A method for selectively regulating the pore size distribution of micropores / mesopores in hierarchical porous carbon structures

By adjusting the combination of solvents and organic molecule precursors, the micropore and mesopore size distribution of porous carbon materials is accurately optimized, solving the problem of non-uniform pore size structure of porous carbon materials, improving the adsorption and separation performance of low-concentration gas, and achieving high efficiency. Gas purification effect.

CN118221099BActive Publication Date: 2024-10-18CHINA UNIV OF MINING & TECH

Patent Information

Application Number
CN202410481834.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-22
Publication Date
2024-10-18
Estimated Expiration
2044-04-22

AI Technical Summary

Technical Problem

The pore structure of existing porous carbon materials is multi-scale and continuously distributed, resulting in a low equilibrium separation coefficient and a narrow gas purification range during the adsorption and separation of low-concentration gas. Moreover, precise control of the porous carbon pore structure has not been achieved, and the preparation process is complex and unsuitable for large-scale applications. scale production.

Method used

By adjusting the combination of solvents with different polarities and organic molecule precursors with different molecular weights and configurations, and using vacuum impregnation and secondary carbonization technology, the micropore and mesopore size distribution in porous carbon materials can be accurately optimized to achieve adsorption separation. Modification of the pore structure of the material.

Benefits of technology

The separation efficiency of CH4 and impurity gases is significantly improved, the separation factor is significantly improved, the process is more green and environmentally friendly, the cost is low, and it is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118221099B_ABST
    Figure CN118221099B_ABST
Patent Text Reader

Abstract

The present application discloses a method for selectively regulating the pore size distribution of micropores / mesopores in a multi-level porous carbon structure, which belongs to the field of functional material synthesis and adsorption separation application. The carbon matrix body is placed in a sealed glass container, and a mixed solution of a solvent and organic molecules is injected after vacuum treatment; ultrasonic treatment is performed 3-4 times, the sealed glass container is placed in a water bath for heating, and then the sealed glass container containing the mixed solution is subjected to a secondary vacuum treatment, the mixed solution in the sealed glass container is transferred to a rotary evaporator, and the sample after spin drying is placed in a tubular furnace protected by inert gas for carbonization; the sample obtained after the final carbonization is evaluated for gas adsorption separation performance; the method can accurately achieve different goals of regulating only the mesoporous structure of the porous carbon material, regulating only its microporous structure, and regulating its micro / mesopores together, and the obtained samples show excellent effects and development potential in the field of low-concentration gas concentration such as CH4 / N2 separation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of functional material synthesis and adsorption separation application, and in particular to a method for selectively regulating the pore size distribution of micropores / mesopores in a multi-level porous carbon structure. Background Art

[0002] The extraction and utilization of coal mine gas has the triple benefits of "safety, resources, and environment", but the utilization rate of coal mine gas extraction is only about 45%, which causes the waste of clean energy and the aggravation of the greenhouse effect. At present, the utilization of coal mine gas is closely related to the concentration of its main component CH4, that is, the utilization technology of high / medium concentration gas in chemical raw materials, civilian fuels and internal combustion engine power generation is mature and widely used, but the lower concentration gas is still forced to be emptied due to the lack of mature utilization technology. Therefore, the efficient utilization of low-concentration coal mine gas is of great significance to the realization of goals such as increasing the supply of clean energy, reducing greenhouse gas emissions, and promoting safe production in coal mines.

[0003] Gas purification technology is also one of the ways to comprehensively utilize low-concentration gas in coal mines. It is to separate CH4 from impurity gases such as nitrogen (N2), oxygen (O2) and carbon dioxide (CO2) in low-concentration gas and then supply them to other industries for use. At present, pressure swing adsorption has become a gas purification technology with great industrial application prospects due to its significant advantages such as high automation and low energy consumption. Among them, adsorbents are the core and basis of pressure swing adsorption technology to achieve separation and purification. They are generally found and designed based on the differences in the physical properties of gas molecules. Compared with adsorbents such as zeolite molecular sieves [1-4] and metal organic frameworks (MOFs) [5-7], porous carbon materials not only have many cost advantages such as wide raw material sources, simple preparation process, and good regeneration performance, but also have excellent characteristics such as developed pore structure, ultra-high specific surface area and strong mechanical properties. Therefore, they have become one of the most commonly used adsorbents in pressure swing adsorption separation processes.

