A hard carbon negative electrode material, preparation method thereof and battery
By pre-carbonizing, activating, and double-coating peony shell material, a core-shell structured hard carbon anode material is formed, which solves the problems of low initial efficiency, low specific capacity, and poor rate performance of hard carbon materials in sodium-ion batteries, and achieves high specific capacity, high initial efficiency, and good cycle stability.
Patent Information
- Application Number
- CN202410324416.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-20
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-03-20
AI Technical Summary
Existing hard carbon materials used as anode materials for sodium-ion batteries suffer from problems such as low initial efficiency, low specific capacity, poor rate performance, and rapid degradation during low-temperature cycling.
Using peony shells as raw material, after pre-carbonization, activation, and high-temperature carbonization, a double-layer coating of asphalt and alumina is applied to form a core-shell structured hard carbon anode material.
It improves the material's initial efficiency, specific capacity, and rate performance, enhances cycle stability, and improves the overall performance of the battery.
Smart Images

Figure CN118183696B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a hard carbon negative electrode material, a preparation method thereof, and a battery. Background Art
[0002] With the rapid development of economy, the dependence on energy is increasing. Traditional fossil energy is a non-renewable energy and is becoming increasingly exhausted. The environmental pollution problems it brings cannot be underestimated. As one of the important development directions in the field of new energy, sodium-ion batteries have made breakthrough progress recently, and the positive and negative electrode materials, electrolytes, etc. they contain have also become a hot topic in the field of sodium batteries.
[0003] Currently, most of the negative electrode materials for commercial sodium-ion batteries are hard carbon materials. Hard carbon materials are a structure in which local microcrystals and cross-links coexist. Compared with soft carbon, they are difficult to graphitize at 2500°C. Existing hard carbon materials have many local defects, which cause some irreversible adsorption of sodium ions. They have a large specific surface area, and consume more sodium ions to form the SEI membrane surface during the first charge and discharge, thereby reducing the initial efficiency of the battery. Existing hard carbon materials have poor sodium ion diffusion kinetics, which is reflected in the poor rate, especially high current charging, which is easy to cause sodium precipitation and capacity decay, and the low-temperature cycle decay is faster. Summary of the invention
[0004] The invention discloses a hard carbon negative electrode material, a preparation method thereof and a battery, so as to solve the problems of low first efficiency, low gram capacity, poor rate performance and fast low-temperature cycle attenuation of batteries formed by existing materials.
[0005] In order to achieve the above purpose, the embodiments of this specification adopt the following technical solutions:
[0006] In a first aspect, a method for preparing a hard carbon negative electrode material is provided, comprising the following steps:
[0007] Taking peony shell and heating it to obtain a pre-carbonized product, and then mixing the pre-carbonized product with a potassium source to obtain an activated precursor;
[0008] Carbonizing the activated precursor to obtain a peony shell carbonized material;
[0009] The peony shell carbonized material is coated with asphalt and subjected to a heating treatment to obtain an asphalt-coated peony shell carbon material;
[0010] The asphalt-coated peony shell carbon material is mixed with aluminum nitrate or aluminum isopropoxide and heated to obtain a hard carbon negative electrode material.
[0011] Optionally, in the step of heating the peony shell to obtain the pre-carbonized product, the heating temperature is 250-400° C.; and / or,
[0012] The heating duration is 2 to 3 hours.
[0013] Optionally, the mass ratio of the pre-carbonized material to the potassium source is (0.5-3):1.
[0014] Optionally, the step of mixing the pre-carbonized material with the potassium source is performed under heating.
[0015] Optionally, in the step of carbonizing the activated precursor to obtain a peony shell carbonized material, the carbonization temperature is 900-1500°C; and / or the duration of the carbonization is 2-5h; and / or the heating rate is 1-5°C / min.
[0016] Optionally, in the step of coating the peony shell carbonized material with asphalt and heating it to obtain the asphalt-coated peony shell carbon material, the mass ratio of the peony shell carbonized material to the asphalt is 8:(1-3); and / or,
[0017] The coating of the peony shell carbonized material with asphalt is achieved by kneading with a kneader; and / or,
[0018] The stirring speed during coating is 200 to 600 r / min; and / or,
[0019] The temperature during coating is 150-250°C.
