A Defect Repair Method Utilizing Friction Stir Solid-Phase Deposition Additive Technology
By using arc-shaped channels, spiral grooves, and induction heating coils in friction stir solid-state deposition additive manufacturing technology, the problems of inflexible selection of additive raw material diameter and interruption of repair process in existing technologies have been solved, enabling rapid and continuous repair of defects in metal components and improving repair efficiency and applicability.
Patent Information
- Application Number
- CN202410557341.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-07
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-05-07
AI Technical Summary
Existing friction stir solid-state deposition additive manufacturing technology has several drawbacks when repairing defects in metal components. These include inflexible selection of additive feedstock diameter, difficulty in adapting to different defect sizes, easy interruption of the repair process, and high material damping around the discharge port, making it difficult to quickly introduce feedstock.
By employing friction stir solid-phase deposition additive manufacturing technology, an arc-shaped channel is set at the bottom of the tool head and a spiral groove is set on the stirring needle. Combined with an induction heating coil, the metal wire can be rapidly plasticized and continuously fed in, avoiding material blockage in the inner cavity of the tool head. The spiral groove and concave area work together to ensure that the material quickly fills the defects.
It enables the rapid introduction of additive raw materials into the mixing needle area to fill defects, avoids keyholes, ensures continuous repair process, improves defect repair efficiency and flexibility, adapts to various types of defects, and reduces raw material replacement time.
Smart Images

Figure CN118218747B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of metal component defect repair technology, specifically relating to a defect repair method using friction stir solid-state deposition additive technology. Background Technology
[0002] For many metal components of high-end equipment such as aerospace, vehicle transportation, and weaponry, exploring suitable repair processes to repair damaged components not only extends their service life but also avoids material waste caused by replacing new parts, thus reducing their operating costs.
[0003] Practice has proven that friction stir solid-state deposition (FSD) additive manufacturing technology can effectively repair defects in metal components (such as point defects, strip defects, and pore defects). In the prior art, US 9862054B2 discloses an extrusion-type FSD additive manufacturing process. This process involves feeding a rod-shaped material, which undergoes frictional stirring with the component to be repaired. Under thermomechanical coupling, the fed material plasticizes with the surface material of the component, bridging the defects. However, this approach has several problems: it cannot flexibly select the diameter of the additive raw material (rod), resulting in poor adaptability to defect sizes; continuous repair is difficult to achieve, as changing the rod interrupts the repair process, leading to joints in the repair layer and creating weak areas.
[0004] A previously developed floating solid-phase additive repair device (CN115502544B) involves introducing metal wire into a chamber from above a stirring pin, cutting and plasticizing it using a rotating thread, and then introducing the plasticized material into the stirring pin to achieve frictional solid-phase additive manufacturing. However, when using this device to repair internal defects, the material around the outlet exhibits significant damping, making it difficult to discharge smoothly. This hinders the rapid introduction of additive raw materials into the area where the stirring pin is located to fill the defects, and keyholes may appear during the lifting of the stirring pin. Summary of the Invention
[0005] This invention provides a defect repair method using friction stir solid phase deposition additive technology. This method can at least quickly introduce additive raw materials into the area where the stirring needle is located to fill the defect, while avoiding keyholes during the lifting of the stirring needle.
[0006] The present invention adopts the following technical solution.
[0007] A defect repair method using friction stir solid-state deposition additive manufacturing technology, comprising the following steps: Step 1: Determine the location of the defect to be repaired on the workpiece; Step 2: Pre-process the defect location to be repaired; Step 3: Install the friction stir solid-state deposition additive repair equipment and install a back support on the back side of the defect location on the workpiece. Step 4: Start the friction stir solid-phase deposition additive repair equipment, move its tool head to the defect repair starting point, and then perform defect repair, so that the plasticized metal material fills and repairs the defect location; Step 5: After the defect repair is completed, control the tool head to be raised to the specified height, turn off the friction stir solid phase deposition additive repair equipment, and remove the back support; Step 6: Perform post-processing on the repaired area.
[0008] As a preferred option, when the defect depth exceeds 2mm, a groove is pre-cut at the defect before pretreatment.
[0009] Furthermore, during the defect repair process, feeding stops whenever the tool head moves forward and leaves the original defect position, and then the tool head is adjusted back to the starting position before feeding continues.
[0010] In this invention, the stir-friction solid-phase deposition additive repair equipment includes: The main shaft and wire feeding mechanism are connected to the main body of the friction stir additive manufacturing equipment. The tool head is connected to the end of the main shaft. The wire feeding mechanism is arranged on the side of the tool head and rotates synchronously with the tool head during the friction stir additive manufacturing process. An arc-shaped channel is provided at the lower part of the tool head. The arc-shaped channel extends from the outer wall of the bottom of the tool head inward to the area near the middle of the lower end face of the tool head, and the diameter of the arc-shaped channel gradually decreases from the outside to the inside. A stirring pin is provided at the lower end of the tool head. During the friction stir additive manufacturing process, the metal wire continuously fed by the wire feeding mechanism enters the inner end of the arc-shaped channel laterally and is continuously plasticized under the spinning action of the lower end face of the tool head and the stirring action of the stirring pin. The wire feeding mechanism includes a cantilever fixedly connected to the upper part of the main shaft, on which a wire spool is mounted. The axis of the wire spool is perpendicular to the main shaft. A bracket is mounted inside the wire spool and above the tool head. A roller assembly is mounted on the bracket, and a heating module is mounted inside the roller assembly. The metal wire drawn from the wire spool passes through the roller assembly, then through the heating module, and then enters the arc-shaped channel laterally. As a more preferred and ingenious solution, the heating module uses an induction heating coil. The axis of the induction heating coil coincides with the center line of the arc-shaped channel entrance. The induction heating coil can both quickly heat the metal wire and guide and stably feed the wire.
[0011] In order to introduce additive raw materials into the area where the stirring pin is located more quickly to fill defects, a spiral groove is provided on the stirring pin. The upper end of the spiral groove extends to the root of the stirring pin and is close to the inner end of the arc-shaped channel, and the lower end of the spiral groove extends to the lower end of the stirring pin.
[0012] In order to plasticize and cut the fed metal wire more quickly and smoothly, a concave area is provided at the root of the stirring needle. The junction of the concave area and the arc-shaped channel is on the same plane as the lower end face of the tool head. The concave area is also directly connected to the spiral groove. During the defect repair process, the fed metal wire is crushed / cut through this junction.
[0013] As a preferred option, the arc-shaped channel adopts an arc-shaped open groove set at the bottom of the tool head; one section of the heating module is inserted into the arc-shaped channel, and the other end of the heating module is inserted into the bracket.
[0014] As a preferred approach, during defect repair, after completing the additive manufacturing process along a single-layer additive manufacturing path, the tool head is gradually lifted away from the surface of the deposited layer. After continuing to feed the wire for a period of time, it is retracted and directly switched to the next single-layer additive manufacturing path. This ensures that the filler at the final position (end) is sufficient and defect-free, and also utilizes the feeding force of the continuous metal wire to clean up any residual plasticized metal material in the arc-shaped channel.
[0015] During the period when the defect repair is about to end, the tool head is controlled to rotate and slowly rise, with the rising rate of the tool head not exceeding 0.5 mm / s, so as to allow the plasticized metal material to be backfilled into the keyhole.
