A calcium aluminate synthetic slag and its preparation method and its application in the smelting method of high carbon steel
Through the preparation method of calcium aluminate synthetic slag, aluminum-killed steel refining waste slag is mechanically mixed with lime and bauxite to form a low melting point CaO-Al2O3-SiO2-MgO quaternary refining slag system, which solves the problem of the high cost and high cost of traditional synthetic slag. The problem of high fluorspar consumption has led to the realization of an efficient and environmentally friendly high-carbon steel smelting process.
Patent Information
- Application Number
- CN202410608315.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-05-16
AI Technical Summary
The production cost of traditional synthetic slag is high, and the high consumption of fluorspar during the smelting process of high-carbon steel leads to high smelting costs and pollution problems, and it is difficult to effectively utilize aluminum-killed steel refining waste slag with existing technology.
Calcium aluminate synthetic slag is used, and the calcium aluminate refining slag produced during the secondary refining of aluminum-killed steel is mechanically mixed with lime and bauxite to form a low melting point CaO-Al2O3-SiO2-MgO quaternary refining slag system. It is used in the smelting of high carbon steel to reduce the use of fluorspar and realize the secondary utilization of aluminum-killed steel refining waste residue.
It reduces the production cost of calcium aluminate synthetic slag, reduces the use of fluorspar, improves smelting efficiency and environmental protection effects, and ensures steel quality and desulfurization effects.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to calcium aluminate synthetic slag, a preparation method thereof and a smelting method thereof applied to high carbon steel, and belongs to the technical field of high carbon steel smelting. Background Art
[0002] Traditional synthetic slag is obtained by mixing and melting lime, high-purity alumina, bauxite, quartz sand, fluorite and other materials at high temperatures, and then crushing and screening. The raw material and process costs are relatively high. After water cooling and iron selection, the waste slag produced in the secondary refining process of molten steel in steel mills is directly recovered in hot state for smelting of the same steel grade, and part of it is used for cement production after iron selection. The rest is basically buried and piled up, causing certain pollution to the environment. Therefore, in order to reduce the production cost of synthetic slag, it is urgent to optimize and improve the raw materials and production process.
[0003] High carbon steel represented by hard steel strands is actually a type of silicon-killed steel. Aluminum deoxidation is not used in its smelting process. Secondary refining mainly produces CaO-SiO2-MgO refining slag system to complete desulfurization, adsorb inclusions in molten steel, isolate air and keep warm. Since the melting point of CaO-SiO2-MgO refining slag is relatively high, more fluorite needs to be added to assist in slagging. Otherwise, the refining slag will agglomerate, and the fluidity and liquid sealing effect will deteriorate. The desulfurization, adsorption of inclusions, isolation of air and insulation effects are difficult to meet the requirements of secondary refining. Moreover, the price of fluorite is relatively high, which increases the smelting cost. The main component of fluorite is CaF2, which will also produce some fluorides that are harmful to the human body during use, and the fluorine-containing waste slag will also cause certain pollution to the environment during stacking and treatment. In order to reduce the use of fluorite in silicon-killed steel refining, the main existing process methods are: 1) hot recycling of calcium silicate refining slag. This process can play a certain role in fluxing and slag removal, but as the number of refined slag cycles increases, the sulfur content in the refined slag is enriched, which is not conducive to the desulfurization of molten steel. 2) Reduce the basicity of the slag. This method can also reduce the melting point of CaO-SiO2-MgO refined slag and accelerate the slag removal rate, but the lower basicity is not conducive to the desulfurization of molten steel. 3) Add some metallic aluminum during the deoxidation process of molten steel to make CaO-Al2O3-SiO2-MgO low-melting point refined slag. This method can achieve rapid slag removal, but the Al melted into the molten steel will not only cause the Al element in the molten steel to exceed the standard, but also cause the increase of Al2O3 inclusions, a deoxidation product, in the molten steel. On the one hand, Al2O3 inclusions are very easy to deposit on the inner wall of the nozzle during pouring, causing nodules and blockage; on the other hand, Al2O3 entering the finished material will cause the material to fracture hard and brittle, and the fatigue life will be reduced. Therefore, this technical field urgently needs to develop a low-cost silicon-killed steel refining and slag making method to reduce the use of fluorite while ensuring good refining effect and steel quality. Summary of the invention
[0004] The present invention provides a calcium aluminate synthetic slag and a preparation method thereof and a smelting method for high carbon steel, thereby realizing the secondary utilization of aluminum killed steel refining waste slag and solving the problems of high production cost of traditional synthetic slag and high fluorite consumption in the high carbon steel smelting process leading to high smelting cost and serious pollution.
[0005] The technical solution adopted by the present invention to solve its technical problem is:
[0006] A calcium aluminate synthetic slag, comprising calcium aluminate refined slag produced in the secondary refining process of aluminum killed steel;
[0007] It also includes lime and bauxite, wherein the mass ratio of calcium aluminate refining slag, lime and bauxite is 8:0.5:1.5-8:1.5:0.5;
[0008] As a further preferred embodiment of the present invention, in the calcium aluminate synthetic slag formed by mixing calcium aluminate refining slag, lime and bauxite, the mass fractions include 60-65% CaO, 30-35% Al2O3, ≤2% of the total amount of FeO and MnO, ≤3% of SiO2, and ≤0.1% of S.
[0009] According to the preparation method of calcium aluminate synthetic slag,
[0010] The specific steps include:
[0011] Step S1: recovering calcium aluminate refining slag produced during the secondary refining process of aluminum killed steel;
[0012] Step S2: cooling the recovered calcium aluminate refined slag to room temperature, crushing it to form powder slag with a particle size less than or equal to 6 mm, and removing iron from the calcium aluminate refined slag powder slag by magnetic separation;
[0013] Step S3: Select lime and bauxite, and crush the lime and bauxite to form powder residue with a particle size less than or equal to 6 mm;
[0014] Step S4: uniformly mixing the calcium aluminate refined slag, lime and bauxite obtained after magnetic separation in step S2 in a mass ratio of 8:0.5:1.5-8:1.5:0.5 to form calcium aluminate synthetic slag;
[0015] As a further preferred embodiment of the present invention, the recovered calcium aluminate refined slag has a sulfur content of ≤0.005% after pre-desulfurization of molten iron in the smelting process of aluminum-killed steel;
[0016] As a further preferred embodiment of the present invention, the silicon content of the aluminum-killed steel product formed by the recycled calcium aluminate refined slag after the aluminum-killed steel smelting process is ≤0.3%;
[0017] The method for smelting high carbon steel using the calcium aluminate synthetic slag specifically comprises the following steps:
[0018] Step S1: After the smelting in the primary furnace is completed, lime and deoxidation alloy are added to the molten steel in the ladle during the steel tapping process;
[0019] Step S2: after the ladle is finished tapping, the ladle bottom blowing and stirring are started, and hot excess steel and slag are added to the molten steel in the ladle in sequence, followed by adding carbon powder and the calcium aluminate synthetic slag; wherein the amount of the calcium aluminate synthetic slag added is determined according to the sulfur content of the molten steel tapped from the primary furnace in step S1;
[0020] Step S3: The ladle enters the refining process, firstly, sampling and temperature measurement are carried out, refining bottom blowing and stirring are started, and then electrodes are inserted into the ladle to energize and heat up;
[0021] Step S4: according to the composition of the molten steel sampled and measured in step S3, alloy and carbon powder are added to adjust the composition of the molten steel to the target composition range, calcium carbide is added to the slag surface of the molten steel, and the continuous casting process is carried out after sufficient soft stirring;
[0022] As a further preferred embodiment of the present invention, in step S1, the amount of lime added to the molten steel in the ladle during the steel tapping process is 1-3 kg / t;
[0023] The deoxidizing alloys added are ferrosilicon and ferromanganese, and the amount of ferrosilicon added is:
[0024] m 硅铁 =(P Si成品 -P Si初始 )×1000×m 钢水 / η Si / P 硅铁 ,
[0025] The amount of ferromanganese added is:
[0026] m 锰铁 =(P Mn成品 -P Mn初始 )×1000×m 钢水 / η Mn / P 锰铁 ,
[0027] Among them, m 硅铁 is the amount of ferrosilicon added during steelmaking, kg; P Si成品 is the silicon content of the finished steel product, %; P Si初始 is the silicon content of molten steel, %; m 钢水 is the weight of molten steel, t; η Si is the silicon recovery coefficient, ranging from 0.5 to 0.8; P 硅铁 is the silicon content in ferrosilicon, %; m 锰铁is the amount of ferromanganese added during steelmaking, kg; P Mn成品 is the manganese content of the finished steel product, %; P Mn初始 is the manganese content of molten steel, %; η Mn is the manganese recovery coefficient, ranging from 1.0 to 1.2; P 锰铁 is the manganese content in ferromanganese, %;
[0028] As a further preferred embodiment of the present invention, in step S2, hot excess steel slag is added to the molten steel in the ladle in sequence, specifically, the ladle filled with hot excess steel slag is set as ladle No. 1, the ladle hoisted from the refining process is set as ladle No. 2, the ladle that completes the secondary refining process through power-on charging in step S4 is ladle No. 3, the ladle from which the molten steel in the primary refining furnace is tapped is ladle No. 4, and the hot excess steel slag of ladle No. 1 is poured into ladle No. 4;
[0029] As a further preferred embodiment of the present invention, in step S2, the amount of carbon powder added is:
[0030] m 碳粉 =(P C成品 -P C初始 )×1000×m 钢水 ×85% / η C / P 碳粉 ,
[0031] Among them, m 碳粉 P is the amount of carbon powder added to steel, kg; C成品 is the carbon content of the finished steel product, %; P C初始 is the carbon content of molten steel, %; m 钢水 is the weight of molten steel; C is the carbon recovery coefficient, ranging from 0.8 to 1.0; P 碳粉 is the carbon content in carbon powder, %;
[0032] As a further preferred embodiment of the present invention, in step S2, the amount of calcium aluminate synthetic slag added is determined according to the sulfur content of the molten steel tapped from the primary furnace in step S1, specifically:
[0033] When the sulfur content of molten steel is ≤0.03%, add 1.5kg / t<the weight of calcium aluminate synthetic slag ≤2.5kg / t;
[0034] When the sulfur content of molten steel is 0.03%<≤0.05%, add 2.5kg / t<the weight of calcium aluminate synthetic slag ≤4kg / t;
[0035] When the sulfur content of molten steel is greater than 0.05%, add 4kg / t<5kg / t of calcium aluminate synthetic slag and add 0.5-1.5kg / t of lime;
[0036] As a further preferred embodiment of the present invention, in step S2, after the ladle is finished tapping, the ladle bottom blowing and stirring are started, wherein the ladle bottom blowing and stirring lasts for 10-15 minutes, and the bottom blowing argon flow rate is 600-900NL / min;
[0037] As a further preferred embodiment of the present invention, in step S3, during refining bottom blowing and stirring, the argon flow rate is 300-400NL / min;
[0038] As a further preferred embodiment of the present invention, in step S4, during soft stirring, the argon flow rate is 50-150 NL / min.