[0004] At present, most porous carbon materials are porous carbonaceous materials with high specific surface area generated by high-temperature pyrolysis of precursors such as coal [8-10], biomass [11-13] and organic molecules [14-16], and are widely used in the field of low-concentration gas adsorption and separation. The kinetic diameter of molecular gases such as CH4, N2 and O2 contained in low-concentration coal mine gas is less than 0.4nm, and they are generally adsorbed in micropores. According to Everett's ideal fracture pore model theory, when the kinetic diameter of the adsorbate is close to the pore size, it is most conducive to its adsorption

[17] . It can be seen that the adsorption capacity of the adsorbent for gas molecules mainly depends on the pore structure size and its surface chemical properties. However, due to many factors such as the wide range of carbon precursor sources and the uncontrollability of high-temperature decomposition and cracking, the porous carbon pore structure on the market is multi-scale and continuously distributed, that is, it is composed of micropores, mesopores and macropores. The uneven pore size distribution often leads to shortcomings such as low equilibrium separation coefficient and narrow gas purification range in the process of low-concentration gas adsorption and separation. Existing research results show that physical and chemical activation methods can increase the specific surface area and micropore volume of porous carbon materials by adjusting the activation temperature and time, but the precise control of the pore size structure of porous carbon has not been achieved so far. In addition, the carbon aerogel method and template method are better than physical and chemical activation methods in regulating micropores, but the preparation process is complicated and requires the use of toxic chemical reagents, which is not suitable for large-scale production. Therefore, studying new strategies for optimizing the pore size of porous carbon materials is the key for researchers to fundamentally improve the adsorption and separation of CH4 and other impurity gases (N2 and CO2, etc.).

[0005] References

[0006] [1] Li, S. S., Chen, J., Wang, Y., Li, K. B., Li, K. J., Guo, W. J., Zhang, X. R., Liu, J. Q., Tang, X., Yang, J. F., & Li, JP, 2022. Separation and Purification Technology, 286, 120497.

[0007] [2]Shang, H., Li, YP, Liu, JQ, Tang, X., Yang, JF, & Li, JP, 2019. Chinese Journal of Chemical Engineering, 27(5), 1044-1049.

[0008] [3] Sun, YB, Tang, JF, Li, GY, Hua, YH, Li, H., & Hu, SY, 2022. ACS Omega, 7(22), 18542-18551.

[0009] [4]Yang,JF,Tang,X.,Liu,JQ,Wang,J.,Shang,H.,Wu,LG,Li,JP,&Deng,SG,2020a.Chemical Engineering Journal,406.

[0010] [5]Huang,Zh,Hu,P.,Liu,J.,Shen,F.,Zhang,Yq,Chai,KG,Ying,YP,Kang,CG,Zhang,ZQ,&Ji,HB,2022.Separation and Purification Technology,286.

[0011] [6]Pereira,A.,Ferreira,AFP,Rodrigues,A.,Ribeiro,AM,&Regufe,MJ,2022.Microporous and Mesoporous Materials,331.

[0012] [7]Chang,M.,Yan,T.,Wei,Y.,Wang,JX,Liu,DH,&Chen,JF,2022.ACSApplied Materials&Interfaces,14(22),25374-25384.

[0013] [8]Hamyali,H.,Nosratinia,F.,Rashidi,A.,&Ardjmand,M.,2022.JournalofEnvironmental Chemical Engineering,10(1).

[0014] [9]Yang,ZY,Ning,HL,Liu,JP,Meng,ZY,Li,YY,Ju,XQ,&Chen,ZP,2020.Chemical Engineering Research andDesign,161,312-321.

[0015]

[10] Zhang,B.,Liu,P.,Huang,Z.,&Liu,JJ,2023.ACS Omega,8(11),10303-10313.

[0016]

[11] Surra, E., Ribeiro, R., P.P.L., Santos, T., Bernardo, M., José, P.B.M., Lapa, N., & Isabel, A.A.C.E., 2022. Journal of Environmental Chemical Engineering, 10(1).

[0017]

[12] Song, C., Ye, W., Liu, Y., Huang, H., Zhang, H., Lin, H., Lu, R., & Zhang, S., 2020. ACS Omega, 5(43), 28255 - 28263.

[0018]

[13] Prasetyo, I., Mukti, N.I.F., Cahyono, R.B., Prasetya, A., & Ariyanto, T., 2020. Waste and Biomass Valorization, 11(10), 5599 - 5606.

