleaf, four-leaf clover, toothed ball, cylinder, and porous honeycomb structure.

[0045] Preferably, the shaped and calcined catalyst can be further pre-sulfurized to produce a highly active pre-sulfurized catalyst.

[0046] Preferably, pre-sulfurization can be carried out in the following manner: the calcined catalyst is placed in a pre-sulfurization reactor, and after nitrogen purging, a sulfurizing agent is introduced. The reaction is carried out at a certain temperature and pressure for a certain time, and then the temperature is lowered in a nitrogen atmosphere, and lubricating oil is introduced for passivation.

[0047] Preferably, the vulcanizing agent is one or more of elemental sulfur, hydrogen sulfide, thiols, thioethers, and organic polysulfides dissolved in lubricating oil to form a liquid.

[0048] Preferably, the sulfur content in the vulcanizing agent is 1-30%.

[0049] Preferably, the pre-vulcanization temperature is 200–450°C, the pre-vulcanization pressure is atmospheric pressure to 3 MPa, and the pre-vulcanization time is 2–16 hours.

[0050] In addition to providing the above-mentioned method for preparing the catalyst, the present invention also provides a catalyst prepared by the above-mentioned method, wherein the catalyst uses one of alumina, titanium oxide, and silicon oxide or a composite oxide thereof as a support, and one or more components and oxides and / or sulfides of nickel, cobalt, iron, molybdenum, and tungsten as active components.

[0051] Preferably, the catalyst has a pore size of 5–15 nm, a specific pore volume of 0.8–1.5 mL / g, and a macropore ratio of 30–65% with a pore size between 10–20 nm. This 30–65% ratio refers to the proportion of the total pore volume. In existing impregnation and wet kneading methods, the pore structure mainly depends on the pore structure of the support, with typical values ​​of a specific pore volume of 0.3–0.8 mL / g and a macropore ratio of 10–30% with a pore size between 10–20 nm. Compared with existing methods, this invention not only has simpler steps but also offers advantages in pore size and distribution ratio, resulting in better beneficial effects.

[0052] The catalyst described above can adsorb and accommodate large organic molecules while also possessing hydrodesulfurization performance. It is characterized by having abundant large pores, which enables it to maintain hydrodesulfurization performance stably for a long time.

[0053] Preferably, the composition of the catalyst active components, based on oxides, is as follows: MoO3: 5wt%–15wt%, NiO: 2wt%–8wt%, Fe2O3: 2wt%–8wt%, CoO: 2wt%–8wt%; the catalyst support components are: Al2O3: 50wt%–95wt%, the mass ratio of TiO2 to Al2O3 is 0.1%–10%, and the mass ratio of SiO2 to Al2O3 is 0%–3%. Nickel, cobalt, and iron can be selected as one or more, and molybdenum and tungsten can be selected as one or both.

[0054] More preferably, the composition of the catalyst active components, based on oxides, is as follows: MoO3: 7wt%–13wt%, NiO: 4wt%–7wt%, Fe2O3: 4wt%–7wt%, CoO: 3wt%–6wt%; the catalyst support components are: Al2O3: 55wt%–85wt%, the mass ratio of TiO2 to Al2O3 is 1%–5%, and the mass ratio of SiO2 to Al2O3 is 0%–2.5%. Nickel, cobalt, and iron can be selected as one or more, and molybdenum and tungsten can be selected as one or two.

[0055] In addition, the present invention also provides the use of the above-mentioned catalyst in the preparation of purified syngas through hydrodesulfurization, especially in the processes of coke oven gas, pyrolysis gas, converter gas, blast furnace gas, and coal-to-syngas.

[0056] In summary, the hydrodesulfurization catalyst of this invention is prepared by a mixed precipitation method. By controlling the preparation conditions, the active component and the support precursor are mixed, precipitated, and organically combined, resulting in a larger pore size and volume. The preparation process is simple; the raw materials can contain more sulfur, reducing the production cost of the catalyst; the active component is well dispersed, with small crystallites, high reactivity, and the catalyst is not prone to carbon buildup, resulting in a long service life. The catalyst prepared by this invention has a large specific pore volume, with most pores being macropores of 10–20 nm. Moreover, the distribution ratio is controlled to a certain proportion by appropriate operating conditions in the preparation method. Such a catalyst is more conducive to the mass transfer and conversion of organic sulfur in coke oven gas. The specific conversion rate and yield can be supported by the experimental data of the subsequent examples. It also has a greater capacity for adsorption, containment, and conversion of large molecular organic matter such as tar in coke oven gas. The catalyst surface is not prone to carbon buildup, and the reactor pressure drop is small, solving the problem of frequent catalyst replacement commonly faced by existing industrial plants.

