Oil-absorbing polyurethane foam material and preparation method thereof

By preparing oil-absorbing polyurethane foam materials with modified monomers and metal-organic structures, the problem of polyurethane foam water absorption affecting oil absorption efficiency is solved, high-efficiency oil absorption and low water absorption are achieved, and the effect of oily wastewater treatment is improved.

CN118206800BActive Publication Date: 2024-10-18YANGZHOU SANJIANGHUANAN EQUIP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410460220.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-17
Publication Date
2024-10-18
Estimated Expiration
2044-04-17

AI Technical Summary

Technical Problem

At this stage, polyurethane foam absorbs water while absorbing oil, resulting in low oil absorption and cannot effectively solve the problems of low separation efficiency and secondary pollution in oily wastewater treatment.

Method used

By preparing an oil-absorbing polyurethane foam material, benzaldehyde, 3,4-diaminobenzenethiol and other raw materials are reacted to form modified monomers, and are ultrasonically treated in KH570 n-hexane solution, combined with an ethanol solution of zinc nitrate hexahydrate Soaked to form a metal-organic structure, reduce water absorption and increase hydrophobicity, thereby improving oil absorption effect.

Benefits of technology

It significantly increases the oil absorption capacity and oil absorption rate of polyurethane foam materials, reduces water absorption, improves the efficiency of treating oily wastewater, and reduces the risk of secondary pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004795501720000101
    Figure BDA0004795501720000101
  • Figure BDA0004795501720000111
    Figure BDA0004795501720000111
Patent Text Reader

Abstract

The invention discloses an oil-absorbing polyurethane foam material and a preparation method thereof. The method comprises the following steps: a pre-treated substrate, a modified monomer, octadecyl methacrylate and butyl acrylate are reacted, polyacrylate molecules are coated on the surface of the pre-treated substrate, and then the substrate is immersed in an ethanol solution of hexahydrate zinc nitrate to obtain the oil-absorbing polyurethane foam material. The pre-treated substrate molecules contain an organic silicon structure and a large number of benzene ring structures and long-chain fluorocarbon structures, and the molecules are in a grid-like structure, so that the water absorption of the modified substrate is reduced, thereby improving the oil absorption effect. The polyacrylate structure is coated on the surface of the modified substrate, and the polyacrylate molecules contain long-chain alkyl and benzene ring structures, which can further improve the hydrophobicity of the polyurethane foam material. At the same time, the organic structure of zinc on the surface can ensure hydrophobic stability, thereby reducing the water absorption of the polyurethane foam material and increasing its oil absorption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oil-absorbing material preparation, in particular to an oil-absorbing polyurethane foam material and a preparation method thereof. Background Art

[0002] Oily wastewater is one of the common pollution sources in the current environment, mainly from the petrochemical industry. Oily wastewater contains a large amount of organic pollutants, which causes serious pollution to the environment. Since oily wastewater seriously endangers the survival of humans and various organisms, traditional oily wastewater treatment methods mainly include high-speed centrifugation, flotation, electric field, gravity separation, coagulation, biological treatment, etc. Although traditional treatment methods meet most separation needs, problems such as low separation efficiency and secondary pollution have not been effectively solved. Therefore, countries around the world have been committed to the research and development of new methods and new materials for oily wastewater treatment, to efficiently treat oily wastewater and reduce the harm of oily wastewater to the environment. The research on oil-absorbing materials mainly focuses on polyurethane sponge, polyacrylic resin, polypropylene fiber, etc. These three materials are synthesized from different monomers, but because polyurethane contains a large number of polar groups, the material can absorb oil and water at the same time, which affects the oil absorption efficiency. Summary of the invention

[0003] The purpose of the present invention is to provide an oil-absorbing polyurethane foam material and a preparation method thereof, which solves the problem that the current polyurethane foam absorbs water while absorbing oil, resulting in low oil absorption.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for preparing an oil-absorbing polyurethane foam material comprises the following steps:

[0006] Step A1: benzaldehyde, 3,4-diaminobenzenethiol, potassium carbonate and anhydrous ethanol are mixed evenly, and refluxed for reaction at a speed of 120-150 r / min and a temperature of 80-82° C. for 10-15 hours, and the pH value is adjusted to 5-5.5 to obtain intermediate 1; 2,2'-dichlorobenzidine, maleic anhydride and DMF are mixed evenly, and stirred for 10-15 minutes at a speed of 150-200 r / min and a temperature of 5-10° C., and then the temperature is raised to 55-60° C. and the reaction is carried out for 30-40 minutes, and triethylamine, acetic anhydride and nickel acetate are added, and the reaction is continued for 2-3 hours to obtain intermediate 2;

[0007] Step A2: The intermediate 1, potassium hydroxide, tetrabutylammonium bromide and DMF are uniformly mixed, stirred and the intermediate 2 is added at a speed of 60-80r / min and a temperature of 20-25°C, and the reaction is carried out for 2-3h to obtain a modified monomer, and the modified substrate is immersed in a n-hexane solution of KH570, ultrasonically treated at a frequency of 20-30kHz, and deionized water is added, and the ultrasonic treatment is carried out for 20-30min, and then dried to obtain a pretreated substrate;

[0008] Step A3: The pretreated substrate, modified monomer, octadecyl methacrylate, butyl acrylate and deionized water are mixed, nitrogen is introduced for protection, the temperature is kept at 75-80°C, azobisisobutyronitrile is added, the reaction is carried out for 7-9 hours, and then the precursor is dried to obtain the precursor, the precursor is immersed in an ethanol solution of zinc nitrate hexahydrate, and ultrasonically treated for 20-25 hours at a frequency of 20-30kHz and a temperature of 20-25°C to obtain an oil-absorbing polyurethane foam material.

[0009] Furthermore, the molar ratio of benzaldehyde, 3,4-diaminobenzenethiol and potassium carbonate in step A1 is 1:1:1.5, and the molar ratio of 2,2'-dichlorobenzidine, maleic anhydride, triethylamine, acetic anhydride and nickel acetate is 25mmo l:50mmo l:5mL:12mL:3.5g.

[0010] Furthermore, the molar ratio of the intermediate 1, potassium hydroxide and intermediate 2 in step A2 is 1:3.5:2, the amount of tetrabutylammonium bromide used is 2% of the mass of the intermediate 1, and the amount of KH570 used is 5% of the mass of the modified substrate.

[0011] Furthermore, the mass ratio of the pretreated substrate, modified monomer, octadecyl methacrylate and butyl acrylate described in step A3 is 0.8:6:32:5:5, the amount of azobisisobutyronitrile is 0.3% of the mass of the modified monomer, and the mass fraction of the ethanol solution of zinc nitrate hexahydrate is 3%.

[0012] Further, the modified matrix is ​​prepared by the following steps:

[0013] Step B1: diphenyldichlorosilane and deionized water are mixed, stirred for 10-15 minutes at a speed of 200-300 r / min and a temperature of 60-70° C., concentrated sulfuric acid and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane are added, and the reaction is carried out for 4-6 hours, and the pH is adjusted to neutral to obtain a diamine-terminated polysiloxane;

[0014] Step B2: mixing diamine-terminated polysiloxane, 2-(2,2,3,3,4,4,4-heptafluorobutyl)methyl oxirane and DMF uniformly, reacting for 6-8 hours at a speed of 150-200 r / min, a temperature of 30-40° C. and a pH of 11-12 to obtain hydroxy polysiloxane;

[0015] Step B3: Mix polyether polyol, hydroxypolysiloxane, ethylene glycol, dibutyltin dilaurate and deionized water evenly, stir and add diphenylmethane diisocyanate at a speed of 2000-2500r / min and a temperature of 20-25°C, stir for 10-20s, pour into a mold for foaming and curing, and obtain a modified matrix.

[0016] Furthermore, the amount ratio of diphenyldichlorosilane, deionized water and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane described in step B1 is 1 mmol:20 mL:1.5 mmol, and the amount of concentrated sulfuric acid is 1-1.5% of the total mass of diphenyldichlorosilane and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane.

[0017] Furthermore, the molar ratio of the diamine-terminated polysiloxane and 2-(2,2,3,3,4,4,4-heptafluorobutyl)methyl oxirane described in step B2 is 1:4.

[0018] Furthermore, the mass ratio of the polyether polyol, hydroxypolysiloxane, ethylene glycol and deionized water in step B3 is 50:20:5:4, the isocyanate index is 0.9, and the amount of dibutyltin dilaurate is 2% of the mass of diphenylmethane diisocyanate.