[0039] Through the above technical solution, compared with the prior art, the present invention has the following beneficial effects:
[0040] 1. The calcium aluminate synthetic slag provided by the present invention uses aluminum-killed steel refining slag as raw material, and uses it for refining and slag-making of silicon-killed steel series. By adding a small amount of lime and bauxite, adjusting the proportion of CaO and Al2O3 components in the slag, and reducing the content of other impurity components, a calcium aluminate synthetic slag with a composition similar to that of the calcium aluminate synthetic slag currently on the market and the same function can be obtained. Compared with raw ore materials such as lime, the cost is lower, and the secondary utilization of aluminum-killed steel refining waste slag is realized;
[0041] 2. The method for preparing calcium aluminate synthetic slag provided by the present invention designs a low-melting-point CaO-Al2O3-SiO2-MgO quaternary refining slag system and adopts a processing method of mechanically mixing aluminum-killed steel refining waste slag, a small amount of lime and bauxite. Compared with remelting and crushing of raw ore materials, the energy consumption is very low and the production efficiency is greatly improved;
[0042] 3. The present invention provides a method for smelting high carbon steel using the calcium aluminate synthetic slag. According to the sulfur content of molten steel from the primary smelting furnace, a method for adding the calcium aluminate synthetic slag is designed, and a method for recycling excess steel and slag is combined to achieve rapid slagging and obtain a stable desulfurization effect. DETAILED DESCRIPTION
[0043] As described in the background technology, the traditional calcium aluminate synthetic slag production mainly uses lime, high-purity alumina, bauxite, fluorite and other raw materials, which are mixed and melted at high temperature, and then cooled, crushed and screened to obtain the finished product. Fresh lime, high-purity alumina, bauxite, fluorite and the like are relatively expensive, and the production process is long and the process energy consumption is high, which leads to the disadvantages of high cost of calcium aluminate synthetic slag and high selling price.
[0044] When smelting high-carbon steel of silicon-killed steel series represented by hard steel strand, in order to ensure that the mechanical properties of hard steel strand meet the working conditions, it is necessary to ensure a low aluminum content and the number of Al2O3 inclusions in the steel when smelting this type of steel. Therefore, aluminum deoxidation is not used in the deoxidation of molten steel, but silicon deoxidation is selected, resulting in the mainstream slag system in the secondary refining process being a high-melting-point CaO-SiO2-MgO slag system. In order to ensure the fluidity of the refined slag and obtain good desulfurization and inclusion removal effects, more slag-forming agent fluorite must be added to achieve rapid slag-forming. The use of fluorite also leads to high costs of auxiliary materials for secondary refining of molten steel and fluoride pollution problems.
[0045] Therefore, as the first more prominent innovation point of this application, it is found through analysis that the refined waste slag produced by the smelting of aluminum-killed steel has a similar composition to the calcium aluminate synthetic slag, both of which belong to the CaO-Al2O3-SiO2-MgO slag system. By adding a small amount of lime and bauxite, adjusting the proportion of CaO and Al2O3 components in the slag, and reducing the content of other impurity components, a calcium aluminate synthetic slag with a similar composition and the same function as the calcium aluminate synthetic slag currently on the market can be obtained. The refined waste slag of aluminum-killed steel belongs to metallurgical solid waste after pre-melting, and its cost is lower than that of raw ore materials such as lime. Compared with the remelting and crushing of raw ore materials, the processing method of mechanically mixing aluminum-killed steel refined waste slag, a small amount of lime and bauxite has very low energy consumption and greatly improved production efficiency.
[0046] Therefore, the present application provides a calcium aluminate synthetic slag, which mainly includes calcium aluminate refining slag produced in the secondary refining process of aluminum-killed steel; in order to adjust the proportion of CaO and Al2O3 components in the slag, lime and bauxite are also included, and the calcium aluminate refining slag, lime and bauxite are mixed to obtain calcium aluminate synthetic slag. By crushing and mechanically mixing a small amount of lime and bauxite, a calcium aluminate synthetic slag with stable chemical composition and performance is formed, which realizes the secondary utilization of aluminum-killed steel refining slag, not only greatly reducing the production cost of calcium aluminate synthetic slag, but also reducing the discharge of steel mill refining waste slag.
[0047] It is not enough to simply provide the composition of the calcium aluminate synthetic slag. The calcium aluminate synthetic slag obtained by a relevant preparation method can achieve the corresponding effect. Therefore, the present application also provides a preparation method of the calcium aluminate synthetic slag, which specifically includes the following steps:
[0048] Step S1: Recovering the calcium aluminate refining slag produced during the secondary refining of aluminum-killed steel; the recovered calcium aluminate refining slag has a sulfur content of ≤0.005% after pre-desulfurization of molten iron in the smelting process of aluminum-killed steel, and a silicon content of ≤0.3% in the finished aluminum-killed steel product.
[0049] Step S2: Cool the recovered calcium aluminate refined slag to room temperature, crush it to form powder slag with a particle size less than or equal to 6 mm, and remove iron from the calcium aluminate refined slag powder slag by magnetic separation.
[0050] Step S3: Select lime and bauxite, and crush the lime and bauxite to form powder residue with a particle size less than or equal to 6 mm.
[0051] Step S4: The calcium aluminate refining slag, lime and bauxite are uniformly mixed in a mass ratio of 8:0.5:1.5-8:1.5:0.5 to form calcium aluminate synthetic slag.
[0052] The calcium aluminate synthetic slag obtained according to the above preparation method can obtain the CaO-Al2O3-SiO2-MgO quaternary refining slag system, which is a low melting point material, successfully reducing the use of refined fluorite, and achieving low-cost and environmentally friendly smelting. In the formed calcium aluminate synthetic slag, according to the mass fraction, CaO is 60-65%, Al2O3 is 30-35%, the total amount of FeO and MnO is ≤2%, SiO2≤3%, and S≤0.1%. The proportion of the above components can ensure that the steel contains a lower aluminum content and the number of Al2O3 inclusions when smelting the corresponding steel grade, ensuring that the mechanical properties of the corresponding steel grade products meet the working conditions.
[0053] As a high carbon steel represented by hard steel strand, such as hard steel strand SWRH82B, its main components are C 0.81-0.84%, Si 0.18-0.22%, Mn 0.78-0.82%, P ≤0.01%, S ≤0.015%, Cr 0.16-0.20%, Al ≤0.01%, and Fe and other inevitable impurity components. During smelting, in addition to adding the calcium aluminate synthetic slag provided by the present application as a slag-forming agent, it is also necessary to cooperate with corresponding smelting means. Therefore, the present application also provides a smelting method using the calcium aluminate synthetic slag, which specifically includes the following steps:
[0054] Step S1: After the smelting in the primary furnace is completed, lime and deoxidation alloy are added to the molten steel in the ladle during the steel tapping process;
[0055] The amount of lime added to the molten steel in the ladle during the tapping process is 1-3kg / t;
[0056] The deoxidizing alloys added are ferrosilicon and ferromanganese, and the amount of ferrosilicon added is:
[0057] m 硅铁 =(P Si成品 -P Si初始 )×1000×m 钢水 / η Si / P 硅铁 ,
[0058] The amount of ferromanganese added is:
[0059] m 锰铁 =(P Mn成品 -P Mn初始 )×1000×m 钢水 / η Mn / P 锰铁 ,
[0060] Among them, m 硅铁 is the amount of ferrosilicon added during steelmaking, kg; P Si成品 is the silicon content of the finished steel product, %; P Si初始 is the silicon content of molten steel, %; m 钢水 is the weight of molten steel, t; η Si is the silicon recovery coefficient, ranging from 0.5 to 0.8; P 硅铁 is the silicon content in ferrosilicon, %; m 锰铁 is the amount of ferromanganese added during steelmaking, kg; P Mn成品 is the manganese content of the finished steel product, %; P Mn初始 is the manganese content of molten steel, %; η Mn is the manganese recovery coefficient, ranging from 1.0 to 1.2; P 锰铁 is the manganese content in ferromanganese, %.
[0061] Step S2: after the ladle is finished tapping, the ladle bottom blowing and stirring are started, the ladle bottom blowing and stirring lasts for 10-15 minutes, and the bottom blowing argon flow rate is 600-900NL / min; and hot excess steel and slag are added to the molten steel in the ladle in sequence, followed by adding carbon powder and the calcium aluminate synthetic slag; wherein the amount of the calcium aluminate synthetic slag added is determined according to the sulfur content of the molten steel tapped from the primary furnace in step S1;
[0062] This step involves several other major innovations of this application. The first is the hot steel residue. The so-called hot steel residue is actually the remaining molten steel and slag in the ladle of the same steel grade cast in the previous furnace. For the convenience of explanation, the ladle filled with hot steel residue is set as ladle No. 1, the ladle hoisted from the refining process is ladle No. 2, the ladle that completes the secondary refining process through power-on feeding in step S4 is ladle No. 3, and the ladle that taps the molten steel from the primary refining furnace is ladle No. 4, then the hot steel residue of ladle No. 1 is poured into ladle No. 4. Generally, according to experience, the backflow amount of the previous furnace is 8-12kg / t, and the continuous backflow times of surplus steel slag shall not exceed 3 furnaces. The backflow amount of surplus steel slag gradually decreases according to the backflow times, which are 10-12kg / t for the first backflow, 8-10kg / t for the second backflow, and 6-8kg / t for the third backflow. For the furnaces of surplus steel slag that are not backflowed, add 1-2kg / t of lime after adding calcium aluminate casting slag.
[0063] Secondly, the amount of carbon powder and the calcium aluminate synthetic slag added also needs to be strictly controlled. The amount of carbon powder added is:
[0064] m 碳粉 =(P C成品 -P C初始 )×1000×m 钢水 ×85% / η C / P 碳粉 ,
[0065] Among them, m 碳粉 P is the amount of carbon powder added to steel, kg; C成品 is the carbon content of the finished steel product, %; P C初始 is the carbon content of molten steel, %; m 钢水 is the weight of molten steel; C is the carbon recovery coefficient, ranging from 0.8 to 1.0; P 碳粉 is the carbon content in the toner, %.
[0066] The amount of calcium aluminate synthetic slag added is determined according to the sulfur content of the molten steel tapped from the primary furnace in step S1, specifically:
[0067] When the sulfur content of molten steel is ≤0.03%, add 1.5kg / t<the weight of calcium aluminate synthetic slag ≤2.5kg / t;
[0068] When the sulfur content of molten steel is 0.03%<≤0.05%, add 2.5kg / t<the weight of calcium aluminate synthetic slag ≤4kg / t;
[0069] When the sulfur content of molten steel is greater than 0.05%, add 4kg / t<5kg / t of calcium aluminate synthetic slag and add 0.5-1.5kg / t of lime.
[0070] Step S3: The ladle enters the refining process, firstly, sampling and temperature measurement are carried out, and the refining bottom blowing and stirring are turned on. During the refining bottom blowing and stirring, the argon flow rate is 300-400NL / min; then electrodes are inserted into the ladle to energize and heat up.
[0071] Step S4: Measure the composition of the molten steel sampled and tested in step S3, add alloy and carbon powder to adjust the composition of the molten steel to within the target composition range (the preset target of the molten steel here includes not only the impurity elements sulfur and aluminum, but also the alloy content of silicon, manganese, etc. required by the steel grade), add calcium carbide to the slag surface of the molten steel (according to normal experience, the amount of calcium carbide usually added is 60-100kg / furnace), and implement the continuous casting process after sufficient soft stirring. During soft stirring, the argon flow rate is 50-150NL / min to ensure that there is no exposed molten steel on the surface of the molten steel covered by the slag.
[0072] After refining, calculated by weight percentage, the high-melting-point Ca2SiO4 phase in the slag is 30-40%, and the low-melting-point CaAl2O6 phase after cooling and precipitation is 15-20%.
[0073] If the finished product obtained by the above smelting method is a hard steel strand product, the carbon content of the finished product shall be ≤0.9%, the upper limit of the sulfur content of the finished product shall not be less than 0.01%, and the upper limit of the aluminum content of the finished product shall not be less than 0.005%.
[0074] In order to verify the above-mentioned technical means, the present application also provides six groups of specific embodiments of the smelting method of high carbon steel using the above-mentioned calcium aluminate synthetic slag. Through the six groups of specific embodiments, the corresponding desulfurization rate, slag-forming time and increased slag-making cost are obtained. At the same time, four groups of data on desulfurization rate, slag-forming time and increased slag-making cost obtained by smelting high carbon steel without using recycled refined slag are provided. These four groups of examples are used as comparison examples to intuitively reflect the excellence of the technical means of the present application.
[0075] Comparative Example 1
[0076] The smelting method of silicon-killed steel hard strand SWRH82B provided in Comparative Example 1 comprises the following steps:
[0077] In the short-process steelmaking workshop with a nominal capacity of 100t, the steel grade to be smelted is hard steel strand SWRH82B, and the P of ferrosilicon used in the process is Si The P content of ferromanganese is 72%. Mn The P of toner is 66%. 碳粉 The main components of hard steel strand SWRH82B are 0.81-0.84% C, 0.18-0.22% Si, 0.78-0.82% Mn, ≤0.01% P, ≤0.015% S, 0.16-0.20% Cr, ≤0.01% Al, and Fe and other unavoidable impurities. The smelting process includes: electric furnace smelting - LF refining - continuous casting, specifically:
[0078] After the electric furnace smelting is completed, sampling and analysis show that the carbon content of the molten steel is 0.386%, the silicon content is 0.004%, the manganese content is 0.04%, the chromium content is 0.020%, and the sulfur content is 0.035%. 198kg of lime, 452kg of ferrosilicon, and 1154kg of ferromanganese are added to the molten steel during the steel tapping process. After the steel tapping is completed, the bottom blowing and stirring of the ladle are turned on, and the bottom blowing argon flow rate is set to 800NL / min. 1002kg of hot residual steel and slag and 480kg of carbon powder are added to the molten steel in turn. After the bottom blowing and stirring last for 14 minutes, the preliminary slag making and deoxidation alloying are completed; the ladle is hoisted into the refining station by a crane. After the ladle arrives at the station, the temperature is sampled and measured, the bottom blowing flow rate is set to 350NL / min, and the electrode is inserted to energize and heat up. The temperature of the molten steel was measured to be 1501℃, the carbon content of the molten steel was 0.804%, the silicon content was 0.177%, the manganese content was 0.78%, the sulfur content was 0.021%, and the aluminum content was 0.0014%. According to the measured composition of the molten steel, 30kg of carbon powder, 33kg of ferrosilicon, 22kg of ferromanganese, 297kg of ferrochrome, and 108kg of fluorite were added. After 4 minutes of power-on, the slag was not melted well and there were lumps on the surface. 80kg of fluorite was added, and slag was melted after 2 minutes; the temperature was measured and sampled again, and the temperature of the molten steel reached 1527℃, the carbon content of the molten steel was 0.83%, the silicon content was 0.192%, the manganese content was 0.791%, the chromium content was 0.176%, the sulfur content was 0.0088%, and the aluminum content was 0.0017%, which met the quality requirements. 60kg of calcium carbide was added to the slag surface, and the bottom blowing argon flow rate was set to 120NL / min for soft stirring for 12 minutes. Then, a crane was used to lift the continuous casting platform for pouring.
[0079] After smelting in Comparative Example 1, the final desulfurization rate was measured to be 75%, and the increased fluorite slag making cost was 564 yuan / furnace.