[0020] Optionally, in the step of coating the peony shell carbonized material with asphalt and heating it to obtain the asphalt-coated peony shell carbon material, the heating temperature is 200-800° C.; and / or,
[0021] The duration of the heating treatment is 1 to 3 hours.
[0022] Optionally, the mass ratio of the asphalt-coated peony shell carbon material to the aluminum nitrate or aluminum isopropoxide is 1:(0.005-0.05); and / or, in the step of mixing and heating the asphalt-coated peony shell carbon material with aluminum nitrate or aluminum isopropoxide, the heating temperature is 400-850°C; and / or, the heating duration is 1-3h.
[0023] In a second aspect, a hard carbon negative electrode material is provided, which is prepared by the preparation method described in any one of the first aspects.
[0024] In a third aspect, a battery is provided, wherein the battery comprises the hard carbon negative electrode material prepared by any preparation method described in the first aspect or the hard carbon negative electrode material described in the second aspect.
[0025] At least one of the above technical solutions adopted in the embodiments of the present application can achieve the following beneficial effects:
[0026] The hard carbon negative electrode material, preparation method and battery of the present invention, the peony shell carbon material used has the characteristics of self-doping to improve the active points, and has a higher capacity after pre-carbonization, activation and high-temperature carbonization. The asphalt coating layer improves the ion diffusion performance of the material, and the alumina coating layer reduces the exposure of surface defects of the material and improves the first efficiency of the material, so that the obtained battery has the characteristics of high gram capacity, good rate performance, high first efficiency and good cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0028] Figure 1 This is a scanning electron microscope image of the hard carbon negative electrode material obtained according to Example 1 of the present invention. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the present application clearer, the technical solution of the present application will be clearly and completely described below in combination with the specific embodiments of the present application and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present application.
[0030] According to one embodiment of the present application, a method for preparing a hard carbon negative electrode material is provided, comprising the following steps:
[0031] Taking peony shell and heating it to obtain a pre-carbonized product, and then mixing the pre-carbonized product with a potassium source to obtain an activated precursor;
[0032] Carbonizing the activated precursor to obtain a peony shell carbonized material;
[0033] The peony shell carbonized material is coated with asphalt and subjected to a heating treatment to obtain an asphalt-coated peony shell carbon material;
[0034] The asphalt-coated peony shell carbon material is mixed with aluminum nitrate or aluminum isopropoxide and heated to obtain a hard carbon negative electrode material.
[0035] In the embodiment of the present specification, the step of heating the peony shell to obtain the pre-carbonized product also includes crushing the peony shell and then heating it. The crushing method of the peony shell is not limited by the present invention. Optionally, the peony shell is crushed mechanically. The step of heating the peony shell to obtain the pre-carbonized product also includes crushing the peony shell and then screening the peony shell with a mesh size of less than or equal to 50. The screening method of the peony shell is not limited by the present invention. Optionally, the peony shell is screened with a 50-mesh screen.
[0036] In the embodiments of this specification, the temperature and time of the peony shell heating treatment are not limited by the present invention, as long as the effect of obtaining the pre-carbonized product required by the present invention can be achieved. Optionally, the temperature of the peony shell heating treatment is 250-400°C. Preferably, the temperature of the peony shell heating treatment is 250°C, 260°C, 270°C, 280°C, 290°C, 300°C, 310°C, 320°C, 340°C, 350°C, 360°C, 370°C, 380°C, 390°C, 400°C or any value therebetween. Optionally, the duration of the peony shell heating treatment is 2-3h. Preferably, the duration of the peony shell heating treatment is 2h, 2.5h, 3h or any value therebetween. The peony shell heating treatment is carried out in a tubular furnace. The peony shell heating treatment is carried out in an inert atmosphere.
[0037] In the embodiments of this specification, the type of the potassium source is not limited by the present invention. Optionally, the potassium source is potassium salt, and more preferably, the potassium source is a combination of one or more of potassium hydroxide KOH, potassium carbonate, potassium chloride, potassium nitrate, potassium hydroxide, and potassium bicarbonate. When the potassium source is potassium hydroxide, the pre-carbonized material is mixed with a potassium hydroxide solution, and the concentration of the potassium hydroxide solution is 0.5 to 2.5 mol / L. The concentration of the potassium hydroxide solution is 0.5mol / L, 0.6mol / L, 0.7mol / L, 0.8mol / L, 0.9mol / L, 1.0mol / L, 1.1mol / L, 1.2mol / L, 1.3mol / L, 1.4mol / L, 1.5mol / L, 1.6mol / L, 1.7mol / L, 1.8mol / L, 1.9mol / L, 2.0mol / L, 2.1mol / L, 2.2mol / L, 2.3mol / L, 2.4mol / L, 2.5mol / L or any value therebetween. Under high temperature conditions, the surface of the carbon material can be etched by the potassium source to produce water and carbon dioxide gas, generate a large number of pores, and the potassium element enters the carbon layer to expand, which is conducive to increasing the specific surface of the material.
[0038] In the embodiments of this specification, the mixing of the precarbide and the potassium source is carried out under heating. The heating temperature of the mixing of the precarbide and the potassium source is not limited by the present invention. Optionally, the heating temperature of the mixing of the precarbide and the potassium source is 80-100°C. Preferably, the heating temperature of the mixing of the precarbide and the potassium source is 80°C, 85°C, 90°C, 95°C, 100°C or any value therebetween. The mass ratio of the precarbide to the potassium source is not limited by the present invention. Optionally, the mass ratio of the precarbide to the potassium source is (0.5-3):1. Preferably, the mass ratio of the precarbide to the potassium source is 0.5:1, 1:1, 1.5:1, 2:1, 2.5:1, 3:1 or any value therebetween. The precarbide is mixed with the potassium source and then dried to constant weight to obtain an activated precursor.
[0039] In the embodiments of this specification, the temperature and time of the carbonization treatment of the activated precursor are not limited by the present invention, as long as the effect of obtaining the peony shell carbonized material required by the present invention can be achieved. Optionally, the temperature of the carbonization treatment of the activated precursor is 900-1500°C. Preferably, the temperature of the carbonization treatment of the activated precursor is 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C or any value therebetween. Optionally, the duration of the carbonization treatment of the activated precursor is 2-5h. Preferably, the duration of the carbonization treatment of the activated precursor is 2h, 3h, 4h, 5h or any value therebetween. The carbonization treatment of the activated precursor is carried out in a tubular furnace. The carbonization treatment of the activated precursor is carried out in an inert atmosphere. The process of carbonizing the activated precursor is to gradually increase the temperature, and the heating rate is not limited by the present invention. Optionally, the heating rate of carbonizing the activated precursor is 1 to 5°C / min. Preferably, the heating rate of carbonizing the activated precursor is 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min or any value therebetween.
[0040] In the embodiments of this specification, the mass ratio of the peony shell carbonized material to the asphalt is not limited by the present invention. Optionally, the mass ratio of the peony shell carbonized material to the asphalt is 8:(1-3). Preferably, the mass ratio of the peony shell carbonized material to the asphalt is 8:1, 8:2, 8:3 or any value therebetween. The asphalt is a soft carbon, which is more disordered than the resin-based hard carbon material and is more suitable for the diffusion of sodium ions.
[0041] In the embodiment of this specification, the coating of the peony shell carbonized material and the asphalt is achieved by kneading, specifically, the kneading coating is carried out in a kneader. The stirring speed and temperature during the coating are not limited by the present invention, as long as the coating effect required by the present invention can be achieved. Optionally, the stirring speed during the coating is 200-600r / min. Preferably, the stirring speed during the coating is 200r / min, 300r / min, 400r / min, 500r / min, 600r / min or any value therebetween. Optionally, the temperature during the coating is 150-250°C. Preferably, the temperature during the coating is 150°C, 160°C, 170°C, 180°C, 190°C, 200°C, 210°C, 220°C, 230°C, 240°C, 250°C or any value therebetween. Compared with the traditional coating ball milling or spray coating, the kneading coating asphalt method used in the present invention has the characteristics of higher efficiency and lower energy consumption. If the hard carbon negative electrode material is made of asphalt material alone, the asphalt material is easy to graphitize at high temperature, and usually needs to be pre-oxidized to ether or ester groups, which inhibits the rearrangement of the carbon layer structure at high temperature, and will generate a turbulent layer disordered hard carbon structure, which is not effective.
[0042] In the embodiments of this specification, the peony shell carbonized material is coated with asphalt, and the temperature and time of the subsequent heating treatment are not limited by the present invention, as long as the effect of obtaining the asphalt-coated peony shell carbon material required by the present invention can be achieved. Optionally, the temperature during the heating treatment is 200-800°C. Preferably, the temperature during the heating treatment is 200°C, 300°C, 400°C, 500°C, 600°C, 700°C, 800°C or any value therebetween. Optionally, the duration of the heating treatment is 1-3h. Preferably, the duration of the heating treatment is 1h, 2h, 3h or any value therebetween. The heating treatment is carried out in a tubular furnace. The heating treatment is carried out in an inert atmosphere.
[0043] In the embodiments of this specification, the mass ratio of the asphalt-coated peony shell carbon material to the aluminum nitrate or aluminum isopropoxide is not limited by the present invention. Optionally, the mass ratio of the asphalt-coated peony shell carbon material to the aluminum nitrate or aluminum isopropoxide is 1:(0.005-0.05). Preferably, the mass ratio of the asphalt-coated peony shell carbon material to the aluminum nitrate or aluminum isopropoxide is 1:0.005, 1:0.01, 1:0.02, 1:0.03, 1:0.04, 1:0.05 or any value therebetween. The aluminum nitrate or aluminum isopropoxide is dissolved in ethanol to form an ethanol solution of aluminum nitrate or aluminum isopropoxide, and then mixed with the asphalt-coated peony shell carbon material. After mixing, the mixture of the asphalt-coated peony shell carbon material and aluminum nitrate or aluminum isopropoxide is stirred and dried at 50-80°C before heating. In the step of mixing and heating the asphalt-coated peony shell carbon material with aluminum nitrate or aluminum isopropoxide, the heating temperature is 400-850°C. Preferably, the heating temperature is 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C or any value therebetween. In the step of mixing and heating the asphalt-coated peony shell carbon material with aluminum nitrate or aluminum isopropoxide, the heating duration is 1-3h. Preferably, the heating duration is 1h, 2h, 3h or any value therebetween. The heating is carried out in an inert atmosphere. The present invention can be carried out by mixing the aluminum nitrate or aluminum isopropoxide with a carbon material. Aluminum nitrate can be decomposed into Al under heating. 2 O 3 and NO 2 , can obtain the coating Al 2 O 3 When aluminum isopropoxide is heated, it first forms isopropanol and aluminum hydroxide, the isopropanol evaporates, and the aluminum hydroxide decomposes into the coating Al 2 O 3 .
[0044] The present invention adopts a coating method to improve the first efficiency of hard carbon materials, which is a common problem of low first efficiency. The peony shell-based double-layer coated sodium ion battery hard carbon negative electrode material prepared by the present invention fully utilizes the characteristics of peony shell carbon material, asphalt coating layer, and alumina coating layer, and the prepared material has the characteristics of high gram capacity, high rate performance, and high first efficiency.
[0045] The present invention adopts peony shell carbon material, which is widely used due to its wide sources, low cost, simple preparation method and other characteristics. According to the sodium storage mechanism of hard carbon materials, it mainly includes adsorption, intercalation and closed-pore filling. The pore size and distribution, internal defects, carbon layer spacing and surface morphology of hard carbon materials have a great influence on the electrical properties. The biomass material peony shell carbon material is more suitable for hard carbon preparation due to its unique porosity and self-doping characteristics. In view of the low capacity of biomass materials, the present invention performs heteroatom doping modification on them to increase active sites and improve the sodium storage capacity; the hard carbon negative electrode material has many internal defects, which leads to irreversible adsorption of sodium ions and reduces the efficiency of the battery in the first charge and discharge. The present invention performs a coating modification treatment on them to reduce the contact area between the material surface and the electrolyte, reduce side reactions and increase the first effect, while increasing the number of closed pores and increasing the sodium storage capacity.
[0046] The peony shell carbon material of the present invention is subjected to low-temperature pre-carbonization treatment to remove impurities such as internal moisture and volatile components; the pre-carbonized material is activated, and a potassium source is commonly used to activate the material with an etching property; then high-temperature carbonization is performed, and this step completes thermal decomposition and thermal polycondensation reactions to form aromatic compounds, and graphene sheets in a local graphitized microcrystalline structure continuously grow and tend to be arranged in parallel, forming graphite microcrystals with larger sizes in both the parallel stacking direction and the basal plane direction; while a large number of defects are still contained in the structure of the non-graphitizable carbon material at the cross-linked structure, and the graphene sheets are locally stacked to form a short-range ordered turbulent layer structure.
[0047] The carbon source used in the hard carbon negative electrode material prepared by the present invention is a peony shell material with a wide range of sources and low prices, which is rich in N and S elements and has the characteristics of self-doping. The present invention adopts a peony shell-based material as the main body, and sequentially adopts a double-layer coating method of asphalt and alumina to improve the material performance. The present invention adopts a kneading coating method to coat the peony shell material with asphalt.
[0048] The present invention uses peony shells to prepare active negative electrode carbon materials, which have the characteristics of easy acquisition of raw materials, green environmental protection, sustainability, etc., and the prepared material has a relatively uniform porous structure and a large specific surface area, and contains rich heteroatoms such as N and S, and is a good carbon precursor. The peony shells are pre-carbonized and high-temperature carbonized to obtain a core structure material with a high capacity, and then double-layer coating is performed with asphalt and alumina in sequence. After the asphalt soft carbon coating, the number of peony shell hard carbon closed pores is increased to improve the sodium storage capacity of the material, the asphalt coating layer increases the diffusion rate of sodium ions, and the alumina coating reduces the contact area between the carbon material and the electrolyte to improve the first efficiency. The asphalt kneading coating method used improves the coating efficiency and reduces energy consumption. The hard carbon negative electrode material prepared by the asphalt kneading coating method has the characteristics of high gram capacity, good rate performance, high first efficiency and good cycle stability.
[0049] The present invention crushes the peony shell material for pre-carbonization, activates it with a potassium source, and then carbonizes it at high temperature, and then sequentially coats it with an intermediate layer of asphalt soft carbon and an alumina shell. This method gives full play to the respective advantages of the three materials of the core-shell structure, and the prepared hard carbon negative electrode material has the characteristics of high gram capacity, good rate performance, high first efficiency, and good cycle stability.
[0050] According to one embodiment of the present application, a hard carbon negative electrode material is provided, which is prepared by the preparation method described above.
[0051] The structure of the hard carbon negative electrode material is that the inner core structure is a peony shell carbonized material, the middle is an asphalt coating layer, and the outer shell is an aluminum oxide coating layer.
[0052] According to one embodiment of the present application, a battery is provided, the battery comprising the hard carbon negative electrode material prepared by the preparation method described above or the hard carbon negative electrode material described above.
[0053] The technical solutions provided by various embodiments of the present application are described in detail below in conjunction with the accompanying drawings.
[0054] Embodiment 1:
[0055] A method for preparing a hard carbon negative electrode material is provided, comprising the following steps:
[0056] (1) Weigh 50 g of peony shell raw material, mechanically crush the peony shell raw material and sieve it with a 50-mesh screen; put the screened peony shell into a tubular furnace, and pretreat it in an inert atmosphere at 400° C. for 2.5 h to obtain a pre-carbonized product; mix the obtained pre-carbonized product with a 1.5 mol / L KOH solution, stir and heat at 95° C., mix them evenly at a mass ratio of pre-carbonized product to potassium salt of 2.5:1, and dry them to constant weight to obtain an activated precursor.
[0057] (2) The prepared activated precursor was placed in a tubular furnace and subjected to high-temperature carbonization treatment at 1400°C in an inert atmosphere for 4 h at a heating rate of 3°C / min. After cooling to room temperature, the precursor was washed with hydrochloric acid and deionized water in turn until neutral, and dried to obtain the peony shell carbonized material.
[0058] (3) The obtained peony shell carbonized material is mixed with asphalt, wherein the mass ratio of the peony shell carbonized material to the asphalt is 8:2, and the kneading and coating are carried out in a kneading machine at a kneading stirring speed of 500 r / min and a temperature of 200°C. The obtained product is placed in a tubular furnace and heat-treated in an inert atmosphere at 500°C for 2 h to obtain an asphalt-coated peony shell carbon material.