[0019]

[14] Qin, F.F., Guo, Z.Y., Wang, J.S., Qu, S.J., Zuo, P.P., & Shen, W.Z., 2019. Applied Surface Science, 491, 607 - 615.

[0020]

[15] Wang, S.M., Wu, P.C., Fu, J.W., & Yang, Q.Y., 2021. Separation and Purification Technology, 274, 119121.

[0021]

[16] Xu, S., Li, W.C., Wang, C.T., Tang, L., Hao, G.P., & Lu, A.H., 2020. Angew Chem Int Ed Engl, 60(12), 6339 - 6343.

[0022]

[17] Yoshikawa, M., Katagiri, G., Ishida, H., Ishitani, A., & Akamatsu, T., 1988. Appl Phys Lett, 52, 1639–1641. Summary of the Invention

[0023] Technical Problem to be Solved:

[0024] In view of the deficiencies in the prior art, the present application solves the problems that the existing porous carbon pore structure is multi-scale and continuously distributed, that is, it is composed of micropores, mesopores and macropores, and the uneven pore size distribution often leads to a low equilibrium separation coefficient and a narrow gas purification range in the low-concentration gas adsorption and separation process, as well as the current failure to achieve precise control of the porous carbon pore size structure, the preparation process is complicated, and it is not suitable for large-scale production. A method for selectively controlling the micropore / mesopore pore size distribution in a multi-level porous carbon structure is provided, which is mainly used to meet the industrial application requirements of efficient separation performance of CH4 and impurity gases (N2 and CO2, etc.), thereby improving the utilization efficiency of porous carbon materials in the pressure swing concentration of low-concentration gas in coal mines.

[0025] Technical solution:

[0026] To achieve the above objectives, this application is implemented through the following technical solutions:

[0027] A method for selectively regulating the pore size distribution of micropores / mesopores in a hierarchical porous carbon structure, comprising the following steps:

[0028] Step 1: Weigh 0.5g of the carbon matrix body according to the mass ratio and place it in a sealed glass container, evacuate it for 10 minutes to make the container in a negative pressure state, and then inject 30g of solvent and 0.01-0.05g of organic molecule mixed solution;

[0029] Step 2: subjecting the sealed glass container containing the mixed solution to ultrasonic treatment for 10 minutes each time, for a total of 3-4 times, to ensure that the mixed solution fully enters the pores of the carbon matrix body;

[0030] Step 3: Place the sealed glass container in a 45-60°C water bath and heat for 10-30 minutes, then perform a secondary vacuum treatment on the sealed glass container containing the mixed solution for 10-15 minutes until no bubbles are generated in the solution, then open the sealed glass container to allow the internal and external atmospheric pressures to reach equilibrium instantly;

[0031] Step 4: Transfer the mixed solution in the sealed glass container to a rotary evaporator for spin drying;

[0032] Step 5: The spin-dried sample is placed in a tubular furnace protected by inert gas for carbonization;

[0033] Step 6: Characterize the pore structure of the sample obtained after the final carbonization and evaluate its gas adsorption and separation performance.

[0034] Furthermore, the carbon matrix body is a porous carbon material.

[0035] Furthermore, the porous carbon material is one or more of coal-based activated carbon, coconut shell activated carbon, and carbon black.

[0036] Furthermore, the solvent is one or more of ethyl acetate, tetrahydrofuran, acetone and water.

[0037] Furthermore, when the solvent is water, the organic molecule selects one or more of glucose, sucrose, and hydroxymethyl cellulose as the carbon precursor.

[0038] Furthermore, when the solvent is one or more organic solvents selected from ethyl acetate, tetrahydrofuran, and acetone, the organic molecule is selected from one or more organic solvents selected from o-phenylenediamine, oleylamine, and octylamine.

[0039] Furthermore, in the first step, 0.01-0.05 g of organic molecules are dissolved and dispersed in 30 g of solvent to form a stable and uniform mixed solution, and the mixed solution enters the sealed glass container in the negative pressure state through a syringe under pressure driving.

[0040] Furthermore, in the first step, the mass ratio of the organic molecules to the carrier carbon is 2% to 10%.