[0080] Comparative Example 2
[0081] The smelting method of silicon-killed steel hard strand SWRH82B provided in Comparative Example 2 comprises the following steps:
[0082] In an electric furnace short-process steelmaking workshop with a nominal capacity of 100t, the refining and slag forming method of silicon-killed steel hard strand SWRH82B described in the present invention is adopted, the smelting steel type is hard strand SWRH82B, the silicon iron PSi used in the process is 72%, the manganese iron PMn is 66%, and the carbon powder P carbon powder is 96%. In terms of weight percentage, the main components of the hard strand SWRH82B are C 0.81-0.84%, Si 0.18-0.22%, Mn 0.78-0.82%, P ≤0.01%, S ≤0.015%, Cr 0.16-0.20%, Al ≤0.01%, and Fe and other inevitable impurity components. The smelting process includes: electric furnace smelting-LF refining-continuous casting, specifically:
[0083] After the electric furnace smelting is completed, sampling and analysis show that the carbon content of the molten steel is 0.415%, the silicon content is 0.003%, the manganese content is 0.038%, the chromium content is 0.021%, and the sulfur content is 0.052%. 200kg of lime, 455kg of ferrosilicon, and 1160kg of ferromanganese are added to the molten steel during the steel tapping process. After the steel tapping is completed, the bottom blowing and stirring of the ladle are turned on, and the bottom blowing argon flow rate is set to 800NL / min. 1074kg of hot residual steel and slag and 450kg of carbon powder are added to the molten steel in turn. After the bottom blowing and stirring last for 14 minutes, the preliminary slag making and deoxidation alloying are completed; the ladle is hoisted into the refining station by a crane. After the ladle arrives at the station, the temperature is sampled and measured, the bottom blowing flow rate is set to 350NL / min, and the electrode is inserted to energize and heat up. The temperature of the molten steel was measured to be 1498℃, the carbon content of the molten steel was 0.805%, the silicon content was 0.188%, the manganese content was 0.77%, the sulfur content was 0.035%, and the aluminum content was 0.0014%. According to the measured composition of the molten steel, 25kg of carbon powder, 27kg of ferrosilicon, 32kg of ferromanganese, 279kg of ferrochrome, and 122kg of fluorite were added. After 4 minutes of power-on, the slag was not melted well, and there were many agglomerated slags on the surface. 130kg of fluorite was added successively, and the slag melted after 2.5 minutes; the temperature was measured and sampled again, and the temperature of the molten steel reached 1528℃, the carbon content of the molten steel was 0.832%, the silicon content was 0.192%, the manganese content was 0.79%, the chromium content was 0.167%, the sulfur content was 0.0146%, and the aluminum content was 0.0017%, which met the quality requirements. 60kg of calcium carbide was added to the slag surface, and the bottom blowing argon flow rate was set to 120NL / min for soft stirring for 12 minutes. Then, a crane was used to lift the continuous casting platform for pouring.
[0084] After smelting in Comparative Example 2, the final desulfurization rate was measured to be 72%, and the increased fluorite slag making cost was 756 yuan / furnace.
[0085] Comparative Example 3
[0086] The smelting method of silicon-killed steel hard strand SWRH82B provided in Comparative Example 3 comprises the following steps:
[0087] In an electric furnace short-process steelmaking workshop with a nominal capacity of 100t, the refining and slag forming method of silicon-killed steel hard strand SWRH82B described in the present invention is adopted, the smelting steel type is hard strand SWRH82B, and the P of ferrosilicon used in the process is Si The P content of ferromanganese is 72%. Mn The P of toner is 66%. 碳粉The main components of hard steel strand SWRH82B are 0.81-0.84% C, 0.18-0.22% Si, 0.78-0.82% Mn, ≤0.01% P, ≤0.015% S, 0.16-0.20% Cr, ≤0.01% Al, and Fe and other unavoidable impurities. The smelting process includes: electric furnace smelting - LF refining - continuous casting, specifically:
[0088] This embodiment adopts the method of reducing the basicity of the slag and combining the hot circulation of calcium silicate refining slag to promote slag, reduce the amount of lime added for steel tapping, and no fluorite is added during the process. After the electric furnace smelting is completed, sampling and analysis show that the carbon content of the molten steel is 0.427%, the silicon content is 0.012%, the manganese content is 0.058%, the chromium content is 0.045%, and the sulfur content is 0.035%. 125kg of lime, 373kg of ferrosilicon, and 1005kg of ferromanganese are added to the molten steel during the steel tapping process. After the steel tapping is completed, the bottom blowing and stirring of the ladle are turned on, the bottom blowing argon flow rate is set to 800NL / min, and 1038kg of hot residual steel and residual slag and 437kg of carbon powder are added to the molten steel in turn. The bottom blowing and stirring are continued for 12min to complete the preliminary slag making and deoxidation alloying; the ladle is hoisted into the refining station by a crane, and the temperature is measured after the ladle arrives at the station. The bottom blowing flow rate is set to 350 NL / min, and the electrode is inserted to energize and heat up. The temperature of the molten steel was measured to be 1493℃, the carbon content of the molten steel was 0.816%, the silicon content was 0.18%, the manganese content was 0.772%, the sulfur content was 0.028%, and the aluminum content was 0.0015%. According to the measured composition of the molten steel, 20kg of carbon powder, 30kg of ferrosilicon, 30kg of ferromanganese, and 290kg of ferrochrome were added. After 12 minutes of power-on, the slag was poorly melted and there was a small amount of agglomeration on the surface; the temperature was measured and sampled again, and the molten steel temperature reached 1532℃, the carbon content of the molten steel was 0.83%, the silicon content was 0.19%, the manganese content was 0.79%, the chromium content was 0.172%, the sulfur content was 0.0203%, and the aluminum content was 0.0018%, which met the quality requirements. 60kg of calcium carbide was added to the slag surface, and the bottom blowing argon gas flow rate was set to 120NL / min for soft stirring for 12 minutes, and then the continuous casting platform was cast using a crane.
[0089] After smelting in Comparative Example 3, although the slag-forming was promoted by reducing the slag basicity in combination with the hot recycling of calcium silicate refining slag without increasing the slag-making cost, the slag-forming time was long, the slag basicity was relatively low, and the desulfurization effect was poor; the final desulfurization rate was measured to be 42%, and the sulfur content in the finished molten steel was 0.0203%, which did not meet the quality standards and was judged to be scrapped.
[0090] Comparative Example 4
[0091] Comparative Example 4 uses pre-melted synthetic slag to accelerate slagging. The pre-melted synthetic slag is a mixture of lime, dicalcium silicate, fluorite, etc., and is obtained by high-temperature melting, crushing and screening, and has a high cost.
[0092] The smelting method of silicon-killed steel hard strand SWRH82B provided in Comparative Example 4 comprises the following steps:
[0093] In an electric furnace short-process steelmaking workshop with a nominal capacity of 100t, the refining and slag forming method of silicon-killed steel hard strand SWRH82B described in the present invention is adopted, the smelting steel type is hard strand SWRH82B, and the P of ferrosilicon used in the process is Si The P content of ferromanganese is 72%. Mn The P of toner is 66%. 碳粉 The main components of hard steel strand SWRH82B are 0.81-0.84% C, 0.18-0.22% Si, 0.78-0.82% Mn, ≤0.01% P, ≤0.015% S, 0.16-0.20% Cr, ≤0.01% Al, and Fe and other unavoidable impurities. The smelting process includes: electric furnace smelting - LF refining - continuous casting, specifically:
[0094] After the electric furnace smelting is completed, sampling and analysis show that the carbon content of the molten steel is 0.43%, the silicon content is 0.02%, the manganese content is 0.06%, the chromium content is 0.05%, and the sulfur content is 0.035%. 185kg of lime, 377kg of ferrosilicon, and 1008kg of ferromanganese are added to the molten steel during the steel tapping process. After the steel tapping is completed, the bottom blowing and stirring of the ladle are turned on, and the bottom blowing argon flow rate is set to 800NL / min. 1007kg of hot residual steel and slag, 815kg of pre-melted synthetic slag, and 435kg of carbon powder are added to the molten steel in turn. After the bottom blowing and stirring last for 12 minutes, the preliminary slag making and deoxidation alloying are completed; the ladle is hoisted into the refining station by a crane. After the ladle arrives at the station, the temperature is sampled and measured, the bottom blowing flow rate is set to 350NL / min, and the electrode is inserted to energize and heat up. The temperature of the molten steel was measured to be 1492℃, the carbon content of the molten steel was 0.81%, the silicon content was 0.184%, the manganese content was 0.773%, the sulfur content was 0.022%, and the aluminum content was 0.0015%. According to the measured composition of the molten steel, 20kg of carbon powder, 27kg of ferrosilicon, 28kg of ferromanganese, and 290kg of ferrochrome were added. After 6 minutes of power-on, the slag melted well, and there was no agglomeration on the surface. During the entire slag-melting process; the temperature was measured and sampled again, and the molten steel temperature reached 1528℃, the carbon content of the molten steel was 0.833%, the silicon content was 0.191%, the manganese content was 0.794%, the chromium content was 0.17%, the sulfur content was 0.006%, and the aluminum content was 0.0018%, which met the quality requirements. 60kg of calcium carbide was added to the slag surface, and the bottom blowing argon gas flow rate was set to 120NL / min for soft stirring for 12 minutes, and then the continuous casting platform was cast using a crane.