[0016] Beneficial effects: This invention not only allows for the rapid introduction of additive raw materials into the area where the stirring needle is located to fill defects, but also avoids keyholes during the lifting of the stirring needle. During defect repair, the plasticized metal wire flows and fills quickly, mixing with the existing metal material under the action of the tool head, effectively eliminating defects. More importantly, after being heated by the induction coil, the metal wire is immediately fed into the arc-shaped channel at the lower end of the tool head. As the metal wire continues to be fed in, when it reaches the junction of the concave area and the arc-shaped channel, it is rapidly crushed and broken, forming a plasticized material (this process is fundamentally different from the existing method of spirally breaking / cutting the metal wire, avoiding...). This invention addresses a series of drawbacks caused by the metal wire plasticizing material remaining or temporarily stored in the space above the lower end face / shoulder of the tool head. It fundamentally solves the problem of material blockage within the tool head cavity. This plasticizing material then flows along the spiral grooves on the stirring pin (using the spiral grooves to transfer the plasticizing material downwards), thus combining with the workpiece material agitated by the stirring pin to fill defects. Using this invention, the diameter of the additive raw material (wire) can be flexibly selected, adapting to various types of defect repair. It ensures uninterrupted defect repair, enabling continuous repair work, eliminating the need for material replacement procedures and time during the repair process, improving defect repair efficiency, and allowing for flexible and stable control of the feeding rate, thus expanding its applicability. Attached Figure Description
[0017] Figure 1 This is a partial schematic diagram of the friction-stirred solid-state deposition additive repair equipment in Example 1. Figure 2 This is an enlarged schematic diagram of the tool head of the friction-stirred solid-state deposition additive repair equipment in Example 1. Figure 3 This is a schematic diagram of the friction-stirred solid-state deposition additive repair equipment in Example 2. Figure 4 This is an enlarged schematic diagram of the tool head of the friction-stirred solid-phase deposition additive repair equipment in Example 3. Detailed Implementation
[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention. Example 1
[0019] Combination Figure 1 and Figure 2 As shown, the friction stir solid-state deposition additive repair equipment in this embodiment includes: a main shaft 1 and a wire feeding mechanism. The main shaft 1 is connected to the main body of the friction stir equipment, and a tool head 7 is connected to the end of the main shaft 1. The wire feeding mechanism is arranged on the side of the tool head 7 and rotates synchronously with the tool head 7 during the friction stir additive process. An arc-shaped channel 9 is provided at the lower part of the tool head 7. The arc-shaped channel 9 adopts an arc-shaped open groove set at the bottom end of the tool head 7. The arc-shaped channel 9 extends from the outer wall of the bottom of the tool head 7 inward to the area near the middle of the lower end face of the tool head 7, and the diameter of the arc-shaped channel 9 gradually decreases from the outside to the inside. A stirring needle 8 is provided at the lower end of the tool head 7. During the friction stir additive process, the metal wire continuously fed by the wire feeding mechanism enters the inner end of the arc-shaped channel 9 laterally and is continuously plasticized under the spinning action of the lower end face of the tool head 7 and the stirring action of the stirring needle 8. The wire feeding mechanism includes a cantilever 2 fixedly connected to the upper part of the main shaft 1. A wire spool 3 is mounted on the cantilever 2. The axis of the wire spool 3 is perpendicular to the main shaft 1. A bracket 10 is mounted inside the wire spool 3 and above the tool head 7. A roller group 4 is mounted on the bracket 10. An induction heating coil 6 is mounted inside the roller group 4. The axis of the induction heating coil 6 coincides with the center line of the entrance of the arc-shaped channel 9. The metal wire drawn from the wire spool 3 passes through the roller group 4, passes through the induction heating coil 6, and then enters the arc-shaped channel 9 laterally. A spiral groove 13 is provided on the stirring needle 8. The upper end of the spiral groove 13 extends to the root of the stirring needle 8 and is close to the inner end of the arc-shaped channel 9. The lower end of the spiral groove 13 extends to the lower end of the stirring needle 8. A concave area 14 is provided at the root of the stirring needle 8. The depth of the concave area 14 is 0.5 mm. The outer diameter of the concave area 14 is 5 mm larger than the diameter of the root of the stirring needle 8. The junction 15 between the concave area 14 and the arc-shaped channel 9 is on the same plane as the lower end face of the tool head 7. The concave area 14 is also directly connected to the spiral groove 13. During the defect repair process, the fed metal wire is crushed and cut through the junction 15. The concave area 14 stores some plasticized material to ensure that there is always enough material below the tool head 7 for downward transport along the spiral groove 13.
