A high-entropy oxide catalyst, its preparation method and application
By designing the components of the high-entropy oxide catalyst and achieving synergistic effects of multiple elements, the problems of sintering and carbon deposition in the methane-carbon dioxide dry reforming reaction were solved, resulting in high activity and selectivity, and meeting the requirements for stable industrial operation.
Patent Information
- Application Number
- CN202211617896.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-15
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-12-15
AI Technical Summary
Existing catalysts have problems with insufficient resistance to sintering, carbon deposition, and hydrothermal stability in the methane-carbon dioxide dry reforming reaction, making it difficult to maintain structural stability under high-temperature, strongly reducing reaction atmospheres.
A high-entropy oxide catalyst is used, which is composed of metals or non-metals such as titanium, silicon, cerium, zirconium, aluminum, magnesium, calcium, lanthanum, strontium, and molybdenum in equimolar or near equimolar ratios. Active components such as nickel, cobalt, iron, ruthenium, rhodium, and palladium are added to form a homogeneous solid solution mixed oxide. The structural stability and activity of the catalyst are improved through thermodynamic high-entropy effect and kinetic lag effect.
The catalyst exhibits high activity, selectivity, and anti-carbon deposition properties in the methane-carbon dioxide reaction, and can operate stably for extended periods under harsh conditions, meeting industrial requirements.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This application relates to a high-entropy oxide catalyst, its preparation method, and its application, belonging to the field of catalyst technology. Background Technology
[0002] Carbon dioxide and methane are typical greenhouse gases, and their efficient conversion and resource utilization are particularly important. Dry reforming (DRM) of methane can directly convert these two greenhouse gases into syngas. This reaction can alleviate the pressure of greenhouse gas emission reduction while reducing energy consumption, thus achieving both environmental and economic benefits. However, the strongly endothermic DRM reaction needs to be carried out at high temperatures (700-900℃) and in a strongly reducing reaction atmosphere, requiring catalysts with excellent anti-sintering and anti-coking properties. Furthermore, the addition of a small amount of water vapor to suppress catalyst deactivation due to coking and pipeline blockage places even higher demands on the hydrothermal stability of the catalyst. Therefore, the key technical problem to be solved in dry reforming of methane is the development of catalysts with excellent anti-sintering, anti-coking, hydrothermal resistance, and structural stability. Summary of the Invention
[0003] To address the shortcomings of existing catalysts, this invention provides an application of a high-entropy oxide catalyst in methane-carbon dioxide reforming. The high-entropy oxide catalyst is a homogeneous solid solution mixed oxide obtained by selecting five or more metals or non-metals such as titanium, silicon, cerium, zirconium, aluminum, magnesium, calcium, lanthanum, strontium, and molybdenum in equimolar or near-equimolar ratios, and adding a certain amount of one or more active components such as nickel, cobalt, iron, ruthenium, rhodium, palladium, and platinum, followed by mutual solid solution dissolution. The rich and flexible component design and multi-element synergistic effect of the high-entropy oxide allow for targeted design and directional regulation of its catalytic performance, giving the catalyst both activity and selectivity, and preventing carbon deposition. Furthermore, its thermodynamic high-entropy effect and kinetic hysteresis effect enable the catalyst to maintain structural stability under the harsh conditions of methane-carbon dioxide dry reforming, endowing the catalyst with anti-sintering and hydrothermal resistance properties. Therefore, the high-entropy oxide catalyst synthesized using this strategy exhibits high activity, good selectivity, anti-carbon deposition, anti-sintering, and hydrothermal resistance in the methane-carbon dioxide reaction, meeting the industrial requirements for long-term stable operation.
[0004] According to one aspect of this application, a high-entropy oxide catalyst is provided, the high-entropy oxide catalyst having a porous structure;
[0005] The high-entropy oxide catalyst comprises a first element and a second element;
[0006] The first element is selected from at least five of the following: Ti, Mg, Al, Ce, La, Sr, W, K, Zr, Mn, Ba, Si, Nb, Mo, Nd, and Gd.
[0007] The second element is selected from at least one of Ni, Co, Ru, Rh, Ir, and Pt.
[0008] Optionally, the number of moles of each element in the high-entropy oxide is similar.
[0009] Optionally, Ru, Rh, Ir, and Pt in the second element independently account for 0 to 5.0 wt% of the catalyst mass.
[0010] Optionally, Ni and Co in the second element independently account for 5.0 to 35 wt% of the catalyst mass.
[0011] Optionally, each element in the first element independently accounts for 5.0 to 35 wt% of the mass of the catalyst.
[0012] Optionally, the high-entropy oxide catalyst has a mesoporous structure with a pore size of 3–10 nm.
[0013] According to another aspect of this application, a method for preparing the above-mentioned high-entropy oxide catalyst is provided, comprising the following steps:
[0014] A) Dissolve the first element precursor, the second element precursor, the metal chelating agent, and the pore-forming agent in a solvent to obtain a mixed solution;
[0015] The first element is selected from at least five of the following: Ti, Mg, Al, Ce, La, Sr, W, K, Zr, Mn, Ba, Si, Nb, Mo, Nd, and Gd.
[0016] The second element is selected from at least one of Ni, Co, Ru, Rh, Ir, and Pt;
[0017] B) Evaporate the solvent from the mixed solution to obtain a dry gel sample;
[0018] C) The dry gel sample was ball-milled and calcined in an oxygen-containing atmosphere to obtain the high-entropy oxide catalyst.
[0019] Optionally, the first element precursor is selected from at least one of nitrates, hydrochlorides, acetates, lactates, and sulfates containing the first element;
[0020] The second element precursor is selected from at least one of nitrates, hydrochlorides, acetates, lactates, sulfates, and acetylacetones containing the second element.
[0021] Optionally, the metal chelating agent is selected from at least one of citric acid, ethylenediaminetetraacetic acid, aminotriacetic acid, tartaric acid, and glucose.
[0022] Optionally, the pore-forming agent is selected from at least one of polyvinyl alcohol, polymethyl methacrylate, starch, urea, ammonium chloride, polystyrene, and polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer.
[0023] Optionally, the solvent is selected from at least one of water, ethanol, and acetone.
[0024] Optionally, the ratio of the total molar amount of the metal chelating agent to the first element precursor and the second element precursor is 0.95 to 1.05:1, based on the total molar amount of the first element and the second element.
[0025] Optionally, the ratio of the pore-forming agent to the total mass of the first element precursor and the second element precursor is 0.5 to 1.5:1, based on the total mass of the first element and the second element.
[0026] Optionally, the total molar number of the first element precursor and the second element precursor is used to prepare a solution with a concentration of 0.2 to 0.5 mol / L.
[0027] Optionally, in step B), the temperature for evaporation is 110–160°C.
[0028] Optionally, in step C), the ball milling frequency is 20-50 Hz, and the ball milling time is 10-500 min.
[0029] Optionally, in step C), the ball milling process uses a ball milling jar and a ball milling material selected from at least one of stainless steel, polytetrafluoroethylene, zirconium oxide, and agate.
[0030] Optionally, in step C), the calcination temperature is 600–1200°C, and the calcination time is 0.1–10 h.
[0031] According to another aspect of this application, the application of the above-described high-entropy oxide catalyst or the high-entropy oxide catalyst obtained according to the above-described preparation method in the methane / carbon dioxide reforming to syngas reaction is provided.
[0032] The beneficial effects that this application can produce include:
[0033] 1) The high-entropy oxide catalyst provided in this application has good structural stability. Under the harsh reaction conditions of methane-carbon dioxide reforming, the framework does not collapse and the active components do not sinter. Moreover, the catalyst has a porous structure, which provides a larger catalytic interface and can expose more reactive sites.
[0034] 2) The high-entropy oxide catalyst provided in this application, in the methane-carbon dioxide reaction, the surface acidity and alkalinity of the catalyst, which are directly regulated by the elemental composition, promote the adsorption of carbon dioxide on the surface, inhibit the deep dehydrogenation of methane, enhance the carbon removal effect of carbon dioxide, and make the catalyst less prone to carbon deposition; especially under humid conditions, the high-entropy oxide catalyst can still maintain good stability.
[0035] 3) The method for preparing the high-entropy oxide catalyst provided in this application is simple, convenient, and conducive to large-scale production. Attached Figure Description
[0036] Figure 1 The nitrogen isothermal absorption-desorption curve of the porous high-entropy oxide catalyst prepared in Example 1 of this application, as measured by a porous material specific surface area and pore size distribution instrument;
[0037] Figure 2 These are the results of catalyst pore size analysis. Detailed Implementation
[0038] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.
[0039] Unless otherwise specified, all raw materials used in the embodiments of this application were purchased through commercial channels.
[0040] The analysis method in the embodiments of this application is as follows:
[0041] The pore structure of porous high-entropy oxide catalysts was analyzed using a surface area and pore size (BET) analyzer.
[0042] In the embodiments of this application, the CO2 conversion rate, CH4 conversion rate, and H2 selectivity are calculated as follows:
[0043]
[0044]
[0045]
[0046] In the embodiments of this application, CO2 conversion rate, CH4 conversion rate, and H2 selectivity are all calculated based on the number of carbon moles.
[0047] Example 1
[0048] This example provides a method for preparing porous high-entropy oxides, and the specific implementation steps are as follows:
[0049] 1. Weigh 2 mmol each of titanium oxysulfate, cerium nitrate, zirconium nitrate, lanthanum nitrate, magnesium nitrate, and nickel nitrate, dissolve them in 50 mL of deionized water, then add 10 mmol of tartaric acid and 2.5 g of polyvinyl alcohol (Mw4000), heat to 70 °C and stir until completely dissolved.
[0050] 2. Place the dissolved solution in a preheated drying oven at 120°C for 10 hours to obtain a completely dried mixed precursor dry gel.
[0051] 3. Place the dry gel in a muffle furnace and calcine it at 900℃ for 2 hours at a rate of 5℃ / min to obtain a porous high-entropy oxide catalyst.
[0052] The catalyst obtained using the above synthesis method was applied to methane-carbon dioxide dry reforming. The catalyst was ground, compressed into tablets, sieved through a 40-60 mesh screen, and 200 mg was weighed and placed in a fixed-bed reactor. The dry reforming reaction was carried out at 800℃ under a mixed gas flow rate of 100 mL / min and CH4 / CO2 / N2 = 1 / 1 / 3. The conversion rates of CH4 and CO2 reached 92% and 97%, respectively, and the H2 selectivity reached 97%. After a 48-hour stability test, the activity remained essentially unchanged, and no deactivation occurred.
[0053] Example 2
[0054] This example provides a method for preparing porous high-entropy oxides, and the specific implementation steps are as follows:
[0055] Weigh out 5 mmol each of titanium oxysulfate, cerium acetate, zirconium nitrate, lanthanum nitrate, manganese acetate, potassium chloride, triisopropylaluminum, magnesium carbonate, and nickel chloride, and 300 mg of ruthenium trichloride. Dissolve them in 100 mL of a 1:1 mixture of deionized water and ethanol. Then add 45 mmol of solid citric acid and 20 g of urea. Heat to 80 °C and stir until completely dissolved.
[0056] The dissolved solution was placed in a preheated drying oven at 120°C for 12 hours to obtain a completely dried mixed precursor dry gel.
[0057] The dry gel was placed in a muffle furnace and calcined at 750°C for 2 hours at a rate of 5°C / min to obtain a layered porous high-entropy oxide catalyst.
[0058] The catalyst obtained using the above synthesis method was applied to methane-carbon dioxide dry reforming. The catalyst was ground, compressed into tablets, sieved through a 40-60 mesh screen, and 200 mg was weighed and placed in a fixed-bed reactor. The dry reforming reaction was carried out at 650℃ under a mixed gas flow rate of 100 mL / min and CH4 / CO2 / N2 = 1 / 1 / 3. The conversion rates of CH4 and CO2 reached 94% and 98%, respectively, and the H2 selectivity reached 98%. After a 48-hour stability test, the activity remained essentially unchanged, and no deactivation occurred.
[0059] Example 3
[0060] This example provides a method for preparing porous high-entropy oxides, and the specific implementation steps are as follows:
[0061] Weigh out 3 mmol each of titanium oxysulfate, cerium acetate, zirconium nitrate, lanthanum nitrate, triisopropylaluminum, tetraethyl orthosilicate, magnesium carbonate, and nickel chloride, and dissolve 200 mg of rhodium chloride in a 1:2 mixture of 100 mL of deionized water and acetone. Then add 24 mmol of ethylenediaminetetraacetic acid and 3 g of polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123), heat to 80 °C and stir until completely dissolved.
[0062] The dissolved solution was placed in a preheated drying oven at 120°C for 8 hours to obtain a completely dried mixed precursor dry gel.
[0063] The dry gel is placed in a muffle furnace and calcined at 800°C for 5 hours at a rate of 5°C / min to obtain a porous high-entropy oxide catalyst.
[0064] The catalyst obtained using the above synthesis method was applied to methane-carbon dioxide dry reforming. The catalyst was ground, compressed into tablets, sieved through a 40-60 mesh screen, and 200 mg was weighed and placed in a fixed-bed reactor. The dry reforming reaction was carried out at 700℃ under a mixed gas flow rate of 100 mL / min and CH4 / CO2 / N2 = 1 / 1 / 3. The conversion rates of CH4 and CO2 reached 95% and 99%, respectively, and the H2 selectivity reached 97%. After a 48-hour stability test, the activity remained essentially unchanged, and no deactivation occurred.
[0065] Example 4
[0066] This example provides a method for preparing porous high-entropy oxides, and the specific implementation steps are as follows:
[0067] Weigh out 2 mmol each of titanium oxysulfate, cerium nitrate, zirconium chloride, lanthanum nitrate, triisopropylaluminum, manganese chloride, sodium molybdate, magnesium acetate, and nickel acetylacetone, and 100 mg of ruthenium acetylacetone. Dissolve them in 100 mL of a 1:1:1 mixture of deionized water, acetone, and ethanol. Then add 18 mmol of solid citric acid and 5 g of ammonium chloride. Heat to 60 °C and stir until completely dissolved.
[0068] The dissolved solution was placed in a preheated drying oven at 120°C for 10 hours to obtain a completely dried mixed precursor dry gel.
[0069] The dry gel is placed in a muffle furnace and calcined at 750°C for 3 hours at a rate of 3°C / min to obtain a layered porous high-entropy oxide catalyst.
[0070] The catalyst obtained using the above synthesis method was applied to methane-carbon dioxide dry reforming. The catalyst was ground, compressed into tablets, sieved through a 40-60 mesh screen, and 200 mg was weighed and placed in a fixed-bed reactor. The dry reforming reaction was carried out at 700℃ under a mixed gas flow rate of 100 mL / min and CH4 / CO2 / N2 = 1 / 1 / 3. The conversion rates of CH4 and CO2 reached 93% and 98%, respectively, and the H2 selectivity reached 98%. After a 48-hour stability test, the activity remained essentially unchanged, and no deactivation occurred.
[0071] Example 5
[0072] This example provides a method for preparing porous high-entropy oxides, and the specific implementation steps are as follows:
[0073] Weigh out 2 mmol each of titanium oxysulfate, cerium acetate, zirconium nitrate, lanthanum nitrate, triisopropylaluminum, tetraethyl orthosilicate, and magnesium carbonate, 50 mg of ruthenium chloride, and 30 mg of chloroplatinic acid. Dissolve them in a 1:1 mixture of deionized water and ethanol in 50 mL. Then add 14 mmol of citric acid solid and 5 g of polystyrene beads. Heat to 70 °C and stir for 3 hours.
[0074] The dissolved solution was placed in a preheated drying oven at 120°C for 10 hours to obtain a completely dried mixed precursor dry gel.
[0075] The dry gel is placed in a muffle furnace and calcined at 900°C for 2 hours at a rate of 5°C / min to obtain a porous high-entropy oxide catalyst.
[0076] The catalyst obtained using the above synthesis method was applied to methane-carbon dioxide dry reforming. The catalyst was ground, compressed into tablets, sieved through a 40-60 mesh screen, and 200 mg was weighed and placed in a fixed-bed reactor. The dry reforming reaction was carried out at 800℃ under a mixed gas flow rate of 100 mL / min and CH4 / CO2 / N2 = 1 / 1 / 3. The conversion rates of CH4 and CO2 reached 90% and 97%, respectively, and the H2 selectivity reached 96%. After a 48-hour stability test, the activity remained essentially unchanged, and no deactivation occurred.
[0077] Example 6
[0078] This example provides a method for preparing porous high-entropy oxides, and the specific implementation steps are as follows:
[0079] Weigh out 2 mmol each of titanium oxysulfate, cerium acetate, zirconium nitrate, lanthanum nitrate, triisopropylaluminum, tetraethyl orthosilicate, and magnesium carbonate, 50 mg of ruthenium chloride, and 30 mg of chloroplatinic acid. Dissolve them in a 1:1 mixture of deionized water and ethanol in 50 mL. Then add 14 mmol of citric acid solid and 5 g of polystyrene beads. Heat to 70 °C and stir for 3 hours.
[0080] The dissolved solution was placed in a preheated drying oven at 120°C for 10 hours to obtain a completely dried mixed precursor dry gel.
[0081] The dry gel is placed in a muffle furnace and calcined at 900°C for 2 hours at a rate of 5°C / min to obtain a porous high-entropy oxide catalyst.
[0082] The catalyst obtained using the above synthesis method was applied to methane-carbon dioxide dry reforming. The catalyst was ground, compressed into tablets, sieved through a 40-60 mesh screen, and 200 mg was weighed and placed in a fixed-bed reactor. The dry reforming reaction was carried out at 750 °C with a mixed gas flow rate of 100 mL / min and CH4 / CO2 / N2 = 1 / 1 / 3. The conversion rates of CH4 and CO2 reached 92% and 96%, respectively, and the H2 selectivity reached 97%. After a 48-hour stability test, the activity remained essentially unchanged, and no deactivation occurred.
[0083] Figure 1 The nitrogen isotherm adsorption-desorption curves for the catalyst synthesized in Example 1 are shown below. Figure 2 Analysis of the pore size obtained by the BJH method. Figure 1 As shown in Figure 2, the catalyst exhibits a typical mesoporous structure with a specific surface area of 173.0 m². 2 / g, with pore sizes between 2 and 10 nm.
[0084] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A high-entropy oxide catalyst, characterized in that, The high-entropy oxide catalyst has a porous structure; The high-entropy oxide catalyst comprises a first element and a second element; The first element is selected from at least five of the following: Ti, Mg, Al, Ce, La, Sr, W, K, Zr, Mn, Ba, Si, Nb, Mo, Nd, and Gd. The second element is selected from at least one of Ni, Co, Ru, Rh, Ir, and Pt.
2. The catalyst according to claim 1, characterized in that, The second element, Ru, Rh, Ir, and Pt, independently constitute 0-5.0 wt% of the catalyst mass. Ni and Co in the second element independently account for 5.0 to 35 wt% of the catalyst mass.
3. The catalyst according to claim 1, characterized in that, Each element in the first element independently accounts for 5.0 to 35 wt% of the mass of the catalyst.
4. The catalyst according to claim 1, characterized in that, The high-entropy oxide catalyst has a mesoporous structure with a pore size of 3~10 nm.
5. A method for preparing a high-entropy oxide catalyst according to any one of claims 1 to 4, characterized in that, Includes the following steps: A) Dissolve the first element precursor, the second element precursor, the metal chelating agent, and the pore-forming agent in a solvent to obtain a mixed solution; The first element is selected from at least five of the following: Ti, Mg, Al, Ce, La, Sr, W, K, Zr, Mn, Ba, Si, Nb, Mo, Nd, and Gd. The second element is selected from at least one of Ni, Co, Ru, Rh, Ir, and Pt; B) Evaporate the solvent from the mixed solution to obtain a dry gel sample; C) The dry gel sample was ball-milled and calcined in an oxygen-containing atmosphere to obtain the high-entropy oxide catalyst.
6. The preparation method according to claim 5, characterized in that, The first element precursor is selected from at least one of nitrates, hydrochlorides, acetates, lactates, and sulfates containing the first element; The second element precursor is selected from at least one of nitrates, hydrochlorides, acetates, lactates, sulfates, and acetylacetones containing the second element.
7. The preparation method according to claim 5, characterized in that, The metal chelating agent is selected from at least one of citric acid, ethylenediaminetetraacetic acid, aminotriacetic acid, tartaric acid, and glucose; The pore-forming agent is selected from at least one of polyvinyl alcohol, polymethyl methacrylate, starch, urea, ammonium chloride, polystyrene, and polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer; The solvent is selected from at least one of water, ethanol, and acetone.
8. The preparation method according to claim 5, characterized in that, The ratio of the total molar amount of the metal chelating agent to the first element precursor and the second element precursor is 0.95~1.05:1, based on the total number of moles of the first element and the second element. The ratio of the pore-forming agent to the total mass of the first element precursor and the second element precursor is 0.5~1.5:1, based on the total mass of the first element and the second element. The total number of moles of the first element precursor and the second element precursor is used to prepare a solution with a concentration of 0.2~0.5 mol / L.
9. The preparation method according to claim 5, characterized in that, In step B), the temperature for evaporation is 110~160℃; In step C), the ball milling frequency is 20~50Hz, and the ball milling time is 10~500min; In step C), the ball milling process uses a ball milling jar and a ball milling material selected from at least one of stainless steel, polytetrafluoroethylene, zirconium oxide, and agate. In step C), the roasting temperature is 600~1200℃ and the roasting time is 0.1~10h.
10. The application of a high-entropy oxide catalyst according to any one of claims 1 to 4 or a high-entropy oxide catalyst obtained by the preparation method according to any one of claims 5 to 9 in the reaction of methane / carbon dioxide reforming to syngas.
Citation Information
Patent Citations
Nano-high-entropy alloy electrocatalyst and preparation method thereof
CN110280255A
High-entropy oxide type electro-catalytic anode oxygen evolution catalyst material and preparation method thereof
CN111054378A