[0019] Beneficial effects of the present invention: the oil-absorbing polyurethane foam material prepared by the present invention uses benzaldehyde and 3,4-diaminobenzenethiol as raw materials to react, so that the aldehyde group on the benzaldehyde reacts with the diamino group on the 3,4-diaminobenzenethiol to form an imidazole structure, to obtain an intermediate 1, 2,2'-dichlorobenzidine and maleic anhydride react, so that the amino group on the 2,2'-dichlorobenzidine and the maleic anhydride open the ring, dehydrate and then close the ring, to obtain an intermediate 2, and the intermediate 1 and the intermediate 2 react, so that the thiol group on the intermediate 1 and the chlorine atom on the intermediate 2 are located at the same position. point reaction to obtain a modified monomer, soak the modified substrate in a n-hexane solution of KH570 to graft double bonds on the surface of the modified substrate to obtain a pretreated substrate, react the pretreated substrate, the modified monomer, octadecyl methacrylate and butyl acrylate to coat the surface of the pretreated substrate with polyacrylate molecules, and then soak it in an ethanol solution of hexahydrate zinc nitrate to coordinate the zinc ions with the imidazole structure in the polyacrylic acid molecules to form a metal organic structure to obtain an oil-absorbing polyurethane foam material, and the modified substrate is first hydrolyzed with diphenyldichlorosilane as a raw material, Then, it is polymerized with 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane to obtain diamine-terminated polysiloxane, and the diamine-terminated polysiloxane is reacted with 2-(2,2,3,3,4,4,4-heptafluorobutyl)methyl oxirane to make the amino group on the diamine-terminated polysiloxane react with the epoxy group on the 2-(2,2,3,3,4,4,4-heptafluorobutyl)methyl oxirane to form a new hydroxyl group to obtain hydroxyl polysiloxane, and the hydroxyl polysiloxane, hydroxyl polysiloxane, ethylene glycol and diphenylmethane diisocyanate are reacted. Deionized water is then used as a foaming agent to prepare a modified matrix. The modified matrix molecules contain an organic silicon structure, a large number of benzene ring structures and a long-chain fluorocarbon structure, and the molecules are in a grid-like structure, which reduces the water absorption of the modified matrix and thereby improves the oil absorption effect. A polyacrylate structure is coated on the surface of the modified matrix. The polyacrylate molecules contain a long-chain alkyl and a benzene ring structure, which can further improve the hydrophobicity of the polyurethane foam material. At the same time, the organic structure of zinc on the surface can ensure hydrophobic stability, thereby reducing the water absorption of the polyurethane foam material and increasing its oil absorption. DETAILED DESCRIPTION

[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Example 1

[0022] A method for preparing an oil-absorbing polyurethane foam material comprises the following steps:

[0023] Step A1: benzaldehyde, 3,4-diaminobenzenethiol, potassium carbonate and anhydrous ethanol were mixed evenly, and refluxed for 10 hours at a speed of 120 r / min and a temperature of 80°C, and the pH value was adjusted to 5 to obtain intermediate 1. 2,2'-dichlorobenzidine, maleic anhydride and DMF were mixed evenly, and stirred for 10 minutes at a speed of 150 r / min and a temperature of 5°C, and then the temperature was raised to 55°C and reacted for 30 minutes. Triethylamine, acetic anhydride and nickel acetate were added, and the reaction was continued for 2 hours to obtain intermediate 2;

[0024] Step A2: The intermediate 1, potassium hydroxide, tetrabutylammonium bromide and DMF are mixed uniformly, stirred at a speed of 60 r / min and a temperature of 20° C., and the intermediate 2 is added to react for 2 h to obtain a modified monomer, and the modified substrate is immersed in a n-hexane solution of KH570, ultrasonically treated at a frequency of 20 kHz, and deionized water is added, and the ultrasonic treatment is performed for 20 min, and then dried to obtain a pretreated substrate;

[0025] Step A3: The pretreated substrate, modified monomer, octadecyl methacrylate, butyl acrylate and deionized water are mixed, nitrogen is introduced for protection, the temperature is kept at 75°C, and azobisisobutyronitrile is added to react for 7 hours, and then dried to obtain a precursor. The precursor is immersed in an ethanol solution of zinc nitrate hexahydrate, and ultrasonically treated for 20 hours at a frequency of 20 kHz and a temperature of 20°C to obtain an oil-absorbing polyurethane foam material.

[0026] The molar ratio of benzaldehyde, 3,4-diaminobenzenethiol and potassium carbonate described in step A1 is 1:1:1.5, and the molar ratio of 2,2'-dichlorobenzidine, maleic anhydride, triethylamine, acetic anhydride and nickel acetate is 25mmo l:50mmo l:5mL:12mL:3.5g.

[0027] The molar ratio of intermediate 1, potassium hydroxide and intermediate 2 described in step A2 is 1:3.5:2, the amount of tetrabutylammonium bromide used is 2% of the mass of intermediate 1, and the amount of KH570 used is 5% of the mass of the modified substrate.

[0028] The mass ratio of the pretreated substrate, modified monomer, octadecyl methacrylate and butyl acrylate described in step A3 is 0.8:6:32:5:5, the amount of azobisisobutyronitrile is 0.3% of the mass of the modified monomer, and the mass fraction of the ethanol solution of zinc nitrate hexahydrate is 3%.

[0029] The modified matrix is ​​prepared by the following steps:

[0030] Step B1: diphenyldichlorosilane and deionized water were mixed, stirred for 10 min at a speed of 200 r / min and a temperature of 60° C., concentrated sulfuric acid and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane were added, and the mixture was reacted for 4 h, and the pH was adjusted to neutral to obtain a diamine-terminated polysiloxane;

[0031] Step B2: diamine-terminated polysiloxane, 2-(2,2,3,3,4,4,4-heptafluorobutyl)methyl oxirane and DMF are uniformly mixed, and reacted for 6 hours at a speed of 150 r / min, a temperature of 30° C. and a pH value of 11 to obtain hydroxy polysiloxane;

[0032] Step B3: Mix polyether polyol, hydroxy polysiloxane, ethylene glycol, dibutyltin dilaurate and deionized water evenly, stir and add diphenylmethane diisocyanate at a speed of 2000 r / min and a temperature of 20°C, stir for 10 seconds, pour into a mold for foaming and curing, and obtain a modified matrix.

[0033] The amount ratio of diphenyldichlorosilane, deionized water and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane described in step B1 is 1 mmol:20 mL:1.5 mmol, and the amount of concentrated sulfuric acid is 1% of the total mass of diphenyldichlorosilane and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane.

[0034] The molar ratio of the diamine-terminated polysiloxane and 2-(2,2,3,3,4,4,4-heptafluorobutyl)methyl oxirane described in step B2 is 1:4.

[0035] The mass ratio of the polyether polyol, hydroxypolysiloxane, ethylene glycol and deionized water described in step B3 is 50:20:5:4, the isocyanate index is 0.9, the amount of dibutyltin dilaurate is 2% of the mass of diphenylmethane diisocyanate, and the model of the polyether polyol is 300N.

[0036] Example 2

[0037] A method for preparing an oil-absorbing polyurethane foam material comprises the following steps:

[0038] Step A1: benzaldehyde, 3,4-diaminobenzenethiol, potassium carbonate and anhydrous ethanol were mixed evenly, and the mixture was refluxed for 13 hours at a speed of 120 r / min and a temperature of 81°C, and the pH value was adjusted to 5.5 to obtain intermediate 1. 2,2'-dichlorobenzidine, maleic anhydride and DMF were mixed evenly, and the mixture was stirred for 15 minutes at a speed of 150 r / min and a temperature of 8°C, and then the mixture was heated to 58°C and reacted for 35 minutes. Triethylamine, acetic anhydride and nickel acetate were added, and the reaction was continued for 2.5 hours to obtain intermediate 2.

[0039] Step A2: The intermediate 1, potassium hydroxide, tetrabutylammonium bromide and DMF are mixed uniformly, stirred and the intermediate 2 is added at a speed of 60 r / min and a temperature of 25° C., and the reaction is carried out for 2.5 hours to obtain a modified monomer, and the modified substrate is immersed in a n-hexane solution of KH570, ultrasonically treated at a frequency of 25 kHz, and deionized water is added, and the ultrasonic treatment is carried out for 25 minutes, and then dried to obtain a pretreated substrate;

[0040] Step A3: The pretreated substrate, modified monomer, octadecyl methacrylate, butyl acrylate and deionized water are mixed, nitrogen is introduced for protection, the temperature is kept at 78°C, azobisisobutyronitrile is added, the reaction is carried out for 8 hours, and then the precursor is dried to obtain the precursor, the precursor is immersed in an ethanol solution of zinc nitrate hexahydrate, and ultrasonically treated for 23 hours at a frequency of 25 kHz and a temperature of 28°C to obtain an oil-absorbing polyurethane foam material.

