In-situ synthesis of catalysts for supported high-entropy oxides, their preparation methods and applications

By synthesizing high-entropy oxide catalysts in situ on a honeycomb support, the problems of catalyst deactivation and carbon deposition under high temperature and high pressure were solved, achieving a highly efficient methane/CO2 reforming reaction, simplifying the preparation process and improving catalytic performance.

CN118217998BActive Publication Date: 2026-11-17DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 20 Cites 0 Cited by

Patent Information

Application Number
CN202211617985.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-15
Publication Date
2026-11-17
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

Existing methane dry reforming catalysts are prone to deactivation and carbon deposition under high temperature and high pressure, and the heat and mass transfer control is complex, resulting in a decline in catalytic performance.

Method used

In-situ synthesis and supported high-entropy oxide catalysts were employed. By loading a high-entropy oxide coating onto a honeycomb support and combining it with an alumina coating, the preparation process was simplified, the hydrothermal stability and anti-carbon deposition performance of the catalyst were improved, and the heat and mass transfer performance was enhanced.

Benefits of technology

This approach enables the catalyst to maintain high activity and resistance to carbon deposition at high temperatures, simplifies the preparation process, and improves the efficiency and stability of the methane/CO2 reforming reaction.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This application discloses an in-situ synthesis-supported high-entropy oxide catalyst, its preparation method, and its application. The catalyst comprises a honeycomb support and a catalytic coating, the catalytic coating being supported on the surface of the honeycomb support; the inner layer of the catalytic coating is an alumina coating; and the outer layer of the catalytic coating is a high-entropy oxide coating. The catalyst exhibits excellent high-temperature hydrothermal stability and anti-carbon deposition ability in the methane / CO2 reforming reaction, and maintains high catalytic activity under high-temperature reducing atmospheres, providing a new approach for catalyst development under high-temperature and high-hydrothermal conditions. This invention also provides an in-situ synthesis and supporting method for high-entropy metal oxides with an integral honeycomb structure, simplifying the preparation process, improving technical and economic efficiency, and facilitating the industrial application of the technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to a catalyst for in-situ synthesis of supported high-entropy oxides, its preparation method, and its application, belonging to the field of catalytic material preparation. Background Technology

[0002] Carbon dioxide and methane are typical greenhouse gases, and their efficient conversion and resource utilization are particularly important. Dry reforming (DRM) of methane can directly convert these two greenhouse gases into syngas, reducing energy consumption while alleviating pressure on greenhouse gas emission reduction, thus offering both environmental and economic benefits. However, the DRM reaction requires high temperature (700-850℃) and a strongly reducing reaction atmosphere, necessitating catalysts with excellent anti-sintering, anti-carbonization, and hydrothermal resistance properties.

[0003] High entropy oxides (HEOs) maintain a stable structure even under extreme operating conditions due to their thermodynamic high entropy effect and kinetic hysteresis diffusion effect. Since their inception, HEOs have attracted widespread attention and hold promise for applications in various fields, such as high entropy alloys (CN109182877A), high entropy alloy coatings (CN103484810B), high entropy ceramics (AU2021102229A4, CN111763087A), high entropy semiconductors or insulators (TWI395336B), corrosion-resistant coatings (CN108914041B, CN108914041A), high entropy oxide amorphous materials (CN108821571B), and high thermal conductivity materials. The above-mentioned applications, including (WO2022160471A1), refractory alloys (CN109182877B), high electrical conductivity (CN113023777A), thermal barrier coatings (SG11202100226YA, EP3863990A2, CA3106049A1, WO2020142125A3), electrochromic materials (CN112340787A), and strong magnetic materials (WO2019109059A1), are mainly based on their excellent thermal conductivity, electrical conductivity, and corrosion resistance. However, their application in the catalytic field is relatively limited, with only (US20220134316A1) applying it to the catalytic oxidation reaction of CO; patent CN111790397A discloses a high-entropy metal oxide catalyst for the catalytic oxidation and removal of aromatic organic sulfur compounds from fuel oil. High-entropy oxides possess high thermal stability and conductivity, along with multi-component tunable properties, which can address the requirement for high hydrothermal stability in catalysts during methane-CO2 reforming. Furthermore, since the reaction is affected by heat and mass transfer, the high mass transfer performance of the overall structured catalyst helps eliminate bed hotspots and avoid carbon deposition problems caused by uneven temperature distribution. However, the conventional process of first synthesizing high-entropy oxides and then supporting them is complex; in-situ synthesis and support methods can simplify the process. Summary of the Invention

