Method for extracting silicon and multi-metal products from activated red mud

Through the coordinated treatment and thermal activation technology of red mud, gasified slag and sodium carbonate, the problems of high energy consumption and low resource utilization in traditional red mud extraction mineral technology are solved, and efficient extraction of silicon and polymetal products is achieved, reducing the reduction of Waste emissions have been expanded and product areas have been expanded.

CN118221125BActive Publication Date: 2024-11-01江苏纽赛斯工程技术有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410660406.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-27
Publication Date
2024-11-01
Estimated Expiration
2044-05-27

AI Technical Summary

Technical Problem

Traditional red mud extraction mineral technology has problems such as high energy consumption, low resource utilization, large amounts of waste, and high requirements for the corrosion resistance of equipment.

Method used

By mixing the red mud, gasified slag and sodium carbonate in a certain proportion, heat activation is carried out, then adding hot water to dissolve and filtering, adjusting the pH value to obtain a mixed solution of sodium silicate and polymetal ion. By wet magnetic separation and Control pH value to separate multiple metal products in step by step.

Benefits of technology

It has achieved efficient resource utilization of red mud, reduced waste emissions, improved resource recycling rate, expanded product performance and use, and increased added value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118221125B_ABST
    Figure CN118221125B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of extracting minerals from activated red mud, and provides a method for extracting silicon and multi-metal products from activated red mud, comprising: uniformly mixing red mud, gasified slag and sodium carbonate in proportion; crushing and grinding the mixed material and then performing thermal activation; crushing and grinding the activated material, adding hot water to dissolve and filtering; filtering to obtain a sodium silicate solution and a filter residue, adjusting the pH value of the sodium silicate solution to obtain a silicon product; wet magnetic separation of the filter residue, filtering after wet magnetic separation, mixing the non-magnetic slag obtained by filtration with a concentrated acid solution to obtain a silicon dioxide aerogel and a mixed solution of multi-metal ions; and separating the mixed solution of multi-metal ions in steps by controlling the pH value to obtain multiple metal products. According to the scheme of the present invention, the present invention has low energy consumption, high resource utilization, does not generate a large amount of waste, and has low requirements on the corrosion resistance of the equipment in the process of extracting minerals from red mud.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of activating red mud to extract minerals, and in particular to a method for activating red mud to extract silicon and multi-metal products. Background Art

[0002] Red mud is a kind of strong alkaline industrial solid waste produced in the process of producing alumina from bauxite. It has a complex composition and is mainly composed of hematite, hydrogrossular, cancryogenite, calcite, fayalite, diaspore, goethite, gibbsite and perovskite. It usually contains a high iron content. Damming and stockpiling is currently the main treatment method for red mud, and the actual comprehensive utilization rate does not exceed 5%. Red mud contains a variety of valuable elements, including aluminum and a variety of rare earth elements in addition to iron and titanium. If the various minerals of red mud are recycled and utilized comprehensively, turning waste into treasure, such as extracting valuable metals from red mud and developing high value-added materials, it will realize the resource utilization of industrial waste and relieve the pressure on resources and the environment. There is a strong demand for reducing the amount and harm of solid waste at the source and green recycling. It is imperative to use multidisciplinary cross-cutting and multi-field collaborative technologies to realize the green, collaborative, efficient, high-value and large-scale comprehensive utilization of red mud resources.

[0003] The traditional method of extracting minerals from red mud has the disadvantages of high energy consumption, low resource utilization, large amount of waste generated, and high requirements for the corrosion resistance of equipment. Summary of the invention

[0004] The purpose of the present invention is to solve at least one technical problem in the background technology and provide a method for extracting silicon and multi-metal products from activated red mud.

[0005] To achieve the above object, the present invention provides a method for extracting silicon and multi-metal products from activated red mud, comprising:

[0006] Mix red mud, gasification slag and sodium carbonate evenly according to proportion;

[0007] The mixed materials are crushed and ground and then thermally activated;

[0008] The activated material is crushed and ground into powder, dissolved in hot water and then filtered;

[0009] Filtering to obtain a sodium silicate solution and filter residue, and adjusting the pH value of the sodium silicate solution to obtain a silicon product;

[0010] The filter residue is subjected to wet magnetic separation, and then filtered, and the non-magnetic residue obtained by filtration is mixed with a concentrated acid solution to obtain a mixed solution of silica aerogel and multi-metal ions;

[0011] The mixed solution of multiple metal ions is separated step by step by controlling the pH value to obtain multiple metal products.

[0012] According to one aspect of the present invention, the red mud, the gasification slag and the sodium carbonate are mixed in a ratio of 1:0.5:0.3.

[0013] According to one aspect of the present invention, the thermal activation temperature is 800-820° C. and the thermal activation time is 40 minutes.

[0014] According to one aspect of the present invention, the step of crushing and grinding the mixed material and then thermally activating the material comprises the following reaction process: .

[0015] According to one aspect of the present invention, the activated material is crushed and ground, and then filtered after adding hot water to dissolve:

[0016] The activated material is crushed and ground to a particle size of 5 μm to 74 μm, then added with hot water to dissolve for 10 minutes and filtered.

[0017] According to one aspect of the present invention, the pH of the sodium silicate solution is adjusted to below 6 to obtain a silicon series product.

[0018] According to one aspect of the present invention, the multi-metal ion mixed solution is a multi-metal ion mixed solution rich in iron, aluminum, calcium, manganese, magnesium and titanium.

[0019] According to one aspect of the present invention, the concentrated acid solution is hydrochloric acid or nitric acid.

[0020] According to one aspect of the present invention, a mixed solution of multiple metal ions is separated step by step by controlling the pH value to obtain iron, aluminum, calcium, manganese, magnesium and titanium products respectively.

[0021] To achieve the above objectives, the present invention provides a silicon product prepared by the above method for extracting silicon and multi-metal products from activated red mud.

[0022] To achieve the above objectives, the present invention provides a plurality of metal products prepared by the method for extracting silicon and multi-metal products from activated red mud.

[0023] According to the scheme of the present invention, the present invention realizes maximum utilization and recycling of resources by synergistically treating gasified slag and red mud and utilizing the synergistic effect between the two. The gasified slag and red mud produce a synergistic effect in the synergistic treatment process, which improves the activity of the red mud. After synergistic thermal activation, the mineral morphology is obviously separated, the monomer minerals increase, the inclusion and intergrowth phenomenon is not obvious, and the Fe content increases in elemental composition, wherein the iron-containing phase is transformed into iron element and iron oxide, and the aluminum silicate phase is transformed into nepheline, sodium aluminum silicate, etc. The gasified slag and red mud come from different industrial processes respectively. Through synergistic treatment, the comprehensive utilization of the resources of the two can be achieved, waste emissions can be reduced, and environmental pollution can be reduced. The products after synergistic treatment have new properties and uses, which can expand new product areas and increase added value. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 A flow chart schematically showing a method for extracting silicon and multi-metal products from activated red mud according to one embodiment of the present invention;

[0025] Figure 2 This is the SEM morphology of the red mud concentrate before activation in Example 1;

[0026] Figure 3 This is the EDS spectrum of the red mud concentrate before activation in Example 1;

[0027] Figure 4 This is a diagram of element content of red mud concentrate before activation in Example 1;

[0028] Figure 5 This is the SEM morphology of the red mud after activation in Example 1;

[0029] Figure 6 This is the EDS spectrum of red mud after activation in Example 1;

[0030] Figure 7 This is a diagram of element content of red mud after activation in Example 1;

[0031] Figure 8 is the XRD pattern of red mud before activation in Example 1;

[0032] Fig. 9 This is the XRD diagram of the red mud after activation in Example 1. DETAILED DESCRIPTION

[0033] The present invention will now be discussed with reference to exemplary embodiments. It should be understood that the embodiments discussed are only to enable those skilled in the art to better understand and thus implement the present invention, rather than implying any limitation on the scope of the present invention.

[0034] As used herein, the term “including” and variations thereof are to be interpreted as open-ended terms meaning “including, but not limited to.” The term “based on” is to be interpreted as “based, at least in part, on.” The terms “one embodiment” and “an embodiment” are to be interpreted as “at least one embodiment.”

[0035] Figure 1 A flow chart schematically shows a method for extracting silicon and multi-metal products from activated red mud according to an embodiment of the present invention. Figure 1 As shown, in this embodiment, the method for extracting silicon and multi-metal products from activated red mud includes:

[0036] Mix red mud, gasification slag and sodium carbonate evenly according to proportion;

[0037] The mixed materials are crushed and ground and then thermally activated;

[0038] The activated material is crushed and ground into powder, dissolved in hot water and then filtered;

[0039] Filtering to obtain a sodium silicate solution and filter residue, and adjusting the pH value of the sodium silicate solution to obtain a silicon product;

[0040] The filter residue is subjected to wet magnetic separation, and then filtered, and the non-magnetic residue obtained by filtration is mixed with a concentrated acid solution to obtain a mixed solution of silica aerogel and multi-metal ions;

[0041] The mixed solution of multiple metal ions is separated step by step by controlling the pH value to obtain multiple metal products.

[0042] In this embodiment, hot water dissolution and wet magnetic separation, sodium carbonate plays an important role.

[0043] First, the ore in the red mud is crushed and ground, mixed with hot water, and sodium carbonate is added to the mixture. The role of sodium carbonate is mainly to produce compounds such as sodium silicate and sodium aluminate to extract elements such as silicon and aluminum in the red mud.

[0044] Next, the mixture is subjected to wet magnetic separation, where the magnetic field is used to adsorb the magnetic iron minerals onto the magnetic filter screen to separate the ore. The non-magnetic ore is then excluded, thus achieving ore extraction.

[0045] In contrast, dry magnetic separation is a magnetic separation process that is carried out without water. In dry magnetic separation, the ore is crushed and then separated directly by the action of a magnetic field, without the need to add sodium carbonate or other chemicals. Dry magnetic separation is suitable for ores with larger particle sizes, but due to the absence of water, it may cause dust pollution and poor magnetic separation results.

[0046] According to one embodiment of the present invention, red mud, gasification slag and sodium carbonate are mixed in a ratio of 1:0.5:0.3.

[0047] According to one embodiment of the present invention, the temperature of thermal activation is 800-820° C., and the thermal activation time is 40 minutes.

[0048] According to one embodiment of the present invention, the mixed material is crushed and ground and then thermally activated, which includes the following reaction process: .

[0049] According to one embodiment of the present invention, the activated material is crushed and ground, and then dissolved in hot water and filtered to obtain:

[0050] The activated material is crushed and ground to a particle size of 5 μm to 74 μm, then added with hot water to dissolve for 10 minutes and filtered.

[0051] According to one embodiment of the present invention, the pH of the sodium silicate solution is adjusted to below 6 to obtain a silicon series product, including: 1. Silicon hydroxide (silica gel): the pH value range is usually between 2 and 4. 2. Silicon dioxide (silicon dioxide particles, silicon dioxide powder): the pