A rhombohedral SnSb2Te4 nanomaterial and its preparation method and application
Preparing rhombohedral SnSb2Te4 nanomaterials through a solvothermal method solves the problems of high energy consumption and uncontrollable product size in the existing technology, and achieves the preparation of nanomaterials with uniform morphology and controllable size, and has excellent degradation of environmental pollutants. capabilities for multifunctional material applications.
Patent Information
- Application Number
- CN202410483119.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-22
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-04-22
AI Technical Summary
The synthesis method of SnSb2Te4 nanomaterials in the existing technology has high energy consumption, long time, uncontrollable product size and uneven morphology, making it difficult to achieve macro-scale preparation and micro-nano integrated applications.
The solvothermal method is used to prepare the rhombohedral phase SnSb2Te4 nanomaterial by dissolving the tellurium source in the solvent, mixing the tin source and the antimony source, and performing a heating reaction. The reaction conditions are mild, the process is simple, the cost is low, and the morphology is uniform and the size is obtained. Controllable nanomaterials.
The rhombohedral phase SnSb2Te4 nanomaterial has achieved high crystallinity and morphological size control, has excellent environmental pollutant degradation capabilities, and is suitable for fields such as catalysis, photoelectricity, and thermoelectric conversion.
Smart Images

Figure CN118183636B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of nano material preparation, and in particular relates to a rhombohedral SnSb2Te4 nano material and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background section is intended to enhance understanding of the overall background of the invention and should not necessarily be regarded as an admission or any form of suggestion that this information constitutes the prior art already known to those skilled in the art.
[0003] Achieving green and sustainable development of energy and the environment is a major strategic goal for human society. Nanomaterials, due to their unique structural advantages, have broad research and application prospects in fields such as clean energy development, environmental pollution purification, and biomedicine.
[0004] Ternary SnSb2Te4 nanomaterials are multifunctional materials with potential applications in thermoelectrics, optoelectronics, catalysis, and other research fields. The development of their synthesis methods and the exploration of their structure-property relationships are hot topics in current scientific research and have attracted widespread attention. Currently, most reported methods for synthesizing SnSb2Te4 nanomaterials rely on high-temperature solid-phase methods. For example, using a high-temperature solid-phase reaction, the elements Sn, Sb, and Te are first loaded into a quartz tube. The tube is then heated to 950°C under argon for 93 hours, and finally annealed at 400-450°C for two days to obtain bulk SnSb2Te4. However, this solid-phase synthesis method is not only energy-intensive and time-consuming, but also suffers from uncontrollable product size and heterogeneous morphology, making it unsuitable for large-scale preparation and micro-nanointegrated applications of SnSb2Te4 nanomaterials. Summary of the Invention
[0005] In view of the shortcomings of the prior art, the first object of the present invention is to provide a method for preparing rhombohedral SnSb2Te4 nanomaterials, which has the advantages of simple process, low cost, mild reaction conditions and significantly reduced energy consumption.
[0006] The second object of the present invention is to provide a rhombohedral SnSb2Te4 nanomaterial prepared by the above method, wherein the rhombohedral SnSb2Te4 nanomaterial has the advantages of uniform morphology, controllable size and high crystallinity.
[0007] The third object of the present invention is to provide an application of the above-mentioned rhombohedral SnSb2Te4 nanomaterial. The rhombohedral SnSb2Te4 nanomaterial has a strong absorption capacity in the visible-near infrared light range and exhibits excellent environmental pollutant degradation ability. It can be used as a new multifunctional material in research fields such as catalysis, photoelectricity, and thermoelectric conversion.
[0008] To achieve the above object, the present invention adopts the following technical solutions:
[0009] A method for preparing a rhombohedral SnSb2Te4 nanomaterial, the preparation method comprising the following steps:
[0010] (1) Dissolve the tellurium (Te) source in a solvent to obtain solution A (such as Te-TOP);
[0011] (2) Mix the tin source, the antimony source, the solution A obtained in step (1) and the solvent, heat them, and separate them to obtain the rhombohedral SnSb2Te4 nanomaterial.
[0012] Furthermore, in step (1), the tellurium source is at least one of tellurium powder, tellurium dioxide or biphenyl ditellurium.
[0013] Furthermore, in step (1), the solvent is tri-n-octylphosphine (TOP), n-dodecyl mercaptan or oleylamine.
[0014] Furthermore, in step (1), the ratio of the tellurium source to the solvent is 1 mmol: (1-2) mL.