[0059] (4) Prepare an ethanol solution of aluminum nitrate with a concentration of 50 g / L, and evenly disperse the obtained asphalt-coated peony shell carbon material in the ethanol solution of aluminum nitrate, wherein the mass ratio of the asphalt-coated peony shell carbon material to aluminum nitrate is 1:0.03, use a rotary evaporator to stir and dry the peony shell carbon material and aluminum nitrate at 70°C, and use a tubular furnace to keep the dried product in an inert gas atmosphere at 500°C for 2 hours to obtain a double-layer coated peony shell-based sodium ion battery hard carbon negative electrode material.
[0060] Embodiment 2:
[0061] A method for preparing a hard carbon negative electrode material is provided, comprising the following steps:
[0062] (1) Weigh 50 g of peony shell raw material, mechanically crush the peony shell raw material and sieve it with a 50-mesh screen; put the screened peony shell into a tube furnace, and pretreat it in an inert atmosphere at 300° C. for 2 h to obtain a pre-carbonized product; mix the obtained pre-carbonized product with a 0.5 mol / L KOH solution, stir and heat at 80° C., mix them evenly at a mass ratio of pre-carbonized product to potassium salt of 0.5:1, and dry them to constant weight to obtain an activated precursor.
[0063] (2) The prepared activated precursor was placed in a tubular furnace and subjected to high-temperature carbonization treatment in an inert atmosphere at 900°C for 5 h at a heating rate of 1°C / min. After cooling to room temperature, the precursor was washed with hydrochloric acid and deionized water in turn until neutral, and dried to obtain the peony shell carbonized material.
[0064] (3) The obtained peony shell carbonized material is mixed with asphalt, wherein the mass ratio of the peony shell carbonized material to the asphalt is 8:1, and the kneading and coating are carried out in a kneading machine at a kneading stirring speed of 200 r / min and a temperature of 150°C. The obtained product is placed in a tubular furnace and heat-treated in an inert atmosphere at 200°C for 1 h to obtain a asphalt-coated peony shell carbon material.
[0065] (4) Prepare an ethanol solution of aluminum nitrate with a concentration of 50 g / L, and evenly disperse the obtained asphalt-coated peony shell carbon material in the ethanol solution of aluminum nitrate, wherein the mass ratio of the asphalt-coated peony shell carbon material to aluminum nitrate is 1:0.005, use a rotary evaporator to stir and dry the peony shell carbon material and aluminum nitrate at 50°C, and use a tubular furnace to keep the dried product in an inert gas atmosphere at 400°C for 1 hour to obtain a double-layer coated peony shell-based sodium ion battery hard carbon negative electrode material.
[0066] Embodiment 3:
[0067] A method for preparing a hard carbon negative electrode material is provided, comprising the following steps:
[0068] (1) Weigh 50 g of peony shell raw material, mechanically crush the peony shell raw material, and then sieve it with a 50-mesh screen; put the screened peony shell into a tube furnace, and pretreat it in an inert atmosphere at 250° C. for 3 h to obtain a pre-carbonized product; mix the obtained pre-carbonized product with a 2.5 mol / L KOH solution, stir and heat at 100° C., mix them evenly at a mass ratio of pre-carbonized product to potassium salt of 3:1, and dry them to constant weight to obtain an activated precursor.
[0069] (2) The prepared activated precursor was placed in a tubular furnace and subjected to high-temperature carbonization treatment at 1500°C in an inert atmosphere for 2 h at a heating rate of 5°C / min. After cooling to room temperature, the precursor was washed with hydrochloric acid and deionized water in turn until neutral, and dried to obtain the peony shell carbonized material.
[0070] (3) The obtained peony shell carbonized material is mixed with asphalt, wherein the mass ratio of the peony shell carbonized material to the asphalt is 8:3, and the kneading and coating are carried out in a kneading machine at a kneading stirring speed of 600 r / min and a temperature of 250°C. The obtained product is placed in a tubular furnace and heat-treated in an inert atmosphere at 800°C for 3 hours to obtain an asphalt-coated peony shell carbon material.
[0071] (4) Prepare an ethanol solution of aluminum nitrate with a concentration of 50 g / L, and evenly disperse the obtained asphalt-coated peony shell carbon material in the ethanol solution of aluminum nitrate, wherein the mass ratio of the asphalt-coated peony shell carbon material to aluminum nitrate is 1:0.05, use a rotary evaporator to stir and dry the peony shell carbon material and aluminum nitrate at 80°C, and use a tubular furnace to keep the dried product in an inert gas atmosphere at 850°C for 3 hours to obtain a double-layer coated peony shell-based sodium ion battery hard carbon negative electrode material.