[0041] The molar ratio of benzaldehyde, 3,4-diaminobenzenethiol and potassium carbonate described in step A1 is 1:1:1.5, and the molar ratio of 2,2'-dichlorobenzidine, maleic anhydride, triethylamine, acetic anhydride and nickel acetate is 25mmo l:50mmo l:5mL:12mL:3.5g.

[0042] The molar ratio of intermediate 1, potassium hydroxide and intermediate 2 described in step A2 is 1:3.5:2, the amount of tetrabutylammonium bromide used is 2% of the mass of intermediate 1, and the amount of KH570 used is 5% of the mass of the modified substrate.

[0043] The mass ratio of the pretreated substrate, modified monomer, octadecyl methacrylate and butyl acrylate described in step A3 is 0.8:6:32:5:5, the amount of azobisisobutyronitrile is 0.3% of the mass of the modified monomer, and the mass fraction of the ethanol solution of zinc nitrate hexahydrate is 3%.

[0044] The modified matrix is ​​prepared by the following steps:

[0045] Step B1: diphenyldichlorosilane and deionized water were mixed, stirred for 15 min at a speed of 300 r / min and a temperature of 70° C., concentrated sulfuric acid and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane were added, reacted for 5 h, and the pH was adjusted to neutral to obtain a diamine-terminated polysiloxane;

[0046] Step B2: diamine-terminated polysiloxane, 2-(2,2,3,3,4,4,4-heptafluorobutyl)methyl oxirane and DMF are uniformly mixed, and reacted for 7 hours at a speed of 150 r / min, a temperature of 35° C. and a pH value of 12 to obtain hydroxy polysiloxane;

[0047] Step B3: Mix polyether polyol, hydroxy polysiloxane, ethylene glycol, dibutyltin dilaurate and deionized water evenly, stir and add diphenylmethane diisocyanate at a speed of 2000 r / min and a temperature of 23°C, stir for 15 seconds, pour into a mold for foaming and curing, and obtain a modified matrix.

[0048] The amount ratio of diphenyldichlorosilane, deionized water and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane described in step B1 is 1 mmol:20 mL:1.5 mmol, and the amount of concentrated sulfuric acid is 1.3% of the total mass of diphenyldichlorosilane and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane.

[0049] The molar ratio of the diamine-terminated polysiloxane and 2-(2,2,3,3,4,4,4-heptafluorobutyl)methyl oxirane described in step B2 is 1:4.

[0050] The mass ratio of the polyether polyol, hydroxypolysiloxane, ethylene glycol and deionized water described in step B3 is 50:20:5:4, the isocyanate index is 0.9, the amount of dibutyltin dilaurate is 2% of the mass of diphenylmethane diisocyanate, and the model of the polyether polyol is 300N.

[0051] Example 3

[0052] A method for preparing an oil-absorbing polyurethane foam material comprises the following steps:

[0053] Step A1: benzaldehyde, 3,4-diaminobenzenethiol, potassium carbonate and anhydrous ethanol were mixed evenly, and refluxed for 15 hours at a speed of 150 r / min and a temperature of 82°C, and the pH value was adjusted to 5.5 to obtain intermediate 1; 2,2'-dichlorobenzidine, maleic anhydride and DMF were mixed evenly, and stirred for 15 minutes at a speed of 200 r / min and a temperature of 10°C, and then the temperature was raised to 60°C and reacted for 30-40 minutes, triethylamine, acetic anhydride and nickel acetate were added, and the reaction was continued for 3 hours to obtain intermediate 2;

[0054] Step A2: The intermediate 1, potassium hydroxide, tetrabutylammonium bromide and DMF are mixed uniformly, stirred at a speed of 80 r / min and a temperature of 25° C., and the intermediate 2 is added to react for 3 hours to obtain a modified monomer, and the modified substrate is immersed in a n-hexane solution of KH570, ultrasonically treated at a frequency of 30 kHz, and deionized water is added, and the ultrasonic treatment is performed for 30 minutes, and then dried to obtain a pretreated substrate;