[0004] To overcome the problems of poor hydrothermal stability, easy carbon deposition and deactivation, and mass and heat transfer control of methane dry reforming catalysts, this invention discloses a high-entropy metal oxide methane dry reforming catalyst. High-entropy metal oxides possess excellent high-temperature hydrothermal stability and tunable structural properties; simultaneously, the low diffusion resistance of the monolithic catalyst structure avoids temperature gradients on the catalyst; and the in-situ synthesis and loading method simplifies the catalyst preparation process. The technical problem to be solved is to provide a methane / CO2 reforming catalyst with excellent hydrothermal stability and resistance to carbon deposition, and its preparation method.

[0005] According to one aspect of this application, a catalyst for in-situ synthesis of supported high-entropy oxides is provided, comprising a honeycomb support and a catalytic coating, the catalytic coating being supported on the surface of the honeycomb support;

[0006] The inner layer of the catalytic coating is an alumina coating;

[0007] The outer layer of the catalytic coating is a high-entropy oxide coating;

[0008] The high-entropy oxide includes a first element and a second element;

[0009] The first element is selected from at least five of the following: Mg, Al, Ce, La, Sr, W, K, Zr, Mn, Ba, Si, Nb, Mo, Nd, and Gd.

[0010] The second element is selected from at least one of Ni, Co, Ru, Rh, Ir, and Pt.

[0011] Optionally, the catalytic coating accounts for 5 to 20 wt% of the catalyst mass.

[0012] Optionally, the alumina coating accounts for 5 to 15 wt% of the catalyst mass.

[0013] Optionally, the high-entropy oxide coating accounts for 5 to 10 wt% of the catalyst mass.

[0014] Optionally, each element in the first element independently accounts for 5 to 50 wt% of the mass of the high-entropy oxide.

[0015] Optionally, each element in the first element independently accounts for any value or a range between two values ​​from 5wt%, 15wt%, 25wt%, 35wt%, and 55wt% of the mass of the high-entropy oxide.

[0016] Optionally, each of the elements Ru, Rh, Ir, and Pt in the second element independently accounts for 0 to 5 wt% of the mass of the high-entropy oxide.

[0017] Optionally, Ni or Co in the second element independently accounts for 5 to 50% of the mass of the high-entropy oxide.

[0018] Optionally, Ni or Co in the second element independently accounts for any value or a range between 5 wt%, 15 wt%, 25 wt%, 35 wt%, and 55 wt% of the mass of the high-entropy oxide.

[0019] Optionally, the molar ratios of all elements except Ru, Rh, Ir, and Pt in the high-entropy oxide are the same.

[0020] Optionally, the cellular carrier is selected from ceramic cellular carriers and / or metal cellular ceramics.

[0021] According to another aspect of this application, a method for preparing the above-mentioned catalyst is provided, comprising the following steps:

[0022] (1) A mixture of γ-Al2O3, boehmite, Al(OH)3, polyvinyl alcohol, citric acid and water was ball-milled to obtain slurry A;

[0023] (2) The honeycomb carrier is immersed in the slurry A, dried I, and calcined I under an oxygen-containing atmosphere to obtain an intermediate with an alumina coating;

[0024] (3) The intermediate with the alumina coating is immersed in a precursor solution containing the first element and the second element in equal volume, dried (II), and calcined (II) under a reducing atmosphere to obtain the catalyst;

[0025] The first element is selected from at least five of the following: Mg, Al, Ce, La, Sr, W, K, Zr, Mn, Ba, Si, Nb, Mo, Nd, and Gd.