[0072] Performance Testing:
[0073] Capacity test method: The prepared hard carbon negative electrode material and the sodium sheet are assembled into a button-type half-cell for electrical performance testing.
[0074] Material capacity test: The assembled button half-cell is discharged to 0V with constant current of 0.1C, 0.05C, and 0.02C in sequence, and then charged to 2V with constant current of 0.1C. The cycle is repeated for 3 weeks. The charged capacity is the capacity of the hard carbon negative electrode material. The ratio of the first charged capacity to the first discharged capacity in the first cycle measured by this method is the first efficiency.
[0075] 3C rate test: The assembled button half-cell is discharged to 0V with a 0.1C constant current, and then charged to 2V with a 3C constant current. The cycle is repeated for 3 weeks to obtain the capacity of the material at a 3C rate.
[0076] Cycle test: Discharge to 0V with 0.1C constant current, then charge to 2V with 0.1C constant current for cycle test.
[0077] Table 1 shows the electrochemical properties of the materials obtained in each step of Example 1 (voltage: 0-2V)
[0078]
[0079] The above experimental results show that the peony shell-based sodium ion battery hard carbon negative electrode material prepared by the method of the present invention has significantly improved material capacity, rate and first efficiency on the basis of double-layer coating.
[0080] The above is only the embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application should be included in the scope of the claims of the present application.
Claims
1. A method for preparing a hard carbon negative electrode material, characterized in that: The following steps are involved: Taking peony shell and heating it to obtain a pre-carbonized product, and then mixing the pre-carbonized product with a potassium source to obtain an activated precursor; Carbonizing the activated precursor to obtain a peony shell carbonized material; The peony shell carbonized material is coated with asphalt and subjected to a heating treatment to obtain an asphalt-coated peony shell carbon material; The asphalt-coated peony shell carbon material is mixed with aluminum nitrate or aluminum isopropoxide and heated to obtain a hard carbon negative electrode material.
2. The preparation method according to claim 1, characterized in that: In the step of heating the peony shell to obtain the pre-carbonized product, the heating temperature is 250-400° C.; and / or, The heating duration is 2 to 3 hours.
3. The preparation method according to claim 1, characterized in that: The mass ratio of the pre-carbonized material to the potassium source is (0.5-3):
1.
4. The preparation method according to claim 1, characterized in that: The step of mixing the pre-carbonized material with the potassium source is carried out under heating.
5. The preparation method according to claim 1, characterized in that: In the step of carbonizing the activated precursor to obtain the peony shell carbonized material, The temperature of the carbonization treatment is 900-1500° C.; and / or, The duration of the carbonization treatment is 2 to 5 hours; and / or, The heating rate is 1-5°C / min.
6. The preparation method according to claim 1, characterized in that: In the step of coating the peony shell carbonized material with asphalt and heating it to obtain the asphalt-coated peony shell carbon material, the mass ratio of the peony shell carbonized material to the asphalt is 8:(1-3); and / or, The coating of the peony shell carbonized material with asphalt is achieved by kneading with a kneader; and / or, The stirring speed during coating is 200 to 600 r / min; and / or, The temperature during coating is 150 to 250°C.
7. The preparation method according to claim 1, characterized in that: In the step of coating the peony shell carbonized material with asphalt and heating it to obtain the asphalt-coated peony shell carbon material, the mass ratio of the asphalt-coated peony shell carbon material to the aluminum nitrate or aluminum isopropoxide is 1:(0.005-0.05); and / or, The temperature of the heating treatment is 200-800° C.; and / or, The duration of the heating treatment is 1 to 3 hours.
8. The preparation method according to claim 1, characterized in that: In the step of coating the peony shell carbonized material with asphalt and heating it to obtain the asphalt-coated peony shell carbon material, the heating temperature is 200-800° C.; and / or, The duration of the heating treatment is 1 to 3 hours.
9. A hard carbon negative electrode material, characterized in that: Prepared by the preparation method described in any one of claims 1 to 8.
10. A battery, characterized in that: The battery comprises the hard carbon negative electrode material prepared by the preparation method according to any one of claims 1 to 8 or the hard carbon negative electrode material according to claim 9.