[0055] Step A3: The pretreated substrate, modified monomer, octadecyl methacrylate, butyl acrylate and deionized water are mixed, nitrogen is introduced for protection, the temperature is kept at 80°C, azobisisobutyronitrile is added, the reaction is carried out for 9 hours, and then the precursor is dried to obtain the precursor, the precursor is immersed in an ethanol solution of zinc nitrate hexahydrate, and ultrasonically treated for 25 hours at a frequency of 30 kHz and a temperature of 25°C to obtain an oil-absorbing polyurethane foam material.

[0056] The molar ratio of benzaldehyde, 3,4-diaminobenzenethiol and potassium carbonate described in step A1 is 1:1:1.5, and the molar ratio of 2,2'-dichlorobenzidine, maleic anhydride, triethylamine, acetic anhydride and nickel acetate is 25mmo l:50mmo l:5mL:12mL:3.5g.

[0057] The molar ratio of intermediate 1, potassium hydroxide and intermediate 2 described in step A2 is 1:3.5:2, the amount of tetrabutylammonium bromide used is 2% of the mass of intermediate 1, and the amount of KH570 used is 5% of the mass of the modified substrate.

[0058] The mass ratio of the pretreated substrate, modified monomer, octadecyl methacrylate and butyl acrylate described in step A3 is 0.8:6:32:5:5, the amount of azobisisobutyronitrile is 0.3% of the mass of the modified monomer, and the mass fraction of the ethanol solution of zinc nitrate hexahydrate is 3%.

[0059] The modified matrix is ​​prepared by the following steps:

[0060] Step B1: diphenyldichlorosilane and deionized water were mixed, stirred for 15 min at a speed of 300 r / min and a temperature of 70° C., concentrated sulfuric acid and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane were added, reacted for 6 h, and the pH was adjusted to neutral to obtain a diamine-terminated polysiloxane;

[0061] Step B2: diamine-terminated polysiloxane, 2-(2,2,3,3,4,4,4-heptafluorobutyl)methyl oxirane and DMF are uniformly mixed, and reacted for 8 hours at a speed of 200 r / min, a temperature of 40° C. and a pH value of 12 to obtain hydroxy polysiloxane;

[0062] Step B3: Mix polyether polyol, hydroxy polysiloxane, ethylene glycol, dibutyltin dilaurate and deionized water evenly, stir and add diphenylmethane diisocyanate at a speed of 2500 r / min and a temperature of 25°C, stir for 20 seconds, pour into a mold for foaming and curing, and obtain a modified matrix.

[0063] The amount ratio of diphenyldichlorosilane, deionized water and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane described in step B1 is 1 mmol:20 mL:1.5 mmol, and the amount of concentrated sulfuric acid is 1.5% of the total mass of diphenyldichlorosilane and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane.

[0064] The molar ratio of the diamine-terminated polysiloxane and 2-(2,2,3,3,4,4,4-heptafluorobutyl)methyl oxirane described in step B2 is 1:4.

[0065] The mass ratio of the polyether polyol, hydroxypolysiloxane, ethylene glycol and deionized water described in step B3 is 50:20:5:4, the isocyanate index is 0.9, the amount of dibutyltin dilaurate is 2% of the mass of diphenylmethane diisocyanate, and the model of the polyether polyol is 300N.

[0066] Comparative Example 1

[0067] Compared with Example 1, no hydroxy polysiloxane was added in this comparative example, and the remaining steps were the same.

[0068] Comparative Example 2

[0069] Compared with Example 1, no modified monomer was added in this comparative example, and the remaining steps were the same.

[0070] Comparative Example 3

[0071] Compared with Example 1, this comparative example uses a modified substrate as the polyurethane foam material, and the remaining steps are the same.

[0072] A 400-mesh stainless steel wire mesh was immersed in kerosene, taken out and allowed to stand until no oil dripped, and the weight was measured. The polyurethane foam materials prepared in Examples 1-3 and Comparative Examples 1-3 were weighed, and then placed on the stainless steel wire mesh and immersed in oil, and allowed to stand for 10 min, 30 min, 1 h, and 3 h, respectively. When no oil dripped, the weight was measured and the oil absorption was calculated. The test results are shown in the following table.