[0015] Furthermore, in step (1), the tellurium source is dissolved in a solvent under an inert atmosphere; the tellurium source is dissolved in a solvent under heating and stirring conditions.
[0016] Furthermore, the inert atmosphere is nitrogen or argon.
[0017] Furthermore, the heating temperature is 210-250° C. and the heating time is 60-180 min.
[0018] Furthermore, in step (2), the tin source is at least one of tin iodide, tin acetylacetonate, tin bromide, tin acetate, tin oxalate and tin acetate.
[0019] Furthermore, in step (2), the antimony source is at least one of triphenylantimony, antimony acetate, antimony bromide, antimony chloride and antimony iodide.
[0020] Furthermore, in step (2), the solvent is a high boiling point reaction medium.
[0021] Furthermore, the solvent is at least one of organic amine, oleic acid and octadecene.
[0022] Furthermore, the organic amine is at least one of oleylamine, octadecylamine and hexadecylamine.
[0023] The ratio of the tin source to the solvent is 0.1 mmol: (5.0-10.0) mL.
[0024] Furthermore, in step (2), the heating reaction adopts the following steps: firstly performing a first stirring heating under an inert atmosphere, and then performing a second heating.
[0025] Furthermore, the inert atmosphere is nitrogen or argon, etc.; the temperature of the first stirring and heating is 110-180°C, and the duration is 30-60 minutes. The purpose of the first stirring and heating is to dissolve the tin source, antimony source, and tellurium source, and to remove oxygen, moisture, and low-boiling-point impurities in the reaction system.
[0026] Furthermore, the second heating temperature is 260-340° C., and the time is 10-180 min.
[0027] Furthermore, in step (2), washing and separation are required after the heating to obtain the rhombohedral SnSb2Te4 nanomaterial.
[0028] Furthermore, the solvents used for the washing are anhydrous ethanol and cyclohexane.
[0029] Furthermore, the separation method is centrifugation or filtration.
[0030] Furthermore, the molar ratio of the tin element in the tin source in step (2), the antimony element in the antimony source and the tellurium element in the tellurium source in step (1) is 1:2:(4-8).
[0031] The SnSb2Te4 nanomaterial prepared by the above method has a crystal form of rhombohedral phase and a microscopic morphology of a nanoscale polygonal sheet structure.
[0032] Furthermore, the side length of the SnSb2Te4 nanomaterial is approximately 100-350 nm, and the thickness is approximately 10-30 nm.
[0033] Application of the above SnSb2Te4 nanomaterials in optoelectronics, thermoelectricity or catalysis and other fields.
[0034] Compared to SnSb2Te4 synthesized by traditional solid-phase reaction methods, the two-dimensional rhombohedral SnSb2Te4 nanomaterial synthesized in the present invention is easily micro-nanofabricated into films on device substrates. Furthermore, the two-dimensional rhombohedral SnSb2Te4 nanosheets have the advantage of high crystallinity, which facilitates the effective separation and transport of photogenerated electrons and holes, improving photocatalytic or photoelectric conversion performance. The two-dimensional rhombohedral SnSb2Te4 nanomaterial synthesized in the present invention also has good solvent dispersibility and strong absorption capacity in the visible-near-infrared range, demonstrating excellent photocatalytic ability.
[0035] Beneficial effects: (1) The rhombohedral SnSb2Te4 nanomaterials prepared by the method provided by the present invention have a hexagonal and / or polygonal sheet structure morphology, high crystallinity, and controllable morphology and size. The unique structure enables the SnSb2Te4 nanomaterials to have excellent absorption capacity in the visible-near infrared range, and the SnSb2Te4 nanomaterials show excellent environmental pollutant degradation ability, and can be used as a new multifunctional material in research fields such as catalysis, photoelectricity, and thermoelectric conversion.
[0036] (2) The method for preparing two-dimensional rhombohedral SnSb2Te4 nanomaterials provided by the present invention has the advantages of simple process, low cost, mild reaction conditions and significantly reduced energy consumption. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] The accompanying drawings, which constitute part of the present invention, are provided to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are provided to explain the present invention and do not constitute undue limitations thereon. The embodiments of the present invention will be described in detail below with reference to the accompanying drawings, wherein:
[0038] Figure 1 is the XRD pattern of the SnSb2Te4 nanomaterial prepared in Example 1;
[0039] Figure 2 is a SEM image of the SnSb2Te4 nanomaterial prepared in Example 1;
[0040] Figure 3 HRTEM and ED images of the SnSb2Te4 nanomaterial prepared in Example 1;
[0041] Figure 4 is the XRD pattern of the SnSb2Te4 nanomaterial prepared in Example 2;
[0042] Figure 5 is a SEM image of the SnSb2Te4 nanomaterial prepared in Example 3;
[0043] Figure 6 is a SEM image of the SnSb2Te4 nanomaterial prepared in Example 4;
[0044] Figure 7 is the UV-visible-near-infrared absorption spectrum of the SnSb2Te4 nanomaterial prepared in Example 1;
[0045] Figure 8 This is a curve diagram of the photocatalytic degradation of methylene blue by the SnSb2Te4 nanomaterial prepared in Example 1. Specific embodiments
[0047] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended to illustrate the present invention only and are not intended to limit the scope of the invention. The experimental methods in the following examples, for which specific conditions are not specified, are generally performed under conventional conditions or as recommended by the manufacturer.