[0041] Furthermore, the fifth step is specifically to put the spin-dried sample into a quartz crucible, then put the quartz crucible into a tubular furnace, introduce argon Ar as a protective gas, heat the tubular furnace to 180-200°C at a rate of 2°C / min, keep it warm for 3 hours, then heat it to 650°C at a rate of 5°C / min, keep it warm for 2 hours, and naturally cool it to room temperature to obtain a porous carbon material with a new pore structure.

[0042] Furthermore, the sixth step is specifically as follows: characterizing the pore structure of the sample obtained after carbonization, the characterization instrument is a Quantachrome fully automatic physical adsorption analyzer, model Autosorb-iQ-C, the gas probe molecules are N2 and CO2, and the micropore size distribution and mesopore size distribution in the porous carbon structure are characterized respectively; secondly, the gas adsorption separation performance is evaluated on a Quantachrome fully automatic physical adsorption analyzer, model Autosorb-iQ-C, and the isothermal adsorption curves of gases CH4 and N2 at a temperature of 25°C and a pressure of 0-100kPa are tested respectively, and the separation factor is calculated using the ideal adsorption solution theory IAST.

[0043] Principle explanation: The post-loading method is used to optimize the pore structure ratio of commercial porous carbon materials, that is, by adjusting the combination of solvents with different polarities and organic molecular precursors with different molecular weights and configurations, the content of micropores and mesoporous structures entering the porous carbon carrier material after carbonization of the organic precursor is controlled. In other words, after secondary carbonization, the micropore / mesopore pore size distribution can be accurately optimized, thereby improving the separation efficiency of CH4 and impurity gases (N2 and CO2, etc.).

[0044] Beneficial effects:

[0045] The present application provides a method for selectively regulating the pore size distribution of micropores / mesopores in a hierarchical porous carbon structure, which has the following beneficial effects:

[0046] 1. This patent proposes a new method of adjusting the combination of solvents of different polarity and organic molecular precursors of different molecular weights and configurations, which can accurately achieve three ways of pore modification strategies for adsorption separation materials, namely, regulating only the mesoporous structure of porous carbon materials, regulating only the microporous structure, and regulating micro / mesopores together. It also shows excellent results and development potential in the field of low-concentration gas separation such as CH4 / N2 separation;

[0047] 2. Compared with the physical activation method, this method has a more significant effect on the change of pore structure. Compared with the chemical activation method, it is more environmentally friendly and avoids the production of a large amount of strong acid and strong alkali. Compared with the template method, the process is simple and the cost is low. Therefore, the use of this method to modify the adsorption separation material has great industrial application prospects in terms of performance, environmental protection and cost.

[0048] 3. This patent proposes a new method to control the micropore / mesopore pore size distribution in porous carbon by adjusting the combination of solvents of different polarity and organic molecular precursors of different molecular weights and configurations. The process focuses on ensuring that the carbon precursor solution fully enters the pores of the porous carbon material based on the vacuum impregnation method, and then uses the interaction between the polarity of the solvent and the porous carbon surface, and the adaptability of the molecular configuration of the organic molecules to the pore size to accurately achieve the different goals of only controlling the mesoporous structure of the porous carbon material, only controlling its microporous structure, and jointly controlling its micro / mesopores, thereby providing a new strategy for the targeted regulation of the pores and properties of porous carbon materials;

[0049] 4. In the strategy of modifying the mesopore size distribution only, compared with the original porous carbon carrier, the modified porous carbon material achieves precise control of the pore size distribution and pore volume of the 10-33nm mesopore scale, while there is no obvious change in the 0.35-1.5nm micropore scale; in the strategy of modifying the micropore size distribution only, the modified porous carbon material achieves precise control of the pore size distribution and pore volume of the 0.35-1.5nm micropore scale, while there is no obvious change in the 2-33nm mesopore scale; in the strategy of jointly modifying the micro / mesopores, the modified porous carbon material has obvious changes in the pore size and pore volume of the 0.35-1.5nm and 2-33nm scales;

[0050] 5. The pore structure parameters of porous carbon materials are closely related to the separation performance. Among the three pore structure modification strategies of only mesopores, only micropores, and micro / mesopores, compared with the original porous carbon carrier, precise control of the micropore size alone can significantly improve the IAST separation factor of CH4 / N2 mixed gas, and the separation factor increases from 3.45 to 10.83. In the strategies of only mesopores and micro / mesopores modification, the increase in separation factor is smaller, indicating that the targeted improvement of CH4 / N2 separation performance can be achieved by precise control of pore size. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 This is a mesopore size distribution diagram obtained by low-temperature N2 adsorption-desorption (77K) test of the porous carbon series material in Example 1 of the present application;