[0095] After smelting in Comparative Example 4, the final desulfurization rate was measured to be 83%, and the increased slag making cost was 1,630 yuan / furnace.
[0096] Next are six sets of examples. Example
[0097] Example 1
[0098] A calcium aluminate synthetic slag and a preparation method thereof provided in Example 1 specifically include the following steps:
[0099] The calcium aluminate refining slag is recovered in a converter with a nominal capacity of 180t. The recovered refining slag is the remaining refining waste slag after smelting J30BDGB0 using conventional processes in the field. The silicon content of steel grade J30BDGB0 is ≤0.03%. The smelting process of steel grade J30BDGB0 includes: KR pre-desulfurization-converter smelting-LF refining-continuous casting. The sulfur content of the molten iron used for smelting J30BDGB0 after KR pre-desulfurization is 0.0024%. After the pouring of steel grade J30BDGB0 is completed, the calcium aluminate refining slag in the ladle is poured into a slag basin and cooled to room temperature. After pouring out, it is crushed into powder slag with a particle size of less than 6mm by a crusher, and iron is removed by magnetic separation; the lime and bauxite are crushed to a particle size of less than 6mm; the processed calcium aluminate refining slag, lime and bauxite are mixed evenly according to the mass ratio of 8:0.7:1.3 to obtain. In terms of mass percentage, the main components of the obtained calcium aluminate synthetic slag are CaO of 61%, Al2O3 of 32%, the total amount of FeO and MnO of 1.2%, SiO2 of 2.8%, S of 0.06% and other inevitable impurities.
[0100] Example 1 also provides a method for smelting silicon-killed steel hard strand SWRH82B by applying calcium aluminate synthetic slag, comprising the following steps:
[0101] In an electric furnace short-process steelmaking workshop with a nominal capacity of 100t, the refining and slag forming method of silicon-killed steel hard strand SWRH82B described in the present invention is adopted, the smelting steel type is hard strand SWRH82B, and the P of ferrosilicon used in the process is Si The P content of ferromanganese is 72%. Mn The P of toner is 66%. 碳粉 The main components of hard steel strand SWRH82B are 0.81-0.84% C, 0.18-0.22% Si, 0.78-0.82% Mn, ≤0.01% P, ≤0.015% S, 0.16-0.20% Cr, ≤0.01% Al, and Fe and other unavoidable impurities. The smelting process includes: electric furnace smelting - LF refining - continuous casting, specifically:
[0102] After the electric furnace smelting is completed, sampling and analysis show that the carbon content of the molten steel is 0.43%, the silicon content is 0.01%, the manganese content is 0.06%, the chromium content is 0.05%, and the sulfur content is 0.035%. 188kg of lime, 374kg of ferrosilicon, and 1003kg of ferromanganese are added to the molten steel during the steel tapping process. After the steel tapping is completed, the bottom blowing and stirring of the ladle are turned on, and the bottom blowing argon flow rate is set to 800NL / min. 1058kg of hot residual steel and slag, 300kg of calcium aluminate synthetic slag, and 432kg of carbon powder are added to the molten steel in turn. After the bottom blowing and stirring last for 12 minutes, the preliminary slag making and deoxidation alloying are completed; the ladle is hoisted into the refining station by a crane. After the ladle arrives at the station, the temperature is sampled and measured, the bottom blowing flow rate is set to 350NL / min, and the electrode is inserted to energize and heat up. The temperature of the molten steel was measured to be 1490℃, the carbon content of the molten steel was 0.81%, the silicon content was 0.18%, the manganese content was 0.77%, the sulfur content was 0.028%, and the aluminum content was 0.0015%. According to the measured composition of the molten steel, 20kg of carbon powder, 30kg of ferrosilicon, 30kg of ferromanganese, and 292kg of ferrochrome were added. After 8 minutes of power-on, the slag melted well and there was no agglomeration on the surface; the temperature was measured and sampled again, and the molten steel temperature reached 1532℃, the carbon content of the molten steel was 0.83%, the silicon content was 0.19%, the manganese content was 0.79%, the chromium content was 0.172%, the sulfur content was 0.006%, and the aluminum content was 0.0018%, which met the quality requirements. 60kg of calcium carbide was added to the slag surface, and the bottom blowing argon gas flow rate was set to 120NL / min for soft stirring for 12 minutes, and then the continuous casting platform was cast using a crane.
[0103] Example 1 During the entire smelting process, 300 kg of calcium aluminate synthetic slag was used, and no fluorite was added. The final desulfurization rate reached 83%, the slagging time lasted 4.5 minutes, and the increased slag making cost was 90 yuan / furnace.
[0104] Example 2
[0105] A calcium aluminate synthetic slag and a preparation method thereof provided in Example 2 specifically include the following steps:
[0106] The calcium aluminate refining slag is recovered in a converter with a nominal capacity of 180t. The recovered refining slag is the remaining refining waste slag after smelting J30BDGB0 using conventional processes in the field. The silicon content of steel grade J30BDGB0 is ≤0.03%. The smelting process of steel grade J30BDGB0 includes: KR pre-desulfurization-converter smelting-LF refining-continuous casting. The sulfur content of the molten iron used for smelting J30BDGB0 after KR pre-desulfurization is 0.0041%. After the pouring of steel grade J30BDGB0 is completed, the calcium aluminate refining slag in the ladle is poured into a slag basin and cooled to room temperature. After pouring out, it is crushed into powder slag with a particle size of less than 6mm by a crusher, and iron is removed by magnetic separation; the lime and bauxite are crushed to a particle size of less than 6mm; the processed calcium aluminate refining slag, lime and bauxite are mixed evenly according to the mass ratio of 8:1.5:0.5 to obtain. In terms of mass percentage, the main components of the obtained calcium aluminate synthetic slag are CaO of 63%, Al2O3 of 31%, the total amount of FeO and MnO of 1.1%, SiO2 of 2.5%, S of 0.04% and other inevitable impurities.
[0107] Example 2 also provides a method for smelting silicon-killed steel hard strand SWRH82B by applying calcium aluminate synthetic slag, comprising the following steps:
[0108] In an electric furnace short-process steelmaking workshop with a nominal capacity of 100t, the refining and slag forming method of silicon-killed steel hard strand SWRH82B described in the present invention is adopted, the smelting steel type is hard strand SWRH82B, the silicon iron PSi used in the process is 72%, the manganese iron PMn is 66%, and the carbon powder P carbon powder is 96%. In terms of weight percentage, the main components of the hard strand SWRH82B are C 0.81-0.84%, Si 0.18-0.22%, Mn 0.78-0.82%, P ≤0.01%, S ≤0.015%, Cr 0.16-0.20%, Al ≤0.01%, and Fe and other inevitable impurity components. The smelting process includes: electric furnace smelting-LF refining-continuous casting, specifically:
[0109] After the electric furnace smelting is completed, sampling and analysis show that the carbon content of the molten steel is 0.35%, the silicon content is 0.004%, the manganese content is 0.049%, the chromium content is 0.025%, and the sulfur content is 0.025%. 152kg of lime, 455kg of ferrosilicon, and 1138kg of ferromanganese are added to the molten steel during the steel tapping process. After the steel tapping is completed, the bottom blowing and stirring of the ladle are turned on, and the bottom blowing argon flow rate is set to 800NL / min. 989kg of hot residual steel and slag, 180kg of calcium aluminate synthetic slag, and 520kg of carbon powder are added to the molten steel in turn. After the bottom blowing and stirring last for 12 minutes, the preliminary slag making and deoxidation alloying are completed; the ladle is hoisted into the refining station by a crane. After the ladle arrives at the station, the temperature is sampled and measured, the bottom blowing flow rate is set to 350NL / min, and the electrode is inserted to energize and heat up. The temperature of the molten steel was measured to be 1495℃, the carbon content of the molten steel was 0.80%, the silicon content was 0.19%, the manganese content was 0.76%, the sulfur content was 0.014%, and the aluminum content was 0.001%. According to the measured composition of the molten steel, 30kg of carbon powder, 10kg of ferrosilicon, 40kg of ferromanganese, and 285kg of ferrochrome were added. After 8 minutes of power-on, the slag melted well and there was no agglomeration on the surface; the temperature was measured and sampled again, and the molten steel temperature reached 1532℃, the carbon content of the molten steel was 0.825%, the silicon content was 0.213%, the manganese content was 0.805%, the chromium content was 0.17%, the sulfur content was 0.0033%, and the aluminum content was 0.0015%, which met the quality requirements. 60kg of calcium carbide was added to the slag surface, and the bottom blowing argon gas flow rate was set to 120NL / min for soft stirring for 13 minutes, and then the continuous casting platform was cast using a crane.