[0057] Furthermore, the hydrodesulfurization catalyst of this invention employs an external pre-sulfurization method, which shortens the start-up time and steps of industrial plants, saves investment in online sulfidation equipment, and minimizes environmental pollution. Attached Figure Description

[0058] Various other advantages and benefits will become apparent to those skilled in the art upon reading the following detailed description of preferred embodiments. The accompanying drawings are for illustrative purposes only and are not intended to limit the invention. Furthermore, the same reference numerals denote the same parts throughout the drawings. In the drawings:

[0059] Figure 1 This is an evaluation device for a dual-functional coke oven gas hydrodesulfurization catalyst according to an embodiment of the present invention.

[0060] Figure 2 The results show the pore distribution of the bifunctional coke oven gas hydrodesulfurization catalyst in Example 1 of this invention. Detailed Implementation

[0061] The technical solution of the present invention will be clearly and completely described below with reference to the accompanying drawings and specific embodiments. However, those skilled in the art will understand that the embodiments described below are some embodiments of the present invention, but not all embodiments, and are only used to illustrate the present invention, and should not be regarded as limiting the scope of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall be followed. Where the manufacturers of reagents or instruments are not specified, they are all conventional products that can be purchased commercially.

[0062] In the description of this invention, it should be noted that the terms "center," "upper," "lower," "left," "right," "vertical," "horizontal," "inner," and "outer," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing the invention and for simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on the invention. Furthermore, the terms "first," "second," and "third" are used for descriptive purposes only and should not be construed as indicating or implying relative importance.

[0063] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," and "linking" should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral connection; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; and they can refer to the internal connection of two components. Those skilled in the art can understand the specific meaning of the above terms in this invention based on the specific circumstances.

[0064] Evaluation method of the hydrodesulfurization catalyst of the present invention:

[0065] As attached Figure 1 The catalysts used in the following examples and comparative examples are all... Figure 1 The evaluation was conducted in a fixed-bed evaluation device. The sulfide passage was handled by passivated sulfur-resistant pipelines, effectively preventing sulfide adsorption. The reactor was constructed with a stainless steel reactor lined with quartz tubes to avoid sulfide adsorption. The experimental feed gas was supplied from gas cylinders. The gas was depressurized and metered by a mass flow meter before entering the reactor. A portion of the effluent was collected for analysis using a desulfurization analyzer, while the remainder was cooled, separated, and metered before being vented. Since the evaluation device is a commonly used device in existing technology, its specific structure will not be described in detail.

[0066] Before the experiment, the catalyst sample was crushed and screened into 10-20 mesh particles, then packed into a quartz-lined reactor. The catalyst was placed in the middle of the reactor's isothermal zone, supported above and below by small glass spheres. The reaction took place under specific conditions of temperature, atmospheric pressure, feed gas composition, and sulfur content.

[0067] The reaction feed gas is taken from the purification section of the coke oven gas to methanol plant, specifically from the inlet of the coke oven gas pre-hydrogenation reactor. Its volume composition is as follows: hydrogen: 62.8%, methane: 21.2%, carbon monoxide: 7.2%, carbon dioxide: 3.1%, nitrogen: 3.4%, CnHm: 1.7%, oxygen: 0.35%, hydrogen sulfide 50ppm, thiophene 150ppm, and also contains trace amounts of tar.

[0068] The sulfidation method of the hydrodesulfurization catalyst of the present invention:

[0069] The active component of the hydrodesulfurization catalyst is a metal sulfide. The hydrodesulfurization catalyst of this invention can be sulfided using an online sulfidation method or a pre-sulfidation method.

[0070] Characterization method of the hydrodesulfurization catalyst of the present invention:

[0071] 1. Specific surface area, specific pore volume, and average pore size were measured using a MicroActiveAutoPore V 9600 mercury porosimeter manufactured by Micromerchant Corporation, USA.

[0072] 2. The composition of the catalyst was determined using a Rigaku ZSX Primus Ⅳ X-ray fluorescence spectrometer.

[0073] 3. Catalyst coking was tested using a STA 449F3 Jupiter simultaneous thermal analyzer from NETZSCH.

[0074] 4. The content of sulfur in its physical form was determined by GC-SCD method. The GC was performed using an Agilent 7890N gas chromatograph from Agilent Technologies, USA, and the SCD was performed using an Agilent 8355 sulfur chemiluminescence detector from Agilent Technologies, USA.

[0075] To more clearly illustrate the technical solutions in this invention, specific embodiments are described below.

[0076] Example 1

[0077] Preparation of bifunctional coke oven gas hydrodesulfurization catalyst by mixed precipitation method:

[0078] 1) Preparation of mixed solution: Weigh 23.9g ammonium heptamolybdate tetrahydrate, 23.4g nickel nitrate hexahydrate, and 11.6g cobalt nitrate hexahydrate respectively, and prepare a mixed solution with pH 10.2 at 56℃ using 13wt% ammonia water.

[0079] 2) Preparation of gel sol material: Weigh 182g of boehmite, 6.0g of titanium oxysulfate and 27.0g of carbon black respectively and mix them thoroughly to obtain a mixture. Add 3wt% dilute nitric acid and 10wt% dilute acetic acid to the mixture. Based on the solute, the mass ratio of nitric acid to acetic acid is 1:1. Knead for 30min to obtain a gel sol material with pH 6.8.

[0080] 3) Preparation of mixed precipitate: The prepared mixed solution was slowly added to the colloidal material at 45℃ over 25 minutes to obtain a mixed precipitate with a pH of 8.2. After rolling for 2.5 hours, it was formed into Φ3mm strips using a twin-screw extruder, then dried at 120℃ for 16 hours and calcined at 500℃ for 3 hours to obtain the catalyst precursor. The specific pore volume of this catalyst precursor was 1.27 mL / g, and the macropore volume with a pore size between 10 and 20 nm was 0.66 mL / g, accounting for 52% of the total pore volume. The composition of its components, as determined by X-ray fluorescence spectrometry, was: MoO3-13.01wt%, NiO-3.96wt%, CoO-2.03wt%, Al2O3-79.06wt%, TiO2-1.94wt%.

[0081] 4) Pre-sulfurization operation: Sulfur and dimethyl disulfide in a mass ratio of 1:3 are dissolved in lubricating oil to prepare a sulfurizing agent with a sulfur content of 7%. The above catalyst precursor is placed in a pre-sulfurization reactor, the system is purged with nitrogen and pressurized to 0.8 MPaG, then the sulfurizing agent is introduced, and the system is gradually heated to 260°C at a rate of 30°C / h and maintained for 5 hours. Then, nitrogen is purged and the temperature is lowered to 50°C, and lubricating oil is introduced for passivation, thus obtaining a pre-sulfurized catalyst for use.

[0082] 5) Evaluation Test: Take 20 mL of 10-20 mesh catalyst and pack it into a fixed-bed reactor lined with a quartz tube. The catalyst is placed in the middle of the constant temperature zone of the reactor, supported by quartz sand above and below. The catalyst is not subjected to online sulfidation and is directly subjected to a set temperature of 250℃, atmospheric pressure, and 3000 h. -1 Under airspeed conditions Figure 1 A 100-hour evaluation was conducted on a fixed-bed evaluation device. Initially, the thiophene conversion rate was 99.3%, and the bed pressure dropped to 1.2 kPa. After 100 hours, the thiophene conversion rate was 99.1%, and the bed pressure dropped to 1.2 kPa. The amount of coke deposited on the removed catalyst was 1.8%. Specific catalyst pore distribution results are as follows... Figure 2 As shown.

[0083] Example 2

[0084] Preparation of bifunctional coke oven gas hydrodesulfurization catalyst by mixed precipitation method:

[0085] 1) Preparation of mixed solution: Weigh 23.9g ammonium heptamolybdate tetrahydrate, 23.4g nickel nitrate hexahydrate, and 11.6g ferric nitrate hexahydrate respectively, and prepare a mixed solution with pH 8 at 30℃ using 15wt% ammonia water.

[0086] 2) Preparation of gel sol material: Weigh 182g of boehmite, 6.0g of titanium oxysulfate and 27.0g of carbon black respectively and mix them thoroughly to obtain a mixture. Add 8wt% dilute nitric acid to the mixture and knead for 30min to obtain a gel sol material with pH 4.0.

[0087] 3) Preparation of mixed precipitate: The prepared mixed solution was slowly added to the colloidal material at 45℃ over 25 minutes to obtain a mixed precipitate with a pH of 7.5. After rolling for 2.5 hours, it was formed into Φ3mm strips using a twin-screw extruder, then dried at 120℃ for 16 hours and calcined at 500℃ for 3 hours to obtain the catalyst precursor. The specific pore volume of this catalyst precursor was 1.01mL / g, and the macropore volume with a pore size between 10 and 20nm was 0.47mL / g, accounting for 46.4% of the total pore volume. The composition of its components, as determined by X-ray fluorescence spectrometry, was: MoO3-13.01wt%, NiO-3.96wt%, CoO-2.03wt%, Al2O3-79.06wt%, TiO2-1.94wt%.

[0088] 4) Pre-sulfurization operation: Sulfur and dimethyl disulfide in a mass ratio of 1:3 are dissolved in lubricating oil to prepare a sulfurizing agent with a sulfur content of 7%. The above catalyst precursor is placed in a pre-sulfurization reactor, the system is purged with nitrogen and pressurized to 0.8 MPaG, then the sulfurizing agent is introduced, and the system is gradually heated to 260°C at a rate of 30°C / h and maintained for 5 hours. Then, nitrogen is purged and the temperature is lowered to 50°C, and lubricating oil is introduced for passivation, thus obtaining a pre-sulfurized catalyst for use.

[0089] 5) Evaluation Test: Take 20 mL of 10-20 mesh catalyst and pack it into a fixed-bed reactor lined with a quartz tube. The catalyst is placed in the middle of the constant temperature zone of the reactor, supported by quartz sand above and below. The catalyst is not subjected to online sulfidation and is directly subjected to a set temperature of 250℃, atmospheric pressure, and 3000 h. -1 Under airspeed conditions Figure 1 A 100-hour evaluation was conducted on a fixed-bed evaluation device. Initially, the thiophene conversion rate was 99.0%, and the bed pressure dropped to 1.1 kPa. After 100 hours, the thiophene conversion rate was 96.5%, and the bed pressure dropped to 2.3 kPa. The amount of coke deposited on the removed catalyst was measured to be 3.2%.

[0090] Example 3

[0091] Preparation of bifunctional coke oven gas hydrodesulfurization catalyst by mixed precipitation method:

[0092] 1) Preparation of mixed solution: Weigh 30.7g ammonium heptamolybdate tetrahydrate, 2.7g ammonium metatungstate, 63.3g ferric nitrate nonahydrate, and 38.8g cobalt nitrate hexahydrate respectively, and prepare a mixed solution with pH 11 at 80℃ using 6wt% ammonia water.

[0093] 2) Preparation of gel sol material: Weigh 308g of macroporous pseudoboehmite, 5g of titanium oxysulfate and 43g of carbon black respectively and mix them thoroughly to obtain a mixture. Add 3wt% dilute acetic acid to the mixture and knead for 30min to obtain a gel sol material with pH 8.0.

[0094] 3) Preparation of mixed precipitate: The prepared mixed solution was slowly added to the colloidal material at 45℃ over 25 minutes to obtain a mixed precipitate with a pH of 9.0. After rolling for 2.5 hours, it was formed into Φ3mm strips using a twin-screw extruder, then dried at 120℃ for 16 hours and calcined at 500℃ for 3 hours to obtain the catalyst precursor. The specific pore volume of this catalyst precursor was 1.10 mL / g, and the macropore volume with a pore size between 10 and 20 nm was 0.53 mL / g, accounting for 48.2% of the total pore volume. The composition of its components, as determined by X-ray fluorescence spectrometry, was: MoO3-10.03wt%, WO3-1.01wt%, Fe2O3-4.96%, NiO-5.02wt%, Al2O3-73.92wt%, TiO2-5.06wt%.

[0095] 4) Pre-sulfurization operation: Sulfur and dimethyl disulfide in a mass ratio of 1:3 are dissolved in lubricating oil to prepare a sulfurizing agent with a sulfur content of 7%. The above catalyst precursor is placed in a pre-sulfurization reactor, the system is purged with nitrogen and pressurized to 0.8 MPaG, then the sulfurizing agent is introduced, and the system is gradually heated to 260°C at a rate of 30°C / h and maintained for 5 hours. Then, nitrogen is purged and the temperature is lowered to 50°C, and lubricating oil is introduced for passivation, thus obtaining a pre-sulfurized catalyst for use.

