A catalyst with honeycomb-supported high-entropy oxides, its preparation method and application

By using a honeycomb-supported high-entropy oxide catalyst, the hydrothermal stability and carbon deposition issues of methane dry reforming catalysts were solved, achieving highly efficient methane and CO2 reforming reactions and improving catalytic performance.

CN118217992BActive Publication Date: 2026-11-17DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
CN202211617933.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-15
Publication Date
2026-11-17
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

Existing methane dry reforming catalysts have poor hydrothermal stability under high-temperature, strong reducing reaction conditions, are prone to carbon deposition and deactivation, and are difficult to control in terms of mass and heat transfer.

Method used

A honeycomb-supported high-entropy oxide catalyst is used. The configuration entropy of the high-entropy structure and the solid solution structure enable the active sites to be uniformly dispersed. Combined with the low diffusion resistance of the overall structure, the temperature gradient is avoided. The preparation methods include solid-phase synthesis, precipitation or sol-gel method, and the addition of citric acid and other substances can be used to adjust the pore structure.

Benefits of technology

This study achieved high-temperature hydrothermal stability and anti-carbon deposition properties of the catalyst, enhanced heat and mass transfer performance, and improved the catalytic performance of methane and CO2 reforming reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004000658440000051
    Figure BDA0004000658440000051
  • Figure BDA0004000658440000052
    Figure BDA0004000658440000052
  • Figure BDA0004000658440000053
    Figure BDA0004000658440000053
Patent Text Reader

Abstract

This application discloses a honeycomb-supported high-entropy oxide catalyst, its preparation method, and its application. The catalyst comprises a honeycomb support and a catalytic coating, with the catalytic coating supported on the honeycomb support; the catalytic coating is a high-entropy oxide. The catalyst exhibits excellent high-temperature hydrothermal stability and anti-carbon deposition ability in the methane / CO2 reforming reaction, maintaining high catalytic activity under high-temperature reducing atmospheres, providing a new approach for catalyst development under high-temperature and high-hydrothermal conditions. This invention also provides a method for loading high-entropy metal oxides with an integral honeycomb structure, avoiding the embedding of active components in conventional loading processes, reducing the mass and heat transfer resistance of the catalytic layer, and enhancing the strongly endothermic reaction process. This catalyst can eliminate scale-up effects, which is beneficial for the industrial application of the technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to a catalyst with a honeycomb-supported high-entropy oxide, its preparation method and application, belonging to the field of catalytic materials. Background Technology

[0002] Carbon dioxide and methane are typical greenhouse gases, and their efficient conversion and resource utilization are particularly important. Dry reforming (DRM) of methane can directly convert these two greenhouse gases into syngas, reducing energy consumption while alleviating pressure on greenhouse gas emission reduction, thus offering both environmental and economic benefits. However, the DRM reaction requires high temperature (700-850℃) and a strongly reducing reaction atmosphere, necessitating catalysts with excellent anti-sintering, anti-carbonization, and hydrothermal resistance properties.

[0003] High entropy oxides (HEOs) maintain a stable structure even under extreme operating conditions due to their thermodynamic high entropy effect and kinetic hysteresis diffusion effect. Since their inception, HEOs have attracted widespread attention and hold promise for applications in various fields, such as high entropy alloys (CN109182877A), high entropy alloy coatings (CN103484810B), high entropy ceramics (AU2021102229A4, CN111763087A), high entropy semiconductors or insulators (TWI395336B), corrosion-resistant coatings (CN108914041B, CN108914041A), high entropy oxide amorphous materials (CN108821571B), and high thermal conductivity materials. The above-mentioned applications, including (WO2022160471A1), refractory alloys (CN109182877B), high electrical conductivity (CN113023777A), thermal barrier coatings (SG11202100226YA, EP3863990A2, CA3106049A1, WO2020142125A3), electrochromic materials (CN112340787A), and strong magnetic materials (WO2019109059A1), are mainly based on their excellent thermal conductivity, electrical conductivity, and corrosion resistance. However, their application in the catalytic field is relatively limited, with only (US20220134316A1) applying it to the catalytic oxidation reaction of CO; patent CN111790397A discloses a high-entropy metal oxide catalyst for the catalytic oxidation and removal of aromatic organic sulfur compounds from fuel oil. High-entropy oxides possess high thermal stability and conductivity, along with multi-component tunable properties, which can address the requirement for high hydrothermal stability in catalysts during methane-CO2 reforming. Furthermore, since the reaction is affected by heat and mass transfer, the high mass transfer performance of the overall structured catalyst helps eliminate bed hotspots and avoids carbon buildup caused by uneven temperature distribution. Summary of the Invention