[0110] Example 2 During the entire smelting process, 180 kg of calcium aluminate synthetic slag was used, and no fluorite was added. The final desulfurization rate reached 87%, the slagging time lasted 5.5 minutes, and the increased slag making cost was 54 yuan / furnace.
[0111] Example 3
[0112] A calcium aluminate synthetic slag and a preparation method thereof provided in Example 3 specifically include the following steps:
[0113] The calcium aluminate refining slag is recovered in a converter with a nominal capacity of 180t. The recovered refining slag is the remaining refining waste slag after smelting J30BDGB0 using conventional processes in the field. The silicon content of steel grade J30BDGB0 is ≤0.03%. The smelting process of steel grade J30BDGB0 includes: KR pre-desulfurization-converter smelting-LF refining-continuous casting. The sulfur content of the molten iron used for smelting J30BDGB0 after KR pre-desulfurization is 0.0028%. After the pouring of steel grade J30BDGB0 is completed, the calcium aluminate refining slag in the ladle is poured into a slag basin and cooled to room temperature. After pouring out, it is crushed into powder slag with a particle size of less than 6mm by a crusher, and iron is removed by magnetic separation; the lime and bauxite are crushed to a particle size of less than 6mm; the processed calcium aluminate refining slag, lime and bauxite are mixed evenly according to a mass ratio of 8:1:1 to obtain. In terms of mass percentage, the main components of the obtained calcium aluminate synthetic slag are CaO of 61%, Al2O3 of 32%, the total amount of FeO and MnO of 0.9%, SiO2 of 2.2%, S of 0.03% and other inevitable impurities.
[0114] Example 3 also provides a method for smelting silicon-killed steel hard strand SWRH82B by applying calcium aluminate synthetic slag, comprising the following steps:
[0115] In an electric furnace short-process steelmaking workshop with a nominal capacity of 100t, the refining and slag forming method of silicon-killed steel hard strand SWRH82B described in the present invention is adopted, the smelting steel type is hard strand SWRH82B, the silicon iron PSi used in the process is 72%, the manganese iron PMn is 66%, and the carbon powder P carbon powder is 96%. In terms of weight percentage, the main components of the hard strand SWRH82B are C 0.81-0.84%, Si 0.18-0.22%, Mn 0.78-0.82%, P ≤0.01%, S ≤0.015%, Cr 0.16-0.20%, Al ≤0.01%, and Fe and other inevitable impurity components. The smelting process includes: electric furnace smelting-LF refining-continuous casting, specifically:
[0116] After the electric furnace smelting is completed, sampling and analysis show that the carbon content of the molten steel is 0.41%, the silicon content is 0.002%, the manganese content is 0.039%, the chromium content is 0.023%, and the sulfur content is 0.052%. 255kg of lime, 459kg of ferrosilicon, and 1153kg of ferromanganese are added to the molten steel during the steel tapping process. After the steel tapping is completed, the bottom blowing and stirring of the ladle are turned on, and the bottom blowing argon flow rate is set to 800NL / min. 1003kg of hot residual steel and slag, 456kg of calcium aluminate synthetic slag, and 455kg of carbon powder are added to the molten steel in turn. After the bottom blowing and stirring last for 14 minutes, the preliminary slag making and deoxidation alloying are completed; the ladle is hoisted into the refining station by a crane. After the ladle arrives at the station, the temperature is sampled and measured, the bottom blowing flow rate is set to 350NL / min, and the electrode is inserted to energize and heat up. The temperature of the molten steel was measured to be 1498℃, the carbon content of the molten steel was 0.802%, the silicon content was 0.187%, the manganese content was 0.772%, the sulfur content was 0.028%, and the aluminum content was 0.0015%. According to the measured composition of the molten steel, 25kg of carbon powder, 30kg of ferrosilicon, 30kg of ferromanganese, and 282kg of ferrochrome were added. After 7.5 minutes of power-on, the slag melted well and there was no agglomeration on the surface; the temperature was measured and sampled again, and the molten steel temperature reached 1528℃, the carbon content of the molten steel was 0.83%, the silicon content was 0.194%, the manganese content was 0.791%, the chromium content was 0.166%, the sulfur content was 0.0054%, and the aluminum content was 0.0017%, which met the quality requirements. 60kg of calcium carbide was added to the slag surface, and the bottom blowing argon gas flow rate was set to 120NL / min for soft stirring for 12 minutes, and then the continuous casting platform was cast using a crane.
[0117] Example 3 During the entire smelting process, 456 kg of calcium aluminate synthetic slag was used, and no fluorite was added. The final desulfurization rate reached 90%, the slagging time lasted for 4 minutes, and the increased slag making cost was 136.8 yuan / furnace.
[0118] Example 4
[0119] A calcium aluminate synthetic slag and a preparation method thereof provided in Example 4 specifically comprises the following steps:
[0120] The calcium aluminate refining slag is recovered in a converter with a nominal capacity of 180t. The recovered refining slag is the remaining refining waste slag after smelting J30BDGB0 using conventional processes in the field. The silicon content of steel grade J30BDGB0 is ≤0.03%. The smelting process of steel grade J30BDGB0 includes: KR pre-desulfurization-converter smelting-LF refining-continuous casting. The sulfur content of the molten iron used for smelting J30BDGB0 after KR pre-desulfurization is 0.0033%. After the pouring of steel grade J30BDGB0 is completed, the calcium aluminate refining slag in the ladle is poured into a slag basin and cooled to room temperature. After pouring out, it is crushed into powder slag with a particle size of less than 6mm by a crusher, and iron is removed by magnetic separation; the lime and bauxite are crushed to a particle size of less than 6mm; the processed calcium aluminate refining slag, lime and bauxite are mixed evenly according to a mass ratio of 8:1:1 to obtain. In terms of mass percentage, the main components of the obtained calcium aluminate synthetic slag include 61% CaO, 33% Al2O3, 1% FeO and MnO in total, 2.7% SiO2, 0.04% S and other inevitable impurities.
[0121] Example 4 also provides a method for smelting silicon-killed steel hard strand SWRH82B by applying calcium aluminate synthetic slag, comprising the following steps:
[0122] In an electric furnace short-process steelmaking workshop with a nominal capacity of 100t, the refining and slag forming method of silicon-killed steel hard strand SWRH82B described in the present invention is adopted, the smelting steel type is hard strand SWRH82B, the silicon iron PSi used in the process is 72%, the manganese iron PMn is 66%, and the carbon powder P carbon powder is 96%. In terms of weight percentage, the main components of the hard strand SWRH82B are C 0.81-0.84%, Si 0.18-0.22%, Mn 0.78-0.82%, P ≤0.01%, S ≤0.015%, Cr 0.16-0.20%, Al ≤0.01%, and Fe and other inevitable impurity components. The smelting process includes: electric furnace smelting-LF refining-continuous casting, specifically:
[0123] After the electric furnace smelting is completed, sampling and analysis show that the carbon content of the molten steel is 0.31%, the silicon content is 0.003%, the manganese content is 0.045%, the chromium content is 0.021%, and the sulfur content is 0.042%. 162kg of lime, 456kg of ferrosilicon, and 1143kg of ferromanganese are added to the molten steel during the steel tapping process. After the steel tapping is completed, the bottom blowing and stirring of the ladle are turned on, and the bottom blowing argon flow rate is set to 800NL / min. 993kg of hot residual steel and slag, 367kg of calcium aluminate synthetic slag, and 564kg of carbon powder are added to the molten steel in turn. After the bottom blowing and stirring last for 13 minutes, the preliminary slag making and deoxidation alloying are completed; the ladle is hoisted into the refining station by a crane. After the ladle arrives at the station, the temperature is sampled and measured, the bottom blowing flow rate is set to 350NL / min, and the electrode is inserted to energize and heat up. The temperature of the molten steel was measured to be 1494℃, the carbon content of the molten steel was 0.815%, the silicon content was 0.183%, the manganese content was 0.774%, the sulfur content was 0.017%, and the aluminum content was 0.0012%. According to the measured composition of the molten steel, 20kg of carbon powder, 18kg of ferrosilicon, 35kg of ferromanganese, and 273kg of ferrochrome were added. After 8 minutes of power-on, the slag melted well and there was no agglomeration on the surface; the temperature was measured and sampled again, and the molten steel temperature reached 1532℃, the carbon content of the molten steel was 0.828%, the silicon content was 0.182%, the manganese content was 0.79%, the chromium content was 0.172%, the sulfur content was 0.0062%, and the aluminum content was 0.0016%, which met the quality requirements. 60kg of calcium carbide was added to the slag surface, and the bottom blowing argon gas flow rate was set to 120NL / min for soft stirring for 12 minutes, and then the continuous casting platform was cast using a crane.
[0124] Example 4 During the entire smelting process, 367 kg of calcium aluminate synthetic slag was used, and no fluorite was added. The final desulfurization rate reached 85%, the slagging time lasted for 4 minutes, and the increased slag making cost was 110.1 yuan / furnace.