[0052] Figure 2 This is a micropore size distribution diagram of the porous carbon series material in Example 1 of the present application tested by low-pressure CO2 adsorption (273K);

[0053] Figure 3 This is a mesopore size distribution diagram obtained by low-temperature N2 adsorption-desorption (77K) test of the porous carbon series material in Example 2 of the present application;

[0054] Figure 4 This is a micropore size distribution diagram obtained by low-pressure CO2 adsorption (273K) test of the porous carbon series material in Example 2 of the present application;

[0055] Figure 5 This is a mesopore size distribution diagram obtained by low-temperature N2 adsorption-desorption (77K) test of the porous carbon series material in Example 3 of the present application;

[0056] Figure 6 This is a micropore size distribution diagram of the porous carbon series material in Example 3 of the present application tested by low-pressure CO2 adsorption (273K);

[0057] Figure 7 This is the CH4 / N2 separation performance diagram of the porous carbon series materials in this application. DETAILED DESCRIPTION

[0058] The preferred embodiments of the present invention will be described in detail below with reference to the accompanying drawings in the specification.

[0059] In the following examples, commercial porous carbon materials (named C-support) commonly found on the market with high specific surface area and rich multi-scale pore structure, such as one or more of coal-based activated carbon, coconut shell activated carbon, and carbon black, are selected as the main carbon matrix to examine the changes in their micropore / mesopore pore size distribution.

[0060] According to the polarity of the solvent, four solvents with large differences, ethyl acetate, tetrahydrofuran, acetone and water, were selected to regulate the proportion of organic molecules entering the microporous and mesoporous structures after "secondary carbonization". In order to ensure the uniformity of the dissolution of organic molecules, three organic molecules with different configurations and relative molecular weights, glucose, sucrose and hydroxymethyl cellulose, were selected as carbon precursors when water was used as the solvent, while the organic molecules of organic solvents such as ethyl acetate, tetrahydrofuran and acetone were selected correspondingly, such as o-phenylenediamine, octylamine and oleylamine.

[0061] Embodiment 1:

[0062] A method for selectively regulating the pore size distribution of micropores / mesopores in a hierarchical porous carbon structure, and accurately regulating the mesoporous structure scale of the porous carbon material, the specific steps are:

[0063] a. Dissolve 0.02g or 0.05g of hydroxymethyl cellulose in 30g of distilled water to prepare a stable and uniform mixed solution A; then weigh 0.5g of commercial porous carbon material and place it in a sealed glass container, heat it in a 60°C water bath for 30 minutes, and then vacuum it for 10 to 15 minutes to make the container in a negative pressure state, and solution A enters the sealed glass container through a syringe under pressure;

[0064] b. The sealed glass container containing the mixed solution A is subjected to ultrasonic treatment for 3 to 4 times, each time for 10 minutes, to ensure that the solution A fully enters the pores of the porous material; then it is placed in a 60°C water bath and heated for 30 minutes, and the solution A in the sealed glass container is vacuumed again for 10 to 15 minutes until no bubbles are generated in the solution;

[0065] c. Open the sealed glass container, and the internal and external atmospheric pressures reach equilibrium instantaneously. Transfer solution A to a rotary evaporator to remove the aqueous solvent to obtain a uniform mixture; transfer the resulting mixture to a quartz crucible, put it into a tubular furnace, introduce argon Ar as a protective gas, and heat the tubular furnace to 180°C at a rate of 2°C / min, keep it warm for 3h, then heat it to 650°C at a rate of 5°C / min, keep it warm for 2h, and naturally cool it to room temperature to obtain porous carbon materials with a new pore structure, which were named C1-S (0.02g hydroxymethyl cellulose) and C1-L (0.05g hydroxymethyl cellulose), respectively.

[0066] Embodiment 2:

[0067] A method for selectively regulating the pore size distribution of micropores / mesopores in a hierarchical porous carbon structure, and accurately regulating the microporous structure scale of the porous carbon material, the specific steps are:

[0068] a. 0.01 g or 0.03 g of o-phenylenediamine organic molecules were dissolved and dispersed in 30 g of ethyl acetate organic solvent to prepare a stable and uniform mixed solution B; then 0.5 g of commercial porous carbon material was weighed and placed in a sealed glass container, and the container was placed in a negative pressure state after vacuum treatment for 10 minutes, and solution B entered the sealed glass container through a syringe under pressure drive;

[0069] b. The sealed glass container containing the mixed solution B is subjected to ultrasonic treatment for 3 to 4 times, each time for 10 minutes, to ensure that the solution B fully enters the pores of the porous material; then it is placed in a 45°C water bath and heated for 10 minutes, and then the solution B in the sealed glass container is vacuumed again for 10 to 15 minutes until no bubbles are generated in the solution;

[0070] c. Open the sealed glass container, and the internal and external atmospheric pressures reach equilibrium instantaneously. Transfer solution B to a rotary evaporator to remove the ethyl acetate organic solvent to obtain a uniform mixture; transfer the resulting mixture to a quartz crucible, place it in a tubular furnace, introduce argon Ar as a protective gas, and heat the tubular furnace to 200°C at a rate of 2°C / min, keep it warm for 3h, then heat it to 650°C at a rate of 5°C / min, keep it warm for 2h, and naturally cool it to room temperature to obtain porous carbon materials with a new pore structure, which were named C3-S (0.01g o-phenylenediamine) and C4-L (0.03g o-phenylenediamine), respectively.

[0071] Embodiment 3:

[0072] A method for selectively regulating the pore size distribution of micropores / mesopores in a hierarchical porous carbon structure, and synergistically regulating the micropore / mesopore structure scale of the porous carbon material, the specific steps are:

[0073] a. 0.02g or 0.05g of oleylamine organic molecules are dissolved and dispersed in 30g of tetrahydrofuran organic solvent to prepare a stable and uniform mixed solution C; then 0.5g of commercial porous carbon material is weighed and placed in a sealed glass container, and the container is placed in a negative pressure state after vacuum treatment for 10 minutes, and solution C is driven by pressure into the sealed glass container through a syringe;

[0074] b. The sealed glass container containing the C mixed solution is subjected to ultrasonic treatment for 3 to 4 times, each ultrasonic treatment for 10 minutes, to ensure that the B solution fully enters the pores of the porous material; then it is placed in a 40°C water bath and heated for 10 minutes, and then the B solution in the sealed glass container is vacuumed again for 10 to 15 minutes until no bubbles are generated in the solution;

[0075] c. Open the sealed glass container, and the internal and external atmospheric pressures reach equilibrium instantaneously. Transfer solution C to a rotary evaporator to remove the tetrahydrofuran organic solvent to obtain a uniform mixture; transfer the resulting mixture to a quartz crucible, place it in a tubular furnace, introduce argon Ar as a protective gas, and heat the tubular furnace to 200°C at a rate of 2°C / min, keep it warm for 3h, then heat it to 650°C at a rate of 5°C / min, keep it warm for 2h, and naturally cool it to room temperature to obtain porous carbon materials with a new pore structure, which were named C5-S (0.02g oleylamine) and C6-L (0.05g oleylamine), respectively.

[0076] like Figure 1-6 As shown in the figure, in the strategy of modifying the mesopore size distribution only, compared with the original porous carbon support, the modified porous carbon material achieves precise control of the pore size distribution and pore volume of the mesopore scale of 10-33nm ( Figure 2 ), but there is no obvious change in the 0.35-1.5nm micropore size ( Figure 1 ); In the strategy of modifying the micropore size distribution only, the modified porous carbon material achieved precise control of the pore size distribution and pore volume of the micropore scale of 0.35-1.5nm ( Figure 4 ), but there is no obvious change in the 2-33nm mesopore size ( Figure 3 ); In the common micro / mesopore modification strategy, the pore size and pore volume of the modified porous carbon materials at the scales of 0.35-1.5nm and 2-33nm have obvious changes ( Figure 5 and Figure 6 );

[0077] like Figure 7 As shown in the figure, the pore structure parameters of porous carbon materials are closely related to the separation performance. Among the three pore structure modification strategies of only mesopores, only micropores and micro / mesopores together, that is, compared with the original porous carbon carrier, only precise control of micropore size can achieve a significant improvement in the IAST separation factor of CH4 / N2 mixed gas, and the separation factor increased from 3.45 to 10.83. In the strategies of only mesopores and micro / mesopores modification, the increase in separation factor was smaller, indicating that the targeted improvement of CH4 / N2 separation performance can be achieved by precisely controlling the pore size.

[0078] The embodiments proposed in the present invention are embodiments under preferred conditions, but are not limited to the above-mentioned contents. Relevant technicians in this field can easily repeat the above-mentioned embodiments, and further extend and change the scheme, but as long as they do not deviate from the spirit of the present invention, they are all within the protection scope of the present invention.

Claims

1. A method for selectively regulating the pore size distribution of micropores / mesopores in a hierarchical porous carbon structure, characterized in that: The specific steps are: The first step: weigh 0.5g of the carbon matrix body according to the mass ratio and place it in a sealed glass container, vacuum it for 10-15min to make the container in a negative pressure state, and then inject 30g of a solvent and a mixed solution of 0.01-0.05g of an organic molecule, wherein the carbon matrix body is a porous carbon material, and the porous carbon material is one or more of coal-based activated carbon, coconut shell activated carbon, and carbon black, and the solvent is one or more of ethyl acetate, tetrahydrofuran, acetone, and water. When the solvent is water, the organic molecule selects one or more of glucose, sucrose, and hydroxymethyl cellulose as a carbon precursor; when the solvent is one or more of ethyl acetate, tetrahydrofuran, and acetone, the organic molecule selects one or more of o-phenylenediamine, oleylamine, and octylamine; Step 2: subjecting the sealed glass container containing the mixed solution to ultrasonic treatment for 10 minutes each time, for a total of 3-4 times, to ensure that the mixed solution fully enters the pores of the carbon matrix body; Step 3: Place the sealed glass container in a 45-60°C water bath and heat for 10-30 minutes, then perform a secondary vacuum treatment on the sealed glass container containing the mixed solution for 10-15 minutes until no bubbles are generated in the solution, then open the sealed glass container to allow the internal and external atmospheric pressures to reach equilibrium instantly; Step 4: Transfer the mixed solution in the sealed glass container to a rotary evaporator for spin drying; Step 5: The spin-dried sample is placed in a tubular furnace protected by inert gas for carbonization; Step 6: Characterize the pore structure of the sample obtained after the final carbonization and evaluate its gas adsorption and separation performance.

2. The method for selectively controlling the pore size distribution of micropores / mesopores in a hierarchical porous carbon structure according to claim 1, characterized in that: In the first step, 0.01-0.05 g of organic molecules are dissolved and dispersed in 30 g of solvent to form a stable and uniform mixed solution, and the mixed solution is driven by pressure into the sealed glass container in a negative pressure state through a syringe.

3. The method for selectively regulating the pore size distribution of micropores / mesopores in a hierarchical porous carbon structure according to claim 1, characterized in that: In the first step, the mass ratio of the organic molecules to the carbon matrix main body is 2% to 10%.

4. The method for selectively regulating the pore size distribution of micropores / mesopores in a hierarchical porous carbon structure according to claim 1, characterized in that: The fifth step is specifically to put the spin-dried sample into a quartz crucible, then put the quartz crucible into a tubular furnace, introduce argon Ar as a protective gas, heat the tubular furnace to 180-200°C at a rate of 2°C / min, keep it warm for 3h, then heat it to 650°C at a rate of 5°C / min, keep it warm for 2h, and naturally cool it to room temperature to obtain a porous carbon material with a new pore structure.

5. The method for selectively controlling the pore size distribution of micropores / mesopores in a hierarchical porous carbon structure according to claim 1, characterized in that: The sixth step is specifically as follows: characterizing the pore structure of the sample obtained after carbonization, using a Quantachrome fully automatic physical adsorption analyzer, model Autosorb-iQ-C, and using gas probe molecules N2 and CO2, respectively characterizing the micropore size distribution and mesopore size distribution in the porous carbon structure; secondly, evaluating the gas adsorption separation performance on a Quantachrome fully automatic physical adsorption analyzer, model Autosorb-iQ-C, testing the isothermal adsorption curves of gases CH4 and N2 at a temperature of 25°C and a pressure of 0-100kPa, and calculating the separation factor using the ideal adsorption solution theory IAST.

Citation Information

Patent Citations

  • Preparation method of briquetted active carbon

    CN104528717A

  • Method for preparing silica / carbon nanometer material with micropores and ordered mesopores

    CN107117623A

Cited By

  • High-performance asphalt-based porous carbon as well as preparation method and application thereof

    CN121020582A

  • High performance pitch-based porous carbon, and preparation method and application thereof

    CN121020582B