[0020] A defect repair method using friction stir solid-state deposition additive manufacturing technology, comprising the following steps: Step 1: Determine the location of the 0.5~1mm deep keyhole defect to be repaired on the workpiece (rocket propellant tank), and reserve the tool head start and stop areas before and after the keyhole defect location; Step 2: Pre-treat the defect location to be repaired by cleaning the repair area; Step 3: Install the friction stir solid-state deposition additive repair equipment and install a back support that can move synchronously with the tool head on the back side of the defect location on the workpiece (inside the rocket tank). Step 4: Start the friction stir solid-phase deposition additive repair equipment, move its tool head to the defect repair starting point, and then perform defect repair, so that the plasticized metal material fills and repairs the defect location; Specifically: First, move the tool head to the front of the keyhole defect, then control the tool head to move forward at the set speed. When the tool head moves directly above the starting position of the keyhole defect, control the tool head to start spinning (rotate and press down at a constant speed). When the tool head presses down to the specified height, start feeding the wire and control the tool head to continue moving forward at the set speed. Step 5: After the defect repair is completed, control the tool head to be raised to the specified height, turn off the friction stir solid phase deposition additive repair equipment, and remove the back support; Step 6: Perform post-treatment on the repaired area, sanding away excess material until the surface is smooth.
[0021] During defect repair, the metal wire, driven by the roller assembly 4, smoothly passes through the induction heating coil 6 and is rapidly heated. The heated metal wire then enters the arc-shaped channel 9 laterally. When the tip of the metal wire contacts the junction 15 of the lower end face of the tool head 7, it is quickly crushed and broken, forming a plasticized material. As the tool head 7 moves forward, the plasticized metal material enters the concave area 14 and is transported downwards along the spiral groove 13 on the stirring pin (the spiral groove transfers the plasticized material downwards), thus combining with the workpiece material stirred by the stirring pin to fill the defect. Because the heated metal wire is delivered to the lower end face of the tool head 7 for plasticization in a very short time (instantly), the plasticized metal material does not pass through the cavity above the shoulder, thus avoiding the problem of material blockage in the cavity above the shoulder that interrupts the deposition process, fundamentally solving the material blockage problem. When a defect repair process ends and it is time to switch to the next defect repair process, only a small amount of metal residue remains in the arc-shaped channel at the moment of machine stop. The metal residue in the arc-shaped channel 9 can be cleaned (poked) with the help of a needle-like tool, or the metal wire can be fed in to clean the metal residue in the arc-shaped channel 9. The entire cleaning process can be completed within five seconds (while cleaning the residue in the traditional tool head takes several minutes or even tens of minutes and requires disassembling the tool head for operation), making the operation very convenient. Example 2
[0022] A defect repair method utilizing friction stir solid-state deposition additive manufacturing technology, referring to Example 1, differs from Example 1 in that: [The method combines...] Figure 3 As shown, one end of the induction heating coil 6 is inserted into the arc-shaped channel 9, and the other end of the induction heating coil 6 is attached to the bracket 10. Compared with Embodiment 1, the further advantages of this embodiment include: further shortening the stroke of the metal wire into the junction 15 of the lower end face of the tool head 7, which enables the heated metal wire to be delivered to the lower end face of the tool head 7 for plasticization more quickly. Example 3
[0023] A defect repair method utilizing friction stir solid-state deposition additive manufacturing technology, referring to Example 1, differs from Example 1 in that: [The method combines...] Figure 4 As shown, the concave area 14 is omitted, and the inner end of the arc-shaped channel 9 is directly connected to the top of the spiral groove 13 on the stirring needle. The junction of the inner end of the arc-shaped channel 9 and the top of the spiral groove 13, as well as the flat area of the lower end face of the tool head 7, are used to plasticize the heated metal wire. Example 4