[0096] 5) Evaluation Test: Take 20 mL of 10-20 mesh catalyst and pack it into a fixed-bed reactor lined with a quartz tube. The catalyst is placed in the middle of the constant temperature zone of the reactor, supported by quartz sand above and below. The catalyst is not subjected to online sulfidation and is directly subjected to a set temperature of 250℃, atmospheric pressure, and 3000 h. -1 Under airspeed conditions Figure 1 A 100-hour evaluation was conducted on a fixed-bed evaluation device. Initially, the thiophene conversion rate was 98.9%, and the bed pressure dropped to 1.2 kPa. After 100 hours, the thiophene conversion rate was 97.1%, and the bed pressure dropped to 1.8 kPa. The amount of coke deposited on the removed catalyst was measured to be 2.9%.

[0097] Example 4

[0098] Other operating conditions are basically the same as in Example 1, except that:

[0099] In step 1), the concentration of ammonia solution is selected as 25 wt%.

[0100] In step 3), the volume of macropores with a pore size between 10 and 20 nm is 0.31 mL / g, accounting for 34.7% of the total pore volume. The composition of each component, as determined by X-ray fluorescence spectrometry, is as follows: MoO3-13.00 wt%, NiO-3.95 wt%, CoO-2.03 wt%, Al2O3-79.08 wt%, TiO2-1.94 wt%.

[0101] In step 5), the evaluation test is performed as follows: 20 mL of 10-20 mesh catalyst is packed into a fixed-bed reactor lined with a quartz tube. The catalyst is placed in the middle of the constant-temperature zone of the reactor, supported by quartz sand above and below. The catalyst is not subjected to online sulfidation; it is directly subjected to a set temperature of 250℃, atmospheric pressure, and 3000 h⁻¹. -1 Under airspeed conditions Figure 1 A 100-hour evaluation was conducted on a fixed-bed evaluation device. Initially, the thiophene conversion rate was 99.3%, and the bed pressure dropped to 1.2 kPa. After 100 hours, the thiophene conversion rate was 99.0%, and the bed pressure dropped to 5.6 kPa. The amount of coke deposited on the removed catalyst was measured to be 6.2%.

[0102] Example 5

[0103] Other operating conditions are basically the same as in Example 1, except that:

[0104] The temperature at which the ammonia solution is dissolved in step 1) is 95℃.

[0105] In step 3), the volume of macropores with a pore size between 10 and 20 nm is 0.58 mL / g, accounting for 50.3% of the total pore volume. The composition of each component, as determined by X-ray fluorescence spectrometry, is as follows: MoO3-13.01 wt%, NiO-3.96 wt%, CoO-2.03 wt%, Al2O3-79.06 wt%, TiO2-1.94 wt%.

[0106] In step 5), the evaluation test is performed as follows: 20 mL of 10-20 mesh catalyst is packed into a fixed-bed reactor lined with a quartz tube. The catalyst is placed in the middle of the constant-temperature zone of the reactor, supported by quartz sand above and below. The catalyst is not subjected to online sulfidation; it is directly subjected to a set temperature of 250℃, atmospheric pressure, and 3000 h⁻¹. -1 Under airspeed conditions Figure 1 A 100-hour evaluation was conducted on a fixed-bed evaluation device. Initially, the thiophene conversion rate was 99.2%, and the bed pressure dropped to 1.2 kPa. After 100 hours, the thiophene conversion rate was 98.5%, and the bed pressure dropped to 1.4 kPa. The amount of coke deposited on the removed catalyst was measured to be 2.2%.

[0107] Example 6

[0108] Other operating conditions are basically the same as in Example 1, except that:

[0109] In step 1), the pH of the mixed solution is controlled to be 6.0.

[0110] In step 3), the volume of macropores with a pore size between 10 and 20 nm is 0.63 mL / g, accounting for 51.8% of the total pore volume. The composition of each component, as determined by X-ray fluorescence spectrometry, is as follows: MoO3-13.01 wt%, NiO-3.96 wt%, CoO-2.03 wt%, Al2O3-79.06 wt%, TiO2-1.94 wt%.

[0111] In step 5), the evaluation test is performed as follows: 20 mL of 10-20 mesh catalyst is packed into a fixed-bed reactor lined with a quartz tube. The catalyst is placed in the middle of the constant-temperature zone of the reactor, supported by quartz sand above and below. The catalyst is not subjected to online sulfidation; it is directly subjected to a set temperature of 250℃, atmospheric pressure, and 3000 h⁻¹. -1 Under airspeed conditions Figure 1 A 100-hour evaluation was conducted on a fixed-bed evaluation device. Initially, the thiophene conversion rate was 97.8%, and the bed pressure dropped to 1.2 kPa. After 100 hours, the thiophene conversion rate was 95.4%, and the bed pressure dropped to 3.2 kPa. The amount of coke deposited on the removed catalyst was measured to be 4.5%.

[0112] Example 7

[0113] Other operating conditions are basically the same as in Example 1, except that:

[0114] In step 2), the colloidal material is prepared by adding 3 wt% dilute nitric acid and 10 wt% dilute acetic acid to the mixture. The mass ratio of nitric acid to acetic acid is 4:1 based on the solute.

[0115] In step 3), the volume of macropores with a pore size between 10 and 20 nm is 0.55 mL / g, accounting for 49.6% of the total pore volume. The composition of each component, as determined by X-ray fluorescence spectrometry, is as follows: MoO3-13.01 wt%, NiO-3.96 wt%, CoO-2.03 wt%, Al2O3-79.06 wt%, TiO2-1.94 wt%.

[0116] In step 5), the evaluation test is performed as follows: 20 mL of 10-20 mesh catalyst is packed into a fixed-bed reactor lined with a quartz tube. The catalyst is placed in the middle of the constant-temperature zone of the reactor, supported by quartz sand above and below. The catalyst is not subjected to online sulfidation; it is directly subjected to a set temperature of 250℃, atmospheric pressure, and 3000 h⁻¹. -1 Under airspeed conditions Figure 1A 100-hour evaluation was conducted on a fixed-bed evaluation device. Initially, the thiophene conversion rate was 99.0%, and the bed pressure dropped to 1.2 kPa. After 100 hours, the thiophene conversion rate was 97.5%, and the bed pressure dropped to 1.6 kPa. The amount of coke deposited on the removed catalyst was measured to be 2.6%.

[0117] Example 8

[0118] Other operating conditions are basically the same as in Example 1, except that:

[0119] In step 2), prepare the colloidal material by adding 10wt% dilute acetic acid to the mixture.

[0120] In step 3), the volume of macropores with a pore size between 10 and 20 nm is 0.54 mL / g, accounting for 49.5% of the total pore volume. The composition of each component, as determined by X-ray fluorescence spectrometry, is as follows: MoO3-13.01 wt%, NiO-3.96 wt%, CoO-2.03 wt%, Al2O3-79.06 wt%, TiO2-1.94 wt%.

[0121] In step 5), the evaluation test is performed as follows: 20 mL of 10-20 mesh catalyst is packed into a fixed-bed reactor lined with a quartz tube. The catalyst is placed in the middle of the constant-temperature zone of the reactor, supported by quartz sand above and below. The catalyst is not subjected to online sulfidation; it is directly subjected to a set temperature of 250℃, atmospheric pressure, and 3000 h⁻¹. -1 Under airspeed conditions Figure 1 A 100-hour evaluation was conducted on a fixed-bed evaluation device. Initially, the thiophene conversion rate was 99.2%, and the bed pressure dropped to 1.2 kPa. After 100 hours, the thiophene conversion rate was 89.9%, and the bed pressure dropped to 1.6 kPa. The amount of coke deposited on the removed catalyst was measured to be 2.3%.

[0122] Comparative Example 1

[0123] Preparation of coke oven gas hydrodesulfurization catalyst by wet kneading method:

[0124] Weigh 23.9g of ammonium heptamolybdate tetrahydrate, 23.4g of nickel nitrate hexahydrate, and 11.6g of cobalt nitrate hexahydrate respectively, and prepare a mixed solution with a pH of 10.2 at 56℃ using 13wt% ammonia water.

[0125] Weigh 182g of boehmite, 6.0g of titanium oxysulfate, and 27.0g of carbon black respectively, and mix them thoroughly to obtain a mixture.

[0126] The prepared carrier mixture was added to a mixture containing active metals, rolled at 45°C for 2.5 hours, and then extruded into Φ3mm strips using a twin-screw extruder. The strips were then dried at 120°C for 16 hours and calcined at 500°C for 3 hours to obtain the catalyst precursor. This catalyst precursor had a specific pore volume of 0.70 mL / g, with macropores (10–20 nm) accounting for 0.08 mL / g and representing 11% of the total pore volume. X-ray fluorescence spectroscopy revealed the following composition: MoO3-13.01 wt%, NiO-3.96 wt%, CoO-2.03 wt%, Al2O3-79.06 wt%, and TiO2-1.94 wt%.