[0004] To overcome the problems of poor hydrothermal stability, easy carbon deposition and deactivation, and catalytic reaction being controlled by mass and heat transfer in methane dry reforming catalysts, this invention utilizes the unique configuration entropy of the high-entropy structure and the high-temperature stabilization of each component in the solid solution structure, so that the active sites are uniformly dispersed and maintained in a high-temperature stable state. At the same time, the low diffusion resistance of the overall structure catalyst is utilized to avoid temperature gradients on the catalyst. The technical problem to be solved is to provide a methane / CO2 reforming catalyst with excellent hydrothermal stability and resistance to carbon deposition, as well as its preparation method.

[0005] According to one aspect of this application, a catalyst for a honeycomb-supported high-entropy oxide is provided, comprising a honeycomb support and a catalytic coating, the catalytic coating being supported on the honeycomb support;

[0006] The catalytic coating is a high-entropy oxide;

[0007] The high-entropy oxide includes a base element and an active element;

[0008] The base element is selected from at least five of the following: Mg, Al, Ce, La, Sr, W, K, Zr, Mn, Ba, Si, Nb, Mo, Nd, Gd, and Cu.

[0009] The active element is selected from at least one of Ni, Co, Ru, Rh, Ir, and Pt.

[0010] Optionally, the catalytic coating accounts for 5 to 30 wt% of the catalyst by mass.

[0011] Optionally, each element in the substrate independently accounts for 5.0 to 50 wt% of the mass of the catalytic coating;

[0012] The Ni and Co elements in the active elements independently account for 5.0 to 50 wt% of the mass of the catalytic coating;

[0013] The active elements Ru, Rh, Ir, and Pt independently account for 0–5 wt% of the mass of the catalyst coating.

[0014] Optionally, the molar ratios of all elements except Ru, Rh, Ir, and Pt in the high-entropy oxide are the same.

[0015] Optionally, the cellular carrier is selected from ceramic cellular carriers and / or metal cellular carriers.

[0016] According to another aspect of this application, a method for preparing the above-mentioned catalyst is provided, comprising the following steps:

[0017] A) High-entropy oxides are synthesized from precursors containing base elements and active elements using solid-phase synthesis, precipitation, or sol-gel methods.

[0018] The base element is selected from at least five of the following: Mg, Al, Ce, La, Sr, W, K, Zr, Mn, Ba, Si, Nb, Mo, Nd, Gd, and Cu.

[0019] The active element is selected from at least one of Ni, Co, Ru, Rh, Ir, and Pt;

[0020] B) The mixed slurry containing the high-entropy oxide, pseudoboehmite, Al(OH)3, polyvinyl alcohol, citric acid, and water is ball-milled to obtain slurry A;

[0021] C) The honeycomb carrier is impregnated in the slurry A and dried to obtain sample B;

[0022] D) The sample B was calcined in an air atmosphere to obtain the catalyst.

[0023] Optionally, the mass ratio of the high-entropy oxide to boehmite, Al(OH)3, polyvinyl alcohol, citric acid, and water is 1:0.1-0.5:0.2-1.0:0.5-2.0:0.05-2.0:2.0-4.0.