[0026] The second element is selected from at least one of Ni, Co, Ru, Rh, Ir, and Pt.

[0027] Optionally, the mass ratio of γ-Al2O3, pseudoboehmite, Al(OH)3, polyvinyl alcohol, citric acid, and water is 1:0.1-0.5:0.2-1.0:0.5-2.0:0.05-0.2:2.0-4.0.

[0028] Optionally, the precursor solution containing the first element and the second element is selected from at least one of nitrates, hydrochlorides, and acetates containing the first element and the second element.

[0029] Optionally, the cellular carrier is selected from ceramic cellular carriers and / or metal cellular ceramics;

[0030] The cellular carrier is acid-treated before use.

[0031] Optionally, in step (1), the rotation speed of the ball mill is 300-800 r / min, and the ball milling time is 2-10 h.

[0032] Optionally, in step (1), the average particle size of the slurry A is 1.0 to 4.0 μm.

[0033] Optionally, in step (1), the pH of the slurry A is 1.0 to 6.0.

[0034] Optionally, in step (2), the soaking time is 1 to 3 minutes.

[0035] Optionally, in step (2), the temperature of drying I is 100-150°C, and the drying time is 2-10 hours.

[0036] Optionally, in step (2), the temperature of calcination I is 600-900°C, and the calcination time is 2-6 hours.

[0037] Optionally, the drying temperature in step (3) is 100-150°C, and the drying time is 2-10 hours.

[0038] Optionally, in step (3), the roasting time of the second step is 700-1100°C and the roasting time of the second step is 2-8 hours.

[0039] Optionally, the solid-liquid ratio of the honeycomb carrier to the slurry A is 1:1 to 3.

[0040] According to another aspect of this application, the application of the above-described catalyst or the catalyst obtained according to the above-described preparation method is provided in the reaction of reforming methane and CO2 to produce syngas.

[0041] The beneficial effects that this application can produce include:

[0042] 1) The catalyst for in-situ synthesis-supported high-entropy oxides provided in this application has excellent high-temperature hydrothermal stability and anti-carbon deposition properties.

[0043] 2) The in-situ synthesis-supported high-entropy oxide catalyst provided in this application has the high-entropy oxide supported on a honeycomb support with an alumina layer. The overall structure of the catalyst enhances heat and mass transfer and improves the performance of strong endothermic catalytic reactions.

[0044] 3) The preparation method provided in this application is simple in process and easy to be applied in engineering.

[0045] 4) The catalyst provided in this application has excellent high-temperature hydrothermal stability and anti-carbon deposition ability in methane / CO2 reforming reaction, and can maintain high catalytic activity under high-temperature reducing atmosphere. Detailed Implementation

[0046] The present application is described in detail below with reference to the embodiments, but the present application is not limited to these embodiments.

[0047] Unless otherwise specified, all raw materials used in the embodiments of this application were purchased through commercial channels.

[0048] In the embodiments of this application, the CO2 conversion rate, CH4 conversion rate, and H2 selectivity are calculated as follows:

[0049] CO2 conversion rate

[0050] CH4 conversion rate

[0051] H2 selectivity is

[0052] In the embodiments of this application, CO2 conversion rate, CH4 conversion rate, and H2 selectivity are all calculated based on the number of carbon moles.

[0053] Example 1:

[0054] This example provides a method for preparing a monolithic honeycomb in-situ synthesis of a supported high-entropy metal oxide methane / CO2 reforming catalyst.

[0055] 1. γ-Al2O3, boehmite, Al(OH)3, 5wt% polyvinyl alcohol aqueous solution, citric acid, and deionized water were mixed in a weight ratio of 1.0:0.2:0.6:0.5:0.15:2.5;

[0056] 2. The mixed slurry from step 1 is ball-milled in a high-energy ball mill at a speed of 500 rpm for 5 hours to obtain slurry A. The average particle size (D50) of slurry A is 2.0 micrometers. Dilute nitric acid is added to adjust the pH value of the slurry to be within the range of 4.0.