[0073]

[0074]

[0075] It can be seen from the above table that the present invention has very good oil absorption and oil absorption rate.

[0076] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing an oil-absorbing polyurethane foam material, characterized in that: The specific steps include: Step A1: benzaldehyde, 3,4-diaminobenzenethiol, potassium carbonate and anhydrous ethanol are mixed and refluxed for reaction, and the pH is adjusted to be acidic to obtain intermediate 1; 2,2'-dichlorobenzidine, maleic anhydride and DMF are mixed and stirred, and the temperature is raised to react, and triethylamine, acetic anhydride and nickel acetate are added, and the reaction is continued to obtain intermediate 2; Step A2: Mix and stir the intermediate 1, potassium hydroxide, tetrabutylammonium bromide and DMF and add the intermediate 2 to react to obtain a modified monomer. Soak the modified substrate in a n-hexane solution of KH570, perform ultrasonic treatment and add deionized water. After ultrasonic treatment, dry the substrate to obtain a pretreated substrate. Step A3: mixing the pretreated substrate, the modified monomer, octadecyl methacrylate, butyl acrylate and deionized water, introducing nitrogen protection, keeping the temperature at high temperature and adding azobisisobutyronitrile, reacting, drying to obtain a precursor, soaking the precursor in an ethanol solution of zinc nitrate hexahydrate, and ultrasonically treating to obtain an oil-absorbing polyurethane foam material; The modified matrix is ​​prepared by the following steps: Step B1: After mixing and stirring diphenyldichlorosilane and deionized water, concentrated sulfuric acid and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane are added to react, and the pH is adjusted to neutral to obtain a diamine-terminated polysiloxane; Step B2: mixing diamine-terminated polysiloxane, 2-(2,2,3,3,4,4,4-heptafluorobutyl)methyl oxirane and DMF to obtain hydroxy polysiloxane; Step B3: Mix and stir polyether polyol, hydroxy polysiloxane, ethylene glycol, dibutyltin dilaurate and deionized water, add diphenylmethane diisocyanate, stir, pour into a mold for foaming and curing, and obtain a modified matrix.

2. The method for preparing an oil-absorbing polyurethane foam material according to claim 1, characterized in that: The molar ratio of benzaldehyde, 3,4-diaminobenzenethiol and potassium carbonate described in step A1 is 1:1:1.5, and the molar ratio of 2,2'-dichlorobenzidine, maleic anhydride, triethylamine, acetic anhydride and nickel acetate is 25mmol:50mmol:5mL:12mL:3.5g.

3. The method for preparing an oil-absorbing polyurethane foam material according to claim 1, characterized in that: The molar ratio of intermediate 1, potassium hydroxide and intermediate 2 described in step A2 is 1:3.5:2, the amount of tetrabutylammonium bromide used is 2% of the mass of intermediate 1, and the amount of KH570 used is 5% of the mass of the modified substrate.

4. The method for preparing an oil-absorbing polyurethane foam material according to claim 1, characterized in that: The mass ratio of the pretreated substrate, modified monomer, octadecyl methacrylate and butyl acrylate described in step A3 is 0.8:6:32:5:

5.

5. The method for preparing an oil-absorbing polyurethane foam material according to claim 1, characterized in that: The amount ratio of diphenyldichlorosilane, deionized water and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane in step B1 is 1 mmol:20 mL:1.5 mmol.

6. The method for preparing an oil-absorbing polyurethane foam material according to claim 1, characterized in that: The molar ratio of the diamine-terminated polysiloxane and 2-(2,2,3,3,4,4,4-heptafluorobutyl)methyl oxirane described in step B2 is 1:

4.

7. The method for preparing an oil-absorbing polyurethane foam material according to claim 1, characterized in that: The mass ratio of the polyether polyol, hydroxy polysiloxane, ethylene glycol and deionized water described in step B3 is 50:20:5:4, and the isocyanate index is 0.

9.

8. An oil-absorbing polyurethane foam material, characterized in that: Prepared according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Oil-absorbing polyurethane foam material

    CN101787107A

  • Polyurethane high-power oil absorption material and preparation method therefor

    CN105315427A