[0125] Example 5
[0126] A calcium aluminate synthetic slag and a preparation method thereof provided in Example 5 specifically include the following steps:
[0127] The calcium aluminate refining slag is recovered in a converter with a nominal capacity of 180t. The recovered refining slag is the remaining refining waste slag after smelting J30BDGB0 using conventional processes in the field. The silicon content of steel grade J30BDGB0 is ≤0.03%. The smelting process of steel grade J30BDGB0 includes: KR pre-desulfurization-converter smelting-LF refining-continuous casting. The sulfur content of the molten iron used for smelting J30BDGB0 after KR pre-desulfurization is 0.0012%. After the pouring of steel grade J30BDGB0 is completed, the calcium aluminate refining slag in the ladle is poured into a slag basin and cooled to room temperature. After pouring out, it is crushed into powder slag with a particle size of less than 6mm by a crusher, and iron is removed by magnetic separation; the lime and bauxite are crushed to a particle size of less than 6mm; the processed calcium aluminate refining slag, lime and bauxite are mixed evenly according to the mass ratio of 8:0.5:1.5 to obtain. In terms of mass percentage, the main components of the obtained calcium aluminate synthetic slag are CaO of 60%, Al2O3 of 33%, the total amount of FeO and MnO of 1.3%, SiO2 of 2.7%, S of 0.02% and other inevitable impurities.
[0128] Example 5 also provides a method for smelting silicon-killed steel hard strand SWRH82B by applying calcium aluminate synthetic slag, comprising the following steps:
[0129] In an electric furnace short-process steelmaking workshop with a nominal capacity of 100t, the refining and slag forming method of silicon-killed steel hard strand SWRH82B described in the present invention is adopted, the smelting steel type is hard strand SWRH82B, the silicon iron PSi used in the process is 72%, the manganese iron PMn is 66%, and the carbon powder P carbon powder is 96%. In terms of weight percentage, the main components of the hard strand SWRH82B are C 0.81-0.84%, Si 0.18-0.22%, Mn 0.78-0.82%, P ≤0.01%, S ≤0.015%, Cr 0.16-0.20%, Al ≤0.01%, and Fe and other inevitable impurity components. The smelting process includes: electric furnace smelting-LF refining-continuous casting, specifically:
[0130] After the electric furnace smelting is completed, sampling and analysis show that the carbon content of the molten steel is 0.39%, the silicon content is 0.003%, the manganese content is 0.041%, the chromium content is 0.021%, and the sulfur content is 0.035%. 150kg of lime, 456kg of ferrosilicon, and 1150kg of ferromanganese are added to the molten steel during the steel tapping process. After the steel tapping is completed, the bottom blowing and stirring of the ladle are turned on, and the bottom blowing argon flow rate is set to 800NL / min. 1011kg of hot residual steel and slag, 278kg of calcium aluminate synthetic slag, and 476kg of carbon powder are added to the molten steel in turn. After the bottom blowing and stirring last for 14 minutes, the preliminary slag making and deoxidation alloying are completed; the ladle is hoisted into the refining station by a crane. After the ladle arrives at the station, the temperature is sampled and measured, the bottom blowing flow rate is set to 350NL / min, and the electrode is inserted to energize and heat up. The temperature of the molten steel was measured to be 1501℃, the carbon content of the molten steel was 0.805%, the silicon content was 0.178%, the manganese content was 0.782%, the sulfur content was 0.014%, and the aluminum content was 0.0013%. According to the measured composition of the molten steel, 30kg of carbon powder, 37kg of ferrosilicon, 25kg of ferromanganese, and 299kg of ferrochrome were added. After 6 minutes of power-on, the slag melted well and there was no agglomeration on the surface; the temperature was measured and sampled again, and the molten steel temperature reached 1527℃, the carbon content of the molten steel was 0.832%, the silicon content was 0.196%, the manganese content was 0.798%, the chromium content was 0.177%, the sulfur content was 0.004%, and the aluminum content was 0.0016%, which met the quality requirements. 60kg of calcium carbide was added to the slag surface, and the bottom blowing argon gas flow rate was set to 120NL / min for soft stirring for 12 minutes, and then the continuous casting platform was cast using a crane.
[0131] Example 5 During the entire smelting process, 278 kg of calcium aluminate synthetic slag was used, and no fluorite was added. The final desulfurization rate reached 89%, the slagging time lasted 4.5 minutes, and the increased slag making cost was 83.4 yuan / furnace.
[0132] Example 6
[0133] A calcium aluminate synthetic slag and a preparation method thereof provided in Example 6 specifically comprises the following steps:
[0134] The calcium aluminate refining slag is recovered in a converter with a nominal capacity of 180t. The recovered refining slag is the remaining refining waste slag after smelting J30BDGB0 using conventional processes in the field. The silicon content of steel grade J30BDGB0 is ≤0.03%. The smelting process of steel grade J30BDGB0 includes: KR pre-desulfurization-converter smelting-LF refining-continuous casting. The sulfur content of the molten iron used for smelting J30BDGB0 after KR pre-desulfurization is 0.0043%. After the pouring of steel grade J30BDGB0 is completed, the calcium aluminate refining slag in the ladle is poured into a slag basin and cooled to room temperature. After pouring out, it is crushed into powder slag with a particle size of less than 6mm by a crusher, and iron is removed by magnetic separation; the lime and bauxite are crushed to a particle size of less than 6mm; the processed calcium aluminate refining slag, lime and bauxite are mixed evenly according to the mass ratio of 8:1.5:0.5 to obtain. In terms of mass percentage, the main components of the obtained calcium aluminate synthetic slag are CaO of 64%, Al2O3 of 30%, the total amount of FeO and MnO of 1.2%, SiO2 of 2.3%, S of 0.04% and other inevitable impurities.
[0135] Example 6 also provides a method for smelting silicon-killed steel hard strand SWRH82B by applying calcium aluminate synthetic slag, comprising the following steps:
[0136] In an electric furnace short-process steelmaking workshop with a nominal capacity of 100t, the refining and slag forming method of silicon-killed steel hard strand SWRH82B described in the present invention is adopted, the smelting steel type is hard strand SWRH82B, the silicon iron PSi used in the process is 72%, the manganese iron PMn is 66%, and the carbon powder P carbon powder is 96%. In terms of weight percentage, the main components of the hard strand SWRH82B are C 0.81-0.84%, Si 0.18-0.22%, Mn 0.78-0.82%, P ≤0.01%, S ≤0.015%, Cr 0.16-0.20%, Al ≤0.01%, and Fe and other inevitable impurity components. The smelting process includes: electric furnace smelting-LF refining-continuous casting, specifically:
[0137] After the electric furnace smelting is completed, sampling and analysis show that the carbon content of the molten steel is 0.33%, the silicon content is 0.004%, the manganese content is 0.042%, the chromium content is 0.021%, and the sulfur content is 0.030%. 164kg of lime, 457kg of ferrosilicon, and 1149kg of ferromanganese are added to the molten steel during the steel tapping process. After the steel tapping is completed, the bottom blowing and stirring of the ladle are turned on, and the bottom blowing argon flow rate is set to 800NL / min. 1102kg of hot residual steel and slag, 261kg of calcium aluminate synthetic slag, and 543kg of carbon powder are added to the molten steel in turn. After the bottom blowing and stirring last for 11 minutes, the preliminary slag making and deoxidation alloying are completed; the ladle is hoisted into the refining station by a crane. After the ladle arrives at the station, the temperature is sampled and measured, the bottom blowing flow rate is set to 350NL / min, and the electrode is inserted to energize and heat up. The temperature of the molten steel was measured to be 1487℃, the carbon content of the molten steel was 0.814%, the silicon content was 0.187%, the manganese content was 0.772%, the sulfur content was 0.015%, and the aluminum content was 0.0017%. According to the measured composition of the molten steel, 20kg of carbon powder, 21kg of ferrosilicon, 28kg of ferromanganese, and 287kg of ferrochrome were added. After 8 minutes of power-on, the slag melted well and there was no agglomeration on the surface; the temperature was measured and sampled again, and the molten steel temperature reached 1532℃, the carbon content of the molten steel was 0.82%, the silicon content was 0.191%, the manganese content was 0.81%, the chromium content was 0.169%, the sulfur content was 0.005%, and the aluminum content was 0.0016%, which met the quality requirements. 60kg of calcium carbide was added to the slag surface, and the bottom blowing argon gas flow rate was set to 120NL / min for soft stirring for 12 minutes, and then the continuous casting platform was cast using a crane.
[0138] Example 6 During the entire smelting process, 261 kg of calcium aluminate synthetic slag was used, and no fluorite was added. The final desulfurization rate reached 83%, the slagging time lasted 4.5 minutes, and the increased slag making cost was 78.3 yuan / furnace.