[0048] Unless otherwise defined, all professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar to or equivalent to the described content can be applied to the method of the present invention. The preferred implementation methods and materials described in the present invention are for demonstration purposes only. The present invention is further described with reference to the accompanying drawings and specific examples.
[0049] Example 1
[0050] Preparation of a two-dimensional rhombohedral SnSb2Te4 nanomaterial, comprising the following steps:
[0051] (1) In a 100 mL three-necked flask A, add 10 mmol of tellurium powder and 10 mL of tri-n-octylphosphine, then introduce nitrogen and heat to 250 °C under magnetic stirring for 180 min to dissolve the tellurium powder in the tri-n-octylphosphine. Cool to room temperature to obtain a mixed solution.
[0052] (2) In a 100 mL three-necked flask B, 0.1 mmol of tin iodide, 0.2 mmol of triphenylantimony, 0.4 mmol of the mixed solution obtained in step (1) and 8.0 mL of oleylamine were added respectively, and then nitrogen was introduced. The mixture was heated to 130°C under stirring for 60 min to remove oxygen, moisture and low-boiling impurities in the reaction system. The three-necked flask B was then rapidly heated to 300°C and kept warm for 90 min. After the reaction was completed, it was cooled to room temperature, and the product was washed with anhydrous ethanol and cyclohexane 3 times, and centrifuged to obtain a two-dimensional rhombohedral SnSb2Te4 nanomaterial.
[0053] Figure 1 This is the X-ray diffraction (XRD) pattern of the SnSb2Te4 nanomaterial prepared in Example 1. The results show that all diffraction peaks of the SnSb2Te4 nanomaterial can be indexed to the corresponding crystal planes in SnSb2Te4 (JCPDS Card No. 89-1931), and no other impurity peaks appear, proving that the product prepared in Example 1 is a rhombohedral SnSb2Te4 crystal.
[0054] Figure 2This is a scanning electron microscope (SEM) image of the SnSb2Te4 nanomaterial prepared in Example 1. The results show that the SnSb2Te4 nanomaterial prepared in Example 1 is in the form of hexagonal and / or polygonal flakes with a side length of about 100-350 nm and a thickness of about 10-30 nm. The SnSb2Te4 nanomaterial prepared in Example 1 has the characteristics of uniform and controllable size.
[0055] Figure 3 These are the high-resolution transmission electron microscopy (HRTEM) image and electron diffraction (ED) image of the SnSb2Te4 nanomaterial prepared in Example 1. The results show that the SnSb2Te4 nanomaterial prepared in Example 1 has good crystallinity.
[0056] Example 2
[0057] Preparation of a two-dimensional rhombohedral SnSb2Te4 nanomaterial, comprising the following steps:
[0058] (1) In a 100 mL three-necked flask A, add 10 mmol of tellurium powder and 10 mL of tri-n-octylphosphine, then introduce nitrogen and heat to 250 °C under magnetic stirring for 180 min to dissolve the tellurium powder in the tri-n-octylphosphine. Cool to room temperature to obtain a mixed solution.
[0059] (2) In a 100 mL three-necked flask B, 0.1 mmol of tin iodide, 0.2 mmol of triphenylantimony, 0.4 mmol of the mixed solution obtained in step (1) and 8.0 mL of oleylamine were added respectively, and then nitrogen was introduced. The mixture was heated to 130°C under stirring for 60 min to remove oxygen, moisture and low-boiling impurities in the reaction system. The three-necked flask B was then rapidly heated to 280°C and kept warm for 120 min. After the reaction was completed, it was cooled to room temperature, and the product was washed with anhydrous ethanol and cyclohexane 3 times, and then centrifuged to obtain a two-dimensional rhombohedral SnSb2Te4 nanomaterial.