[0024] A defect repair method utilizing friction stir solid-state deposition additive manufacturing technology, employing the friction stir solid-state deposition additive repair equipment described in Example 1, includes the following steps: Step 1: Determine the location of the 2-2.5mm deep strip-shaped defect to be repaired on the workpiece (rocket propellant tank), and reserve the tool head start and stop areas before and after the location of the strip-shaped defect; Step 2: Pre-process the defect location to be repaired. First, excavate and arrange the defect area into a regular shape, and then clean the repair area. Step 3: Install the friction stir solid-state deposition additive repair equipment and install a back support that can move synchronously with the tool head on the back side of the defect location on the workpiece (inside the rocket tank). Step 4: Start the friction stir solid-phase deposition additive repair equipment, move its tool head to the defect repair starting point, and then perform defect repair, so that the plasticized metal material fills and repairs the defect location; Specifically: First, move the tool head to the keyhole defect, then control the tool head to move forward at a set speed. When the tool head is directly above the starting position of the keyhole defect, control the tool head to start spinning (rotating and pressing down at a constant speed). When the tool head is pressed down to the specified height, start feeding wire and control the tool head to continue moving forward at a set speed. When a single-layer repair path is completed, control the tool head to gradually lift away from the deposited layer surface, continue feeding wire for a period of time, then retract and directly switch to the next single-layer repair path. Whenever a repair path is about to be completed, control the tool head to rotate and slowly lift it. The lifting rate of the tool head should not exceed 0.5 mm / s to achieve the backfilling of the keyhole with plasticized metal material. Step 5: After the defect repair is completed, control the tool head to be raised to the specified height, turn off the friction stir solid phase deposition additive repair equipment, and remove the back support; Step 6: Perform post-treatment on the repaired area, sanding away excess material until the surface is smooth.
[0025] The present invention not only enables the rapid introduction of additive raw materials into the area where the stirring needle is located to fill defects, but also avoids keyholes during the lifting of the stirring needle. During defect repair, the plasticized metal wire flows and fills quickly, and mixes with the existing metal material under the action of the tool head, effectively eliminating defects. More importantly, after being heated by the induction coil, the metal wire is immediately fed into the arc-shaped channel at the lower end of the tool head. As the metal wire continues to be fed in, when it moves to the junction of the concave area and the arc-shaped channel, it is rapidly crushed and broken, forming a plasticized material (this process is fundamentally different from the existing method of spirally breaking / cutting the metal wire, avoiding the metal...). This invention addresses a series of drawbacks caused by the plasticizing material remaining or temporarily stored in the space above the lower end face / shoulder of the tool head. It fundamentally solves the problem of material blockage within the tool head cavity. This plasticizing material then flows along the spiral grooves on the stirring pin (using the spiral grooves to transfer the plasticizing material downwards), thus combining with the workpiece material agitated by the stirring pin to fill defects. Using this invention, the diameter of the additive raw material (filament) can be flexibly selected, adapting to various types of defect repair. It ensures uninterrupted defect repair, enabling continuous repair work, eliminating the need for material replacement procedures and time during the repair process, improving defect repair efficiency, and allowing for flexible and stable control of the feeding rate, thus expanding its applicability.
Claims
1. A defect repair method using friction stir solid-state deposition additive manufacturing technology, characterized in that the steps include... include: Step 1: Determine the location of the defect to be repaired on the workpiece; Step 2: Pre-process the defect location to be repaired; Step 3: Install the friction stir solid-state deposition additive repair equipment and install a back support on the back side of the defect location on the workpiece. Step 4: Start the friction stir solid-phase deposition additive repair equipment, move its tool head to the defect repair starting point, and then perform defect repair, so that the plasticized metal material fills and repairs the defect location; Step 5: After the defect repair is completed, control the tool head to be raised to the specified height, turn off the friction stir solid phase deposition additive repair equipment, and remove the back support; Step 6: Perform post-processing on the repaired area; The aforementioned friction-stirred solid-state deposition additive repair equipment includes: The main shaft (1) and the wire feeding mechanism are connected to the main body of the friction stirring equipment. The end of the main shaft (1) is connected to the tool head (7). The wire feeding mechanism is arranged on the side of the tool head (7) and rotates synchronously with the tool head (7) during the friction stirring additive manufacturing process. An arc-shaped channel (9) is provided at the lower part of the tool head (7). The arc-shaped channel (9) extends from the bottom outer wall of the tool head (7) inward to the area near the middle of the lower end face of the tool head (7). The diameter of the arc-shaped channel (9) gradually decreases from the outside to the inside. The arc-shaped channel (9) adopts an arc-shaped open groove at the bottom end of the tool head (7). A stirring needle (8) is provided at the lower end of the tool head (7). During the friction stirring additive manufacturing process, the wire feeding mechanism... After the continuously fed metal wire enters the inner end of the arc-shaped channel (9) laterally, it is continuously plasticized under the spinning action of the lower end face of the tool head (7) and the stirring action of the stirring needle (8). The wire feeding mechanism includes a cantilever (2) fixedly connected to the upper part of the main shaft (1). A wire spool (3) is provided on the cantilever (2). The axis of the wire spool (3) is perpendicular to the main shaft (1). A bracket (10) is provided inside the wire spool (3) and above the tool head (7). A roller group (4) is provided on the bracket (10). A heating module is provided inside the roller group (4). The metal wire drawn from the wire spool (3) passes through the roller group (4) and then passes through the heating module, and then enters the arc-shaped channel (9) laterally.
2. The defect repair method according to claim 1, characterized in that: When the defect depth exceeds 2mm, pre-treatment is performed after grooving at the defect.
3. The defect repair method according to claim 1, characterized in that: During the defect repair process, feeding stops whenever the tool head moves forward and leaves the original defect position. Then, the tool head is adjusted back to the starting position and feeding continues.
4. The defect repair method according to claim 3, characterized in that: A spiral groove (13) is provided on the stirring needle (8). The upper end of the spiral groove (13) extends to the root of the stirring needle (8) and is close to the inner end of the arc-shaped channel (9). The lower end of the spiral groove (13) extends to the lower end of the stirring needle (8).
5. The defect repair method according to claim 4, characterized in that: A concave area (14) is provided at the root of the stirring needle (8). The junction (15) of the concave area (14) and the arc-shaped channel (9) is on the same plane as the lower end face of the tool head (7). The concave area (14) is also directly connected to the spiral groove (13). During the defect repair process, the metal wire is rolled / segmented through the junction (15).
6. The defect repair method according to claim 4 or 5, characterized in that: The heating module uses an induction heating coil (6), and the axis of the induction heating coil (6) coincides with the center line of the entrance of the arc-shaped channel (9).
7. The defect repair method according to claim 6, characterized in that; One end of the heating module is inserted into the arc-shaped channel (9), and the other end of the heating module is inserted into the bracket (10).
8. The defect repair method according to claim 7, characterized in that: During the defect repair process, after completing the additive manufacturing according to the single-layer additive manufacturing path, the control tool head is gradually lifted away from the surface of the deposited layer, and after continuing to feed the wire for a period of time, it is retracted and directly switched to the next single-layer additive manufacturing path.
9. The defect repair method according to claim 8, characterized in that: During the period when the defect repair is about to end, the tool head is controlled to rotate and slowly rise, with the rising rate of the tool head not exceeding 0.5 mm / s, so as to allow the plasticized metal material to be backfilled into the keyhole.
Citation Information
Patent Citations
A floating solid-phase additive repair device and method
CN115502544B
Additive friction stir methods of repairing substrates
US9862054B2
Filler wire static shaft shoulder friction stir welding and additive manufacturing device and method
CN112958902A
Stirring friction material adding device capable of automatically and continuously feeding wires
CN116021144A
Friction agitation repair method
JP2003126971A