[0057] 3. Immerse the ceramic honeycomb carrier treated in 2% dilute nitric acid or the metal honeycomb carrier pretreated at high temperature in the slurry prepared in step 2 for 3 minutes, blow away the excess slurry A with compressed air to obtain sample B; dry sample B at 150°C for 8 hours and weigh it; repeat this step according to the coating amount until the target coating amount is reached.

[0058] 4. Then, the sample C with an inner layer was prepared by calcining in a muffle furnace at 800°C in air atmosphere for 6 hours to obtain the inner layer coating, which accounts for 10 wt.% of the total catalyst weight.

[0059] 5. Prepare a salt solution D of Ni, Mg, Al, Ce, Si, La, Co and Ru precursors, with the outer high-entropy metal oxide accounting for 5% of the total catalyst weight, wherein the non-noble metal elements have the same molar number;

[0060] 6. Immerse catalyst C in the above precursor solution D, and blow away excess solution with compressed air;

[0061] 7. Dry sample C, which has been impregnated with solution D, at 120°C for 10 hours;

[0062] 8. The dried sample was calcined at 700°C for 2 hours in air to obtain catalyst E for in-situ synthesis of supported high-entropy metal oxides for later use.

[0063] Example 2:

[0064] This example provides a method for preparing a monolithic honeycomb in-situ synthesis of a supported high-entropy metal oxide methane / CO2 reforming catalyst.

[0065] 1. γ-Al2O3, boehmite, Al(OH)3, 5wt% polyvinyl alcohol aqueous solution, citric acid, and deionized water were mixed in a weight ratio of 1.0:0.2:0.6:0.5:0.15:2.5;

[0066] 2. The mixed slurry from step 1 is ball-milled in a high-energy ball mill at a speed of 500 rpm for 5 hours to obtain slurry A. The average particle size (D50) of slurry A is 2.0 micrometers. Dilute nitric acid is added to adjust the pH value of the slurry to be within the range of 4.0.

[0067] 3. Immerse the ceramic honeycomb carrier treated in 2% dilute nitric acid or the metal honeycomb carrier pretreated at high temperature in the slurry prepared in step 2 for 3 minutes, blow away the excess slurry A with compressed air to obtain sample B; dry sample B at 150°C for 8 hours and weigh it; repeat this step according to the coating amount until the target coating amount is reached.

[0068] 4. Then, the sample C with the inner layer is calcined in a muffle furnace at 800°C in air atmosphere for 6 hours to obtain the inner layer catalytic coating, which accounts for 10 wt.% of the total catalyst weight.

[0069] 5. Prepare salt solutions D of Ni, Sr, Mn, Mg, Al, Nd, Ce, La and Ru, Pt precursors, with the outer high-entropy metal oxide accounting for 5% of the total catalyst weight, wherein the non-noble metal elements have the same molar number;

[0070] 6. Immerse catalyst C in the above precursor solution D, and blow away excess solution with compressed air;

[0071] 7. Dry sample C, which has been impregnated with solution D, at 120°C for 10 hours;

[0072] 8. The dried sample was calcined at 700°C for 2 hours in air to obtain catalyst E for in-situ synthesis of supported high-entropy metal oxides for later use.

[0073] Example 3:

[0074] This example provides a method for preparing a monolithic honeycomb in-situ synthesis of a supported high-entropy metal oxide methane / CO2 reforming catalyst.

[0075] 1. γ-Al2O3, boehmite, Al(OH)3, 5wt% polyvinyl alcohol aqueous solution, citric acid, and deionized water were mixed in a weight ratio of 1.0:0.2:0.6:0.5:0.15:2.5;

[0076] 2. The mixed slurry from step 1 is ball-milled in a high-energy ball mill at a speed of 500 rpm for 5 hours to obtain slurry A. The average particle size (D50) of slurry A is 2.0 micrometers. Dilute nitric acid is added to adjust the pH value of the slurry to be within the range of 4.0.

[0077] 3. Immerse the ceramic honeycomb carrier treated in 2% dilute nitric acid or the metal honeycomb carrier pretreated at high temperature in the slurry prepared in step 2 for 3 minutes, blow away the excess slurry A with compressed air to obtain sample B; dry sample B at 150°C for 8 hours and weigh it; repeat this step according to the coating amount until the target coating amount is reached.

[0078] 4. Then, the sample C with the inner layer is calcined in a muffle furnace at 800°C in air atmosphere for 6 hours to obtain the inner layer catalytic coating, which accounts for 10 wt.% of the total catalyst weight.

[0079] 5. Prepare a salt solution D of Ni, Mg, Al, Ce, W, Zr, Ba, Co and Ru, Rh precursors, with the outer high-entropy metal oxide accounting for 5% of the total catalyst weight, wherein the non-noble metal elements have the same molar number;

[0080] 6. Immerse catalyst C in the above precursor solution D, and blow away excess solution with compressed air;

[0081] 7. Dry sample C, which has been impregnated with solution D, at 120°C for 10 hours;

[0082] 8. The dried sample was calcined at 700°C for 2 hours in air to obtain catalyst E for in-situ synthesis of supported high-entropy metal oxides for later use.

[0083] Application Example 1:

[0084] This embodiment provides an application of a monolithic honeycomb supported high-entropy oxide catalyst in methane / CO2 reforming.

[0085] The monolithic catalyst prepared in Example 1 was placed in a fixed-bed reactor, and a dry reforming reaction was carried out at 650°C with a mixed gas flow rate of 100 mL / min and CH4 / CO2 / N2 = 1 / 1 / 3. The conversion rates of CH4 and CO2 reached 94% and 98%, respectively, and the H2 selectivity reached 99%. After a 48-hour stability test, the activity remained essentially unchanged, and no deactivation occurred.

[0086] Application Example 2:

[0087] This embodiment provides an application of a monolithic honeycomb supported high-entropy oxide catalyst in methane / CO2 reforming.

[0088] The monolithic catalyst prepared in Example 2 was placed in a fixed-bed reactor, and a dry reforming reaction was carried out at 700°C with a mixed gas flow rate of 100 mL / min and CH4 / CO2 / N2 = 1 / 1 / 3. The conversion rates of CH4 and CO2 reached 92% and 95%, respectively, and the H2 selectivity reached 96%. After a 48-hour stability test, the activity remained essentially unchanged, and no deactivation occurred.

[0089] Application Example 3:

[0090] This embodiment provides an application of a monolithic honeycomb supported high-entropy oxide catalyst in methane / CO2 reforming.

[0091] The monolithic catalyst prepared in Example 2 was placed in a fixed-bed reactor, and a dry reforming reaction was carried out at 700°C with a mixed gas flow rate of 100 mL / min and CH4 / CO2 / N2 = 1 / 1 / 3. The conversion rates of CH4 and CO2 reached 97% and 95%, respectively, and the H2 selectivity reached 99%. After a 48-hour stability test, the activity remained essentially unchanged, and no deactivation occurred.

[0092] The above description is merely a few embodiments of this application and is not intended to limit this application in any way. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A catalyst for in-situ synthesis of supported high-entropy oxides, characterized in that, It includes a honeycomb carrier and a catalytic coating, wherein the catalytic coating is loaded on the surface of the honeycomb carrier; The inner layer of the catalytic coating is an alumina coating; The outer layer of the catalytic coating is a high-entropy oxide coating; The high-entropy oxide includes a first element and a second element; The first element is selected from at least five of the following: Mg, Al, Ce, La, Sr, W, K, Zr, Mn, Ba, Si, Nb, Mo, Nd, and Gd. The second element is selected from at least one of Ni, Co, Ru, Rh, Ir, and Pt.

2. The catalyst according to claim 1, characterized in that, The catalytic coating accounts for 5-20 wt% of the mass of the catalyst. The alumina coating accounts for 5-15 wt% of the catalyst mass; The high-entropy oxide coating accounts for 5-10 wt% of the catalyst mass. Each element in the first element independently accounts for 5-50 wt% of the mass of the high-entropy oxide; Each of the elements Ru, Rh, Ir, and Pt in the second element independently accounts for 0-5 wt% of the mass of the high-entropy oxide; Ni or Co in the second element independently constitutes 5-50 wt% of the mass of the high-entropy oxide; In the high-entropy oxide, the molar ratios of all elements except Ru, Rh, Ir, and Pt are the same; The cellular carrier is selected from ceramic cellular carriers and / or metal cellular ceramics.

3. A method for preparing the catalyst according to claim 1 or 2, characterized in that, Includes the following steps: (1) A mixture of γ-Al2O3, boehmite, Al(OH)3, polyvinyl alcohol, citric acid and water was ball-milled to obtain slurry A; (2) The honeycomb carrier is immersed in the slurry A, dried I, and calcined I under an oxygen-containing atmosphere to obtain an intermediate with an alumina coating; (3) The intermediate with the alumina coating is immersed in a precursor solution containing the first element and the second element in equal volume, dried (II), and calcined (II) under a reducing atmosphere to obtain the catalyst; The first element is selected from at least five of the following: Mg, Al, Ce, La, Sr, W, K, Zr, Mn, Ba, Si, Nb, Mo, Nd, and Gd. The second element is selected from at least one of Ni, Co, Ru, Rh, Ir, and Pt.

4. The preparation method according to claim 3, characterized in that, The mass ratio of γ-Al2O3, pseudoboehmite, Al(OH)3, polyvinyl alcohol, citric acid, and water is 1:0.1~0.5:0.2~1.0:0.5~2.0:0.05~0.2:2.0~4.

0.

5. The preparation method according to claim 3, characterized in that, The precursor solution containing the first element and the second element is selected from at least one of nitrate, hydrochloride, and acetate containing the first element and the second element. The cellular carrier is selected from ceramic cellular carriers and / or metal cellular ceramics; The cellular carrier is acid-treated before use.

6. The preparation method according to claim 3, characterized in that, In step (1), the rotation speed of the ball mill is 300~800 r / min, and the ball milling time is 2~10 h; In step (1), the average particle size of the slurry A is 1.0~4.0μm; In step (1), the pH of the slurry A is 1.0~6.

0.

7. The preparation method according to claim 3, characterized in that, In step (2), the soaking time is 1~3 minutes; In step (2), the temperature of drying I is 100~150℃, and the drying time is 2~10h; In step (2), the temperature of calcination I is 600~900℃, and the calcination time is 2~6h.

8. The preparation method according to claim 3, characterized in that, In step (3), the temperature of drying II is 100~150℃, and the drying time of drying II is 2~10h; In step (3), the roasting time of step II is 700~1100℃ and the roasting time of step II is 2~8h.

9. The preparation method according to claim 3, characterized in that, The solid-liquid ratio of the honeycomb carrier to the slurry A is 1:1~3.

10. The use of a catalyst according to claim 1 or 2, or a catalyst obtained by the preparation method according to any one of claims 3 to 9, in the reaction of methane and CO2 reforming to produce syngas.

Citation Information

Patent Citations

  • A new class of high-entropy perovskite ceramics with robust ferroelectricity

    AU2021102229A4

  • High-entropy oxides for thermal barrier coating (TBC) top coats

    CA3106049A1

  • Plasma cladding in-situ synthesized TiB2-TiC-TiN reinforced high-entropy alloy coating material and preparation method thereof

    CN103484810B

  • A high-entropy oxide amorphous material and its preparation method

    CN108821571B

  • High temperature and hydrochloric acid corrosion resistant synthetic furnace composite material and preparation method thereof

    CN108914041A