[0060] Figure 4 This is the XRD pattern of the SnSb2Te4 nanomaterial prepared in Example 2. The results show that all diffraction peaks of the SnSb2Te4 nanomaterial can be indexed to the corresponding crystal planes in SnSb2Te4 (JCPDS Card No. 89-1931), and no other impurity peaks appear, proving that the product prepared in Example 2 is a rhombohedral SnSb2Te4 crystal.
[0061] Example 3
[0062] Preparation of a two-dimensional rhombohedral SnSb2Te4 nanomaterial, comprising the following steps:
[0063] (1) In a 100 mL three-necked flask A, add 10 mmol of tellurium powder and 10 mL of tri-n-octylphosphine, then introduce nitrogen and heat to 250 °C under magnetic stirring for 180 min to dissolve the tellurium powder in the tri-n-octylphosphine. Cool to room temperature to obtain a mixed solution.
[0064] (2) In a 100 mL three-necked flask B, 0.1 mmol of tin iodide, 0.2 mmol of triphenylantimony, 0.4 mmol of the mixed solution obtained in step (1) and 8.0 mL of oleylamine were added respectively, and then nitrogen was introduced. The mixture was heated to 150°C under stirring for 30 min to remove oxygen, moisture and low-boiling impurities in the reaction system. The three-necked flask B was then rapidly heated to 340°C and kept warm for 30 min. After the reaction was completed, it was cooled to room temperature, and the product was washed with anhydrous ethanol and cyclohexane 3 times, and then centrifuged to obtain a two-dimensional rhombohedral SnSb2Te4 nanomaterial.
[0065] Figure 5 This is an SEM image of the SnSb2Te4 nanomaterial prepared in Example 3. The results show that the SnSb2Te4 nanomaterial prepared in Example 3 is in the form of hexagonal and / or polygonal flakes with a side length of approximately 100-350 nm and a thickness of approximately 10-30 nm. The SnSb2Te4 nanomaterial prepared in Example 3 has the characteristics of uniform and controllable size.
[0066] Example 4
[0067] Preparation of a two-dimensional rhombohedral SnSb2Te4 nanomaterial, comprising the following steps:
[0068] (1) In a 100 mL three-necked flask A, add 10 mmol of tellurium powder and 10 mL of tri-n-octylphosphine, then introduce nitrogen and heat to 250 °C under magnetic stirring for 180 min to dissolve the tellurium powder in the tri-n-octylphosphine. Cool to room temperature to obtain a mixed solution.
[0069] (2) In a 100 mL three-necked flask B, 0.1 mmol of tin iodide, 0.2 mmol of antimony iodide, 0.4 mmol of the mixed solution obtained in step (1) and 8.0 mL of oleylamine were added respectively, and then nitrogen was introduced. The mixture was heated to 150°C with stirring for 30 min to remove oxygen, moisture and low-boiling impurities in the reaction system. The three-necked flask B was then rapidly heated to 300°C and kept warm for 120 min. After the reaction was completed, it was cooled to room temperature, and the product was washed with anhydrous ethanol and cyclohexane 3 times, and then centrifuged to obtain a two-dimensional rhombohedral SnSb2Te4 nanomaterial.
[0070] Figure 6This is an SEM image of the SnSb2Te4 nanomaterial prepared in Example 4. The results show that the SnSb2Te4 nanomaterial prepared in Example 4 is a polygonal sheet structure with a side length of approximately 100-350 nm and a thickness of approximately 10-30 nm. The SnSb2Te4 nanomaterial prepared in Example 4 has the characteristics of uniform and controllable size.
[0071] Performance Testing
[0072] 1. Determination of UV-visible-near-infrared (UV-vis-NIR) light absorption properties
[0073] Figure 7 This is the ultraviolet-visible-near-infrared light absorption (UV-vis-NIR) spectrum of the SnSb2Te4 nanomaterial prepared in Example 1. The results show that the SnSb2Te4 nanomaterial prepared in Example 1 has strong absorption in the ultraviolet-visible light range, indicating that the SnSb2Te4 nanomaterial prepared in Example 1 can be used as a solar energy conversion material in the field of photocatalysis research.