[0127] Sulfur and dimethyl disulfide in a mass ratio of 1:3 were dissolved in lubricating oil to prepare a sulfurizing agent with a sulfur content of 7%. The above catalyst precursor was placed in a pre-sulfurization reactor, the system was purged with nitrogen and pressurized to 0.8 MPaG, and then the sulfurizing agent was introduced. The system was gradually heated to 260°C at a rate of 30°C / h and maintained for 5 hours. Then, nitrogen was purged and the temperature was lowered to 50°C. Lubricating oil was introduced for passivation, and the pre-sulfurized catalyst was obtained for use.

[0128] 20 mL of 10–20 mesh catalyst was packed into a fixed-bed reactor lined with a quartz tube. The catalyst was placed in the middle of the isothermal zone of the reactor, supported by quartz sand above and below. The catalyst was not subjected to online sulfidation and was evaluated directly at a set temperature of 250℃, atmospheric pressure, and a space velocity of 3000 h⁻¹ for 100 hours. The initial thiophene conversion rate was measured to be 99.1%, with a bed pressure drop to 1.1 kPa; after 100 hours, the thiophene conversion rate was 91.9%, and the bed pressure drop was 16.3 kPa. The amount of coke deposited on the removed catalyst was measured to be 13.2%.

[0129] Comparative Example 2

[0130] Preparation of coke oven gas hydrodesulfurization catalyst by impregnation method:

[0131] Weigh 23.9g of ammonium heptamolybdate tetrahydrate, 23.4g of nickel nitrate hexahydrate, and 11.6g of cobalt nitrate hexahydrate respectively, and prepare a mixed solution with a pH of 10.2 at 56℃ using 13wt% ammonia water.

[0132] 182g of boehmite, 6.0g of titanium oxysulfate, and 27.0g of carbon black were weighed and thoroughly mixed to obtain a mixture. 142g of 3wt% dilute nitric acid was added to the mixture, and after rolling at 45℃ for 2.5 hours, it was formed into Φ3mm strips using a twin-screw extruder. The strips were then dried at 120℃ for 16 hours and calcined at 500℃ for 3 hours to obtain 110g of titanium-aluminum carrier for later use.

[0133] The catalyst was prepared by impregnating the titanium-aluminum support twice. The single impregnation method was as follows: the prepared titanium-aluminum support was impregnated in the prepared mixture, heated to 50°C and held for 1 hour, the support was removed and dried at 120°C for 16 hours, and then calcined at 500°C for 3 hours.

[0134] The catalyst has a specific pore volume of 0.58 mL / g, and the volume of macropores with a pore size between 10 and 20 nm is 0.10 mL / g, accounting for 17% of the total pore volume. According to X-ray fluorescence spectroscopy, its composition is as follows: MoO3-13.01wt%, NiO-3.96wt%, CoO-2.03wt%, Al2O3-79.06wt%, TiO2-1.94wt%.

[0135] Take 20 mL of 10-20 mesh catalyst and pack it into a fixed-bed reactor lined with a quartz tube. The catalyst is placed in the middle of the reactor's isothermal zone, supported by quartz sand above and below. The catalyst is then subjected to online sulfidation under the following conditions: H₂S:H₂:N₂ ratio in the sulfiding agent = 1:5:96, sulfidation temperature 350℃, and sulfidation time 6 hours. After sulfidation, the system is cooled to 250℃.

[0136] An evaluation was conducted at atmospheric pressure and a space velocity of 3000 h⁻¹ for 100 hours. The initial thiophene conversion rate was 99.3%, and the bed pressure dropped to 1.2 kPa. After 100 hours, the thiophene conversion rate was 90.1%, and the bed pressure dropped to 19.6 kPa. The amount of coke deposited on the removed catalyst was 14.7%.

[0137] Experimental Example 1

[0138] The performance test results of the hydrodesulfurization catalysts prepared in the above embodiments and comparative examples are summarized in Table 1 below:

[0139] Table 1 Catalyst performance results

[0140]

[0141] As can be seen from the catalyst performance in Table 1 above, compared with the traditional wet mixing and impregnation methods, the hydrodesulfurization catalyst of this invention has a larger specific pore volume, and most of them are macropores of 10-20 nm, which is beneficial to the mass transfer and conversion of organic sulfur in coke oven gas. It also has a greater capacity for adsorption, containment and conversion of large molecular organic matter such as tar in coke oven gas. The catalyst surface is not prone to carbon buildup, the reactor pressure drop is smaller, and the service life is longer.

[0142] The hydrodesulfurization catalyst of this invention is prepared by a mixed precipitation method. In the mixed solution step, appropriate ammonia concentration, dissolution temperature, and solution pH value are conducive to the stable dissolution and dispersion of the active metal components and the formation of macropores. In the preparation of the colloidal material step, appropriate pH conditions can obtain good colloidal solubility of the support material to facilitate the formation of new pore structures without destroying the original pore structure of the support. Furthermore, the addition of a specific ratio of acetic acid can make the active components more uniformly dispersed. By controlling the dissolution parameters of the mixed solution and the parameters for preparing the colloidal material, the pH of the mixed precipitation step can be controlled within an optimal range of 7.5 to 8.5, ultimately forming a uniformly dispersed active component and generating a new pore structure, thus achieving the good effect of good catalyst activity and resistance to carbon deposition.

[0143] Finally, it is understood that the above embodiments are merely exemplary embodiments used to illustrate the principles of the present invention, and the present invention is not limited thereto. For those skilled in the art, various modifications and improvements can be made without departing from the principles and essence of the present invention, and these modifications and improvements are also considered to be within the scope of protection of the present invention.

Claims

1. The use of a bifunctional coke oven gas hydrodesulfurization catalyst for the production of purified synthesis gas by hydrodesulfurization, characterized in that, The preparation method of the bifunctional coke oven gas hydrodesulfurization catalyst includes the following steps: The active component precursor is dissolved in ammonia to form a mixed solution, the pH of which is controlled between 8.0 and 11.

0. The carrier raw material is then kneaded with the acid solution to form a colloidal material. The mixed solution is added to the colloidal material and mixed to precipitate. After mixing and precipitation, the pH is measured to be 7.0-9.

0. The mixture is then kneaded or rolled into a plastic body, and then processed, shaped, dried, calcined, and pre-vulcanized to produce a catalyst. The concentration of the ammonia solution is 6-15 wt%, and the temperature at which the ammonia solution is dissolved is controlled between 40-65°C. The active component precursor includes at least one of nickel nitrate, ferric nitrate, cobalt nitrate, ammonium heptamolybdate, and ammonium metatungstate; the carrier raw material is at least one of alumina precursor, titanium dioxide precursor, and silicon dioxide precursor, as well as a pore expander and a binder.

2. The application according to claim 1, characterized in that, The pH of the mixed solution is controlled between 8.5 and 10.

5.

3. The application according to claim 1, characterized in that, The pH of the colloidal material is controlled between 4.0 and 8.

0.

4. The application according to claim 1, characterized in that, The pH of the colloidal material is controlled between 5.0 and 7.

5.

5. The application according to claim 1, characterized in that... The acid solution is one or a mixture of two of the following: nitric acid and acetic acid.

6. The application according to claim 1, characterized in that, The acid solution is a mixture of nitric acid and acetic acid solutions, wherein the concentration of the nitric acid is 1-8 wt% and the concentration of the acetic acid is 3-15 wt%.

7. The application according to claim 6, characterized in that, The concentration of nitric acid is 2 wt% to 5 wt%; the concentration of acetic acid is 5 wt% to 10 wt%.

8. The application according to claim 6, characterized in that, Based on the solute, the mass ratio of nitric acid to acetic acid is (1-2):

1.

9. The application according to claim 1, characterized in that, After mixing and precipitation, the pH value was measured to be 7.5–8.5.

Citation Information

Patent Citations

  • A magnesium-based coke oven gas hydrodesulfurization catalyst and its preparation method

    CN112354568B

  • Coke oven gas hydrodesulfurization catalyst, its preparation method and application

    CN112742362B

  • Coke oven gas hydrodesulfurization catalyst and preparation method thereof

    CN114433112A

  • Low-loading-quantity coke oven gas hydrogen desulfurization catalyst as well as preparation method and application thereof

    CN108855116A

  • Residual oil hydrodesulfurization catalyst and preparation method thereof

    CN117138795A