[0139] The data of the six groups of embodiments and the four groups of comparative examples are visually compared through the same table, as shown in Table 1:
[0140] Table 1 Technical and economic indicators of this application and integrated data of comparative examples
[0141]
[0142] Through the comparison and verification of the above-mentioned embodiments and comparative examples, the method for preparing calcium aluminate synthetic slag proposed in the present application realizes the secondary utilization of aluminum-killed steel refining waste slag, and solves the problem of high production cost of traditional synthetic slag. The present application adopts a method of combining calcium aluminate synthetic slag to produce low-melting-point CaO-Al2O3-SiO2-MgO quaternary slag and heat recycling of surplus steel slag to better deal with the relationship between the basicity of silicon-killed steel hard strand refining slag, C / A and molten steel desulfurization, aluminum content control and casting performance. It can not only meet the basic requirements of silicon-killed steel refining and desulfurization with a finished product sulfur content of less than 0.01%, but also ensure that the aluminum content of the finished molten steel is ≤0.005%, meeting the product performance and casting performance requirements, and effectively controlling the smelting risk of CaO-Al2O3-SiO2-MgO quaternary refining of silicon-killed steel. The CaO-Al2O3-SiO2-MgO quaternary refining slag replaces fluorite to achieve rapid slag reduction and efficient desulfurization, solving the problem of high smelting cost and pollution caused by high fluorite consumption in the high carbon steel refining process.
[0143] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as generally understood by those skilled in the art to which this application belongs. It should also be understood that terms such as those defined in common dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless defined as herein.
[0144] The meaning of "and / or" described in this application means that the situations where each exists alone or both exist at the same time are included.
[0145] The term “connection” as used in this application may mean a direct connection between components or an indirect connection between components via other components.
[0146] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A calcium aluminate synthetic slag, characterized in that: Including calcium aluminate refining slag produced in the secondary refining process of aluminum killed steel; using aluminum killed steel refining slag as raw material, and using it for refining and slag making of silicon killed steel series; It also includes lime and bauxite, wherein the mass ratio of calcium aluminate refining slag, lime and bauxite is 8:0.5:1.5-8:1.5:0.5; In the calcium aluminate synthetic slag formed by mixing calcium aluminate refining slag, lime and bauxite, according to mass fraction, CaO is 60-65%, Al2O3 is 30-35%, the total amount of FeO and MnO is ≤2%, SiO2 is ≤3%, and S is ≤0.1%.
2. The method for preparing calcium aluminate synthetic slag according to claim 1, characterized in that: The specific steps include: Step S1: recovering calcium aluminate refining slag produced during the secondary refining process of aluminum killed steel; Step S2: cooling the recovered calcium aluminate refined slag to room temperature, crushing it to form powder slag with a particle size less than or equal to 6 mm, and removing iron from the calcium aluminate refined slag powder slag by magnetic separation; Step S3: Select lime and bauxite, and crush the lime and bauxite to form powder residue with a particle size less than or equal to 6 mm; Step S4: The calcium aluminate refining slag after magnetic separation in step S2, lime and bauxite are uniformly mixed in a mass ratio of 8:0.5:1.5-8:1.5:0.5 to form calcium aluminate synthetic slag.
3. The method for preparing calcium aluminate synthetic slag according to claim 2, characterized in that: The recovered calcium aluminate refined slag has a sulfur content of ≤0.005% after pre-desulfurization of molten iron in the smelting process of aluminum-killed steel.
4. The method for preparing calcium aluminate synthetic slag according to claim 3, characterized in that: The silicon content in the aluminum-killed steel product formed by the recycled calcium aluminate refined slag after the aluminum-killed steel smelting process is ≤0.3%.
5. A method for smelting high carbon steel using the calcium aluminate synthetic slag according to claim 1, characterized in that: The specific steps include: Step S1: After the smelting in the primary furnace is completed, lime and deoxidation alloy are added to the molten steel in the ladle during the steel tapping process; Step S2: after the ladle is finished tapping, the ladle bottom blowing and stirring are started, and hot excess steel and slag are added to the molten steel in the ladle in sequence, followed by adding carbon powder and the calcium aluminate synthetic slag; wherein the amount of the calcium aluminate synthetic slag added is determined according to the sulfur content of the molten steel tapped from the primary furnace in step S1; In step S2, hot excess steel slag is added to the molten steel in the ladle in sequence. Specifically, the ladle filled with hot excess steel slag is set as ladle No. 1, the ladle hoisted from the refining process is set as ladle No. 2, the ladle that completes the secondary refining process through power-on charging in step S4 is ladle No. 3, and the ladle from which the molten steel in the primary refining furnace is tapped is ladle No. 4, then the hot excess steel slag of ladle No. 1 is poured into ladle No. 4; The amount of carbon powder added is: m 碳粉 =(P C成品 -P C初始 )×1000×m 钢水 ×85% / η C / P 碳粉 , Among them, m 碳粉 P is the amount of carbon powder added to steel, kg; C成品 is the carbon content of the finished steel product, %; P C初始 is the carbon content of molten steel, %; m 钢水 is the weight of molten steel; C is the carbon recovery coefficient, ranging from 0.8 to 1.0; P 碳粉 is the carbon content in the carbon powder, %; The amount of calcium aluminate synthetic slag added is determined according to the sulfur content of the molten steel tapped from the primary furnace in step S1, specifically: When the sulfur content of molten steel is ≤0.03%, add 1.5kg / t<the weight of calcium aluminate synthetic slag ≤2.5kg / t; When the sulfur content of molten steel is 0.03%<≤0.05%, add 2.5kg / t<the weight of calcium aluminate synthetic slag ≤4kg / t; When the sulfur content of molten steel is greater than 0.05%, add 4kg / t<5kg / t of calcium aluminate synthetic slag and add 0.5-1.5kg / t of lime; Step S3: The ladle enters the refining process, firstly, sampling and temperature measurement are carried out, refining bottom blowing and stirring are started, and then electrodes are inserted into the ladle to energize and heat up; Step S4: According to the composition of the molten steel sampled and measured in step S3, alloy and carbon powder are added to adjust the composition of the molten steel to within the target composition range, calcium carbide is added to the slag surface of the molten steel, and the continuous casting process is implemented after sufficient soft stirring.
6. The method for smelting high carbon steel using the calcium aluminate synthetic slag according to claim 5, characterized in that: In step S1, the amount of lime added to the molten steel in the ladle during the steel tapping process is 1-3 kg / t; The deoxidizing alloys added are ferrosilicon and ferromanganese, and the amount of ferrosilicon added is: m 硅铁 =(P Si成品 -P Si初始 )×1000×m 钢水 / η Si / P 硅铁 , The amount of ferromanganese added is: m 锰铁 =(P Mn成品 -P Mn初始 )×1000×m 钢水 / η Mn / P 锰铁 , Among them, m 硅铁 is the amount of ferrosilicon added during steelmaking, kg; P Si成品 is the silicon content of the finished steel product, %; P Si初始 is the silicon content of molten steel, %; m 钢水 is the weight of molten steel, t; η Si is the silicon recovery coefficient, ranging from 0.5 to 0.8; P 硅铁 is the silicon content in ferrosilicon, %; m 锰铁 is the amount of ferromanganese added during steelmaking, kg; P Mn成品 is the manganese content of the finished steel product, %; P Mn初始 is the manganese content of molten steel, %; η Mn is the manganese recovery coefficient, ranging from 1.0 to 1.2; P 锰铁 is the manganese content in ferromanganese, %.
7. The method for smelting high carbon steel using the calcium aluminate synthetic slag according to claim 5, characterized in that: In step S2, the amount of calcium aluminate synthetic slag added is determined according to the sulfur content of the molten steel tapped from the primary furnace in step S1, specifically: When the sulfur content of molten steel is ≤0.03%, add 1.5kg / t<the weight of calcium aluminate synthetic slag ≤2.5kg / t; When the sulfur content of molten steel is 0.03%<≤0.05%, add 2.5kg / t<the weight of calcium aluminate synthetic slag ≤4kg / t; When the sulfur content of molten steel is greater than 0.05%, add 4kg / t<5kg / t of calcium aluminate synthetic slag and add 0.5-1.5kg / t of lime.
8. The method for smelting high carbon steel using the calcium aluminate synthetic slag according to claim 5, characterized in that: In step S2, after the ladle is finished tapping, the ladle bottom blowing and stirring are started, wherein the ladle bottom blowing and stirring lasts for 10-15 minutes, and the bottom blowing argon flow rate is 600-900NL / min.
9. The method for smelting high carbon steel using the calcium aluminate synthetic slag according to claim 5, characterized in that: In step S3, during refining bottom blowing and stirring, the argon flow rate is 300-400NL / min.
10. The method for smelting high carbon steel using the calcium aluminate synthetic slag according to claim 5, characterized in that: In step S4, during soft stirring, the argon flow rate is 50-150 NL / min.
Citation Information
Patent Citations
Recycling method for refining slag of ladle refining furnace
CN107326149A
Production method for silicon deoxidation low-sulfur high-carbon steel
CN107904355A