[0074] 2. Photocatalytic degradation of methylene blue performance determination
[0075] Before photocatalytic degradation of methylene blue, the SnSb2Te4 nanomaterial was first surface-modified to improve the water solubility of the material; the SnSb2Te4 nanomaterial synthesized in Example 1, 2.0 mL of thioglycolic acid, 3 mL of toluene, and 3 mL of anhydrous ethanol were transferred to a 10 mL test tube and ultrasonically dispersed for 30 minutes, and then allowed to stand for 12 hours; then, the solid product was centrifuged and washed three times with anhydrous ethanol to obtain the target product; 50 mg of the target product was weighed and dispersed in 50 mL of a 10 mg / L methylene blue aqueous solution, and stirred in the dark for 30 minutes to reach adsorption / desorption equilibrium; the catalytic reaction device was irradiated with a 300 W xenon lamp under circulating water cooling conditions, and 0.5 mL of the mixed solution was aspirated with a pipette every 10 minutes for centrifugation. The supernatant was taken and its absorbance was measured using a UV-visible spectrophotometer to calculate the degradation rate.
[0076] The blank group was xenon lamp irradiation without SnSb2Te4 nanomaterials and directly irradiated methylene blue.
[0077] Figure 8 This graph shows the photocatalytic degradation of methylene blue by the surface-modified SnSb2Te4 nanomaterial prepared in Example 1. The results show that after 1.0 h of xenon lamp irradiation, the SnSb2Te4 nanomaterial achieved a 75% degradation rate of methylene blue, compared to only 11% in a blank experiment. These experimental results demonstrate the excellent photocatalytic degradation capabilities of the SnSb2Te4 nanomaterial.
[0078] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art will be able to modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein with equivalents. Any modifications, equivalent replacements, improvements, etc. made within the spirit and principles of the present invention shall be included within the scope of protection of the present invention.
Claims
1. A method for preparing a rhombohedral SnSb2Te4 nanomaterial, characterized in that: The crystal form of the SnSb2Te4 nanomaterial is a rhombohedral phase; the SnSb2Te4 nanomaterial is a polygonal sheet structure; the side length of the SnSb2Te4 nanomaterial is 100-350 nm, and the thickness is 10-30 nm; The preparation method comprises the following steps: (1) dissolving a tellurium source in a solvent to obtain a solution A; (2) mixing the tin source, the antimony source, the solution A obtained in step (1) and the solvent, heating them, and separating them to obtain the rhombohedral SnSb2Te4 nanomaterial; In step (2), the antimony source is at least one of triphenylantimony, antimony acetate, antimony bromide, antimony chloride and antimony iodide; The molar ratio of the tin element in the tin source in step (2), the antimony element in the antimony source and the tellurium element in the tellurium source in step (1) is 1:2:(4-8); In step (2), the heating reaction adopts the following steps: first, heating with stirring at 110-180°C for 30-60 min; then heating at 260-340°C for 10-180 min.
2. The preparation method according to claim 1, characterized in that: In step (1), the tellurium source is at least one of tellurium powder, tellurium dioxide and biphenyl ditellurium; The solvent is tri-n-octylphosphine, n-dodecyl mercaptan or oleylamine; The dissolution is carried out under an inert atmosphere, the temperature required for the dissolution is 210-250° C., and the time is 60-180 min.
3. The preparation method according to claim 2, characterized in that: The ratio of the tellurium source to the solvent is 1 mmol: (1-2) mL.
4. The preparation method according to claim 2, characterized in that: The inert atmosphere is nitrogen or argon.
5. The preparation method according to claim 1, characterized in that: In step (2), the tin source is at least one of tin iodide, tin acetylacetonate, tin bromide, tin acetate, tin oxalate and tin acetate; The solvent is at least one of oleylamine, octadecylamine, hexadecylamine, oleic acid and octadecene.
6. The preparation method according to claim 1, characterized in that: In step (2), the heating reaction is carried out under an inert atmosphere.
7. The preparation method according to claim 6, characterized in that: The inert atmosphere is nitrogen or argon; After the heating, washing and separation are required to obtain the rhombohedral SnSb2Te4 nanomaterial.
8. SnSb2Te4 nanomaterial prepared by the method described in any one of claims 1 to 7.
9. The use of the SnSb2Te4 nanomaterial according to claim 8, characterized in that: The SnSb2Te4 nanomaterial is used in the fields of catalysis, photoelectricity or thermoelectricity.
Citation Information
Patent Citations
Liquid-phase preparation method of cubic phase Cu2SnTe3 nanometer crystal
CN105174235A
Liquid-phase preparation method for tetragonal two-dimensional CuFeSe2 nanosheet crystal
CN109019532A
Two-dimensional non-layered CuGaSe2 porous nanomaterial as well as preparation method and application thereof
CN113683060A
Rhombic phase CuCrSe2 nano material as well as preparation method and application thereof
CN113697777A
Thermoelectric semiconductor material and manufacture thereof
JP2000106460A