[0024] Optionally, the solid-liquid ratio of the honeycomb carrier to the slurry A is 1:1 to 3.

[0025] Optionally, the cellular carrier is selected from ceramic cellular carriers and / or metal cellular carriers;

[0026] The cellular carrier is treated with acid before use.

[0027] Optionally, in step B), the ball mill rotation speed is 300-800 r / min, and the ball milling time is 2-10 h.

[0028] Optionally, the average particle size of the slurry A is 1.0 to 4.0 μm.

[0029] Optionally, the pH value of the slurry A is 2 to 5.

[0030] Optionally, in step C), the immersion time is 1 to 3 minutes.

[0031] Optionally, in step C), the drying temperature is 100–150°C, and the drying time is 2–10 hours.

[0032] Optionally, in step D), the calcination temperature is 600–900°C, and the calcination time is 2–6 hours.

[0033] Optionally, the solid-phase synthesis method is as follows: a precursor containing a base element and an active element is mixed with ethanol, ball-milled at a speed of 300-800 r / min for 6-10 h, dried at 110-150 °C for 5-12 h, and calcined at 600-1100 °C for 3-5 h to obtain the high-entropy oxide, wherein the precursor containing the base element and the active element is an oxide containing the base element and the active element.

[0034] Optionally, the precipitation method includes the following steps:

[0035] (1) A precursor containing base elements and active elements is mixed with sodium carbonate and reacted to obtain a gel-like precipitate.

[0036] (2) The gel-like precipitate is dried at 60-120℃ for 24-48h and calcined at 700-1000℃ for 3-h to obtain the high-entropy oxide;

[0037] The precursor containing the base element and the active element is selected from at least one of nitrate, hydrochloride, and acetate containing the base element and the active element.

[0038] Optionally, the molar ratio of the precursor containing the base element and the active element to the sodium carbonate is 1:1.0 to 1.2, based on the total molar amount of the base element and the active element.

[0039] Optionally, the sol-gel method includes the following steps:

[0040] The precursor containing the base element and the active element is mixed with an organic acid, dried at 120-130°C, and calcined at 700-1100°C for 3-5 hours to obtain the high-entropy oxide.

[0041] The precursor containing the base element and the active element is selected from at least one of nitrate, hydrochloride, and acetate containing the base element and the active element.

[0042] Optionally, the organic acid is selected from citric acid and / or glycine.

[0043] Optionally, the molar ratio of the precursor containing the base element and the active element to the organic acid is 1:1.0 to 1.2, based on the total molar amount of the base element and the active element.

[0044] Optionally, the catalyst further includes a post-treatment process:

[0045] The catalyst is impregnated in a noble metal salt solution and calcined at 700–900°C for 2–6 hours under an oxygen-containing atmosphere, wherein the noble metal element in the noble metal salt solution is selected from at least one of Ru, Rh, or Pt.

[0046] Optionally, the solid-liquid ratio of the catalyst to the noble metal salt solution is 1:0.5 to 1.5.

[0047] Optionally, the concentration of the noble metal salt solution is 2 to 10 mg / mL.

[0048] Optionally, the high-entropy oxide can also be synthesized by flame jetting, atomized jet pyrolysis, or solution combustion.

[0049] According to another aspect of this application, the application of the above-described catalyst or the catalyst obtained according to the above-described preparation method is provided in the reaction of reforming methane and CO2 to produce syngas.

[0050] The beneficial effects that this application can produce include:

[0051] 1) The honeycomb supported high-entropy oxide catalyst provided in this application has excellent high-temperature hydrothermal stability and anti-carbon deposition performance due to its high-entropy metal oxide structure. The overall structure catalyst enhances heat and mass transfer and improves the performance of strong endothermic catalytic reaction.

[0052] 2) The preparation method provided in this application, in which citric acid and other substances are added during the overall catalyst coating process, enriches the internal pore structure of the coating and avoids the embedding of active components during conventional loading processes. Detailed Implementation

[0053] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.

[0054] Unless otherwise specified, all raw materials used in the embodiments of this application were purchased through commercial channels.

[0055] In the embodiments of this application, the CO2 conversion rate, CH4 conversion rate, and H2 selectivity are calculated as follows:

[0056]

[0057]

[0058]

[0059] In the embodiments of this application, CO2 conversion rate, CH4 conversion rate, and H2 selectivity are all calculated based on the number of carbon moles.

[0060] Example 1:

[0061] This example provides a method for preparing high-entropy oxides using solid-phase synthesis.

[0062] Weigh 10 mmol of equimolar amounts of metal oxides NiO, MgO, CeO2, CuO, ZnO, and Al2O3, place them in a ball mill jar, and ball mill at 2000 rpm for 6 hours. Then filter and dry, and calcine the collected powder sample at 900°C for 3 hours to obtain high-entropy oxide 1; Example 2:

[0063] This example provides a method for synthesizing high-entropy oxides using a co-precipitation method.

[0064] Solution A was prepared by dissolving 5 wt% ruthenium nitrate and 10 mmol of equimolar metal precursor salts nickel nitrate, cerium nitrate, zirconium chloride, magnesium chloride, and zinc nitrate in deionized water, and solution B was prepared by dissolving 10.5 mmol of sodium carbonate in deionized water. Then, salt solution A was added dropwise to solution B while stirring, and the mixture was filtered to obtain a gel-like precipitate. The precipitate was washed several times with deionized water and dried overnight at 60°C. The precipitate was then calcined at 800°C for 5 hours to obtain high-entropy metal oxide 2.

[0065] Example 3:

[0066] This example provides a method for synthesizing high-entropy oxides using the sol-gel method.

[0067] 2 wt% ruthenium nitrate and 10 mmol of cerium nitrate, calcium acetate, nickel chloride, zirconium nitrate, aluminum nitrate metal precursor salt and equimolar citric acid were mixed in water at 80 °C and then dried at 120 °C to obtain a dry gel powder. The dry gel powder was then calcined in air at 850 °C for 2 hours to obtain high entropy metal oxide 3.

[0068] Example 4:

[0069] This example provides a method for preparing a monolithically honeycomb-supported high-entropy oxide methane / CO2 reforming catalyst.

[0070] The high-entropy oxide synthesized in Example 1, pseudoboehmite, Al(OH)3, 5wt% polyvinyl alcohol aqueous solution, citric acid, and deionized water were mixed in a weight ratio of 1.0:0.2:0.4:0.7:0.09:2.5 and ball-milled in a high-energy ball mill at 500 rpm for 4-6 hours to obtain slurry A. The average particle size (D50) of slurry A was 2.3 micrometers. Dilute nitric acid was added to adjust the pH of the slurry to 3.5.

[0071] The ceramic honeycomb carrier treated in 2% dilute nitric acid or the metal honeycomb carrier pretreated at high temperature is immersed in the prepared slurry for 1 minute, and the excess slurry A is blown away with compressed air to obtain sample B.

[0072] Sample B was dried at 120℃ for 6 hours and then weighed.

[0073] Repeat steps (2) and (3) until the target coating amount is reached, with the catalytic coating accounting for 20 wt% of the total catalyst weight.

[0074] Then, the catalyst sample C was prepared by calcining it in a muffle furnace at 700°C under air atmosphere for 3.5 hours.

[0075] Noble metals Ru, Rh, and / or Pt can be directly synthesized into high-entropy metal oxides via solid-state synthesis, co-precipitation, or gel-gel methods. They can also be loaded onto the surface of catalyst C via impregnation, as detailed below:

[0076] Based on the water absorption rate of catalyst C, a Ru precursor solution of a certain concentration is prepared.

[0077] Catalyst C was immersed in the above precursor solution, and excess solution was blown away with compressed air.

[0078] The catalyst C, impregnated with precious metals, was dried at 100°C for 10 hours.

[0079] The dried catalyst was calcined at 750°C in air for 2 hours to obtain a catalyst for later use.

[0080] Example 5:

[0081] This example provides a method for preparing a monolithically honeycomb-supported high-entropy oxide methane / CO2 reforming catalyst.

[0082] The high-entropy oxide synthesized in Example 2, pseudoboehmite, Al(OH)3, 5wt% polyvinyl alcohol aqueous solution, citric acid, and deionized water were mixed in a weight ratio of 1.0:0.25:0.35:0.6:0.08:3.0 and ball-milled in a high-energy ball mill at 500 rpm for 5 hours to obtain slurry A. The average particle size (D50) of slurry A was 1.7 micrometers. The pH value of the slurry was adjusted to 4.0 by adding dilute nitric acid.

[0083] The ceramic honeycomb carrier treated in 2% dilute nitric acid or the metal honeycomb carrier pretreated at high temperature was immersed in the prepared slurry for 2 minutes, and the excess slurry A was blown away with compressed air to obtain sample B.

[0084] Sample B was dried at 120℃ for 6 hours and then weighed.

[0085] Repeat steps (2) and (3) until the target coating amount is reached, with the catalytic coating accounting for 12 wt% of the total catalyst weight.

[0086] Then, the catalyst sample C was prepared by calcining it in a muffle furnace at 800°C in air atmosphere for 3 hours.

[0087] Noble metals Ru, Rh, and / or Pt can be directly synthesized into high-entropy metal oxides via solid-state synthesis, co-precipitation, or gel-gel methods. They can also be loaded onto the surface of catalyst C via impregnation, as detailed below:

[0088] Based on the water absorption rate of catalyst C, a Ru and Rh precursor solution of a certain concentration was prepared.

[0089] Catalyst C was immersed in the above precursor solution, and excess solution was blown away with compressed air.

[0090] Catalyst C, impregnated with precious metals, was heated at 110°C for 9 hours.

[0091] The dried catalyst was calcined at 750°C in air for 4 hours to obtain a catalyst for later use.

[0092] Example 6:

[0093] This example provides a method for preparing a monolithically honeycomb-supported high-entropy oxide methane / CO2 reforming catalyst.

[0094] The high-entropy oxide synthesized in Example 3, pseudoboehmite, Al(OH)3, 5wt% polyvinyl alcohol aqueous solution, citric acid, and deionized water were mixed in a weight ratio of 1.0:0.3:0.3:0.6-1.0:0.08:3.0 and ball-milled in a high-energy ball mill at 500 rpm for 4-6 hours to obtain slurry A. The average particle size (D50) of slurry A was 3.0 micrometers. Dilute nitric acid was added to adjust the pH of the slurry to a range of 4.0.

[0095] The ceramic honeycomb carrier treated in 2% dilute nitric acid or the metal honeycomb carrier pretreated at high temperature was immersed in the prepared slurry for 2 minutes, and the excess slurry A was blown away with compressed air to obtain sample B.

[0096] Sample B was dried at 120℃ for 6 hours and then weighed.

[0097] Repeat steps (2) and (3) until the target coating amount is reached, with the catalytic coating accounting for 20 wt% of the total catalyst weight.

[0098] Then, the catalyst sample C is prepared by calcining it in a muffle furnace at 900°C under air atmosphere for 2-6 hours, preferably 3-4 hours, to obtain the catalyst sample C for later use.

[0099] The noble metals Ru, Rh, and Pt can be directly synthesized into high-entropy metal oxides via solid-state synthesis, co-precipitation, or gel-gel methods. Alternatively, they can be loaded onto the surface of catalyst C via impregnation. The specific steps are as follows:

[0100] Based on the water absorption rate of catalyst C, a certain concentration of Ru, Rh and Pt precursor solutions were prepared.

[0101] Catalyst C was immersed in the above precursor solution, and excess solution was blown away with compressed air.

[0102] The catalyst C, impregnated with precious metals, was dried at 100°C for 8 hours.

[0103] The dried catalyst is calcined at 750°C in air for 2-6 hours, preferably 2-4 hours, to obtain the catalyst for later use.

[0104] Application Example 1:

[0105] This embodiment provides an application of a monolithic honeycomb supported high-entropy oxide catalyst in methane / CO2 reforming.

[0106] The monolithic catalyst prepared in Example 4 was placed in a fixed-bed reactor and subjected to dry reforming at 650°C with a mixed gas flow rate of 100 mL / min and CH4 / CO2 / N2 = 1 / 1 / 3. The conversion rates of CH4 and CO2 reached 94% and 98%, respectively, and the H2 selectivity reached 98%. After a 48-hour stability test, the activity remained essentially unchanged, and no deactivation occurred.

[0107] Application Example 2:

[0108] This embodiment provides an application of a monolithic honeycomb supported high-entropy oxide catalyst in methane / CO2 reforming.

[0109] The monolithic catalyst prepared in Example 5 was placed in a fixed-bed reactor and subjected to dry reforming at 700°C with a mixed gas flow rate of 100 mL / min and CH4 / CO2 / N2 = 1 / 1 / 3. The conversion rates of CH4 and CO2 reached 93% and 96%, respectively, and the H2 selectivity reached 97%. After a 48-hour stability test, the activity remained essentially unchanged, and no deactivation occurred.

[0110] Application Example 3:

[0111] This embodiment provides an application of a monolithic honeycomb supported high-entropy oxide catalyst in methane / CO2 reforming.

[0112] The monolithic catalyst prepared in Example 6 was placed in a fixed-bed reactor and subjected to dry reforming at 700°C with a mixed gas flow rate of 100 mL / min and CH4 / CO2 / N2 = 1 / 1 / 3. The conversion rates of CH4 and CO2 reached 95% and 92%, respectively, and the H2 selectivity reached 98%. After a 48-hour stability test, the activity remained essentially unchanged, and no deactivation occurred.

[0113] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A catalyst for a honeycomb-supported high-entropy oxide, characterized in that, It includes a honeycomb carrier and a catalytic coating, wherein the catalytic coating is loaded on the honeycomb carrier; The catalytic coating is a high-entropy oxide; The high-entropy oxide includes a base element and an active element; The base element is selected from at least five of the following: Mg, Al, Ce, La, Sr, W, K, Zr, Mn, Ba, Si, Nb, Mo, Nd, Gd, and Cu. The active element is selected from at least one of Ni, Co, Ru, Rh, Ir, and Pt.

2. The catalyst according to claim 1, characterized in that, The catalytic coating accounts for 5-30 wt% of the mass percentage of the catalyst. Each element in the substrate independently accounts for 5.0~50 wt% of the mass of the catalytic coating; Ni and Co elements in the active elements independently account for 5.0~50 wt% of the mass of the catalytic coating; The active elements Ru, Rh, Ir, and Pt independently account for 0-5 wt% of the mass of the catalyst coating; In the high-entropy oxide, the molar ratios of all elements except Ru, Rh, Ir, and Pt are the same; The cellular carrier is selected from ceramic cellular carriers and / or metal cellular carriers.

3. A method for preparing the catalyst according to claim 1 or 2, characterized in that, Includes the following steps: A) High-entropy oxides are synthesized from precursors containing base elements and active elements using solid-phase synthesis, precipitation, or sol-gel methods. The base element is selected from at least five of the following: Mg, Al, Ce, La, Sr, W, K, Zr, Mn, Ba, Si, Nb, Mo, Nd, and Gd. The active element is selected from at least one of Ni, Co, Ru, Rh, Ir, and Pt; B) The mixed slurry containing the high-entropy oxide, pseudoboehmite, Al(OH)3, polyvinyl alcohol, citric acid, and water is ball-milled to obtain slurry A; C) The honeycomb carrier is impregnated in the slurry A and dried to obtain sample B; D) The sample B was calcined in an air atmosphere to obtain the catalyst.

4. The preparation method according to claim 3, characterized in that, The mass ratio of the high-entropy oxide to pseudoboehmite, Al(OH)3, polyvinyl alcohol, citric acid, and water is 1:0.1~0.5:0.2~1.0:0.5~2.0:0.05~2.0:2.0~4.0; The solid-liquid ratio of the honeycomb carrier to the slurry A is 1:1~3; The cellular carrier is selected from ceramic cellular carriers and / or metal cellular carriers; The cellular carrier is treated with acid before use.

5. The preparation method according to claim 3, characterized in that, In step B), the ball mill rotation speed is 300~800 r / min, and the ball milling time is 2~10 h; The average particle size of slurry A is 1.0~4.0μm; The pH value of the slurry A is 2~5; In step C), the immersion time is 1-3 minutes; In step C), the drying temperature is 100~150℃, and the drying time is 2~10h; In step D), the roasting temperature is 600~900℃ and the roasting time is 2~6h.

6. The preparation method according to claim 3, characterized in that, The solid-phase synthesis method is as follows: a precursor containing a base element and an active element is mixed with ethanol, ball-milled at a speed of 300-800 r / min for 6-10 h, dried at 110-150℃ for 5-12 h, and calcined at 600-1100℃ for 3-5 h to obtain the high-entropy oxide, wherein the precursor containing the base element and the active element is an oxide containing the base element and the active element.

7. The preparation method according to claim 3, characterized in that, The precipitation method includes the following steps: (1) A precursor containing base elements and active elements is mixed with sodium carbonate and reacted to obtain a gel-like precipitate; (2) The gel-like precipitate is dried at 60~120℃ for 24~48h and calcined at 700~1000℃ for 3~h to obtain the high-entropy oxide; The precursor containing the base element and the active element is selected from at least one of nitrate, hydrochloride, and acetate containing the base element and the active element; The molar ratio of the precursor containing the base element and the active element to the sodium carbonate is 1:1.0~1.2, based on the total molar amount of the base element and the active element.

8. The preparation method according to claim 3, characterized in that, The sol-gel method includes the following steps: The precursor containing the base element and the active element is mixed with an organic acid, dried at 120-130℃, and calcined at 700-1100℃ for 3-5 hours to obtain the high-entropy oxide. The precursor containing the base element and the active element is selected from at least one of nitrate, hydrochloride, and acetate containing the base element and the active element; The organic acid is selected from citric acid and / or glycine; The molar ratio of the precursor containing the base element and the active element to the organic acid is 1:1.0~1.2, based on the total molar amount of the base element and the active element.

9. The preparation method according to claim 3, characterized in that, The catalyst also includes a post-treatment process: The catalyst is impregnated in a noble metal salt solution and calcined at 700-900°C for 2-6 hours under an oxygen-containing atmosphere, wherein the noble metal element in the noble metal salt solution is selected from at least one of Ru, Rh or Pt. The solid-liquid ratio of the catalyst to the noble metal salt solution is 1:0.5~1.5; The concentration of the noble metal salt solution is 2~10 mg / mL.

10. The use of a catalyst according to claim 1 or 2, or a catalyst obtained by the preparation method according to any one of claims 3 to 9, in the reaction of methane and CO2 reforming to produce syngas.

Citation Information

Patent Citations

  • A new class of high-entropy perovskite ceramics with robust ferroelectricity

    AU2021102229A4

  • High-entropy oxides for thermal barrier coating (TBC) top coats

    CA3106049A1

  • Plasma cladding in-situ synthesized TiB2-TiC-TiN reinforced high-entropy alloy coating material and preparation method thereof

    CN103484810B

  • A high-entropy oxide amorphous material and its preparation method

    CN108821571B

  • High temperature and hydrochloric acid corrosion resistant synthetic furnace composite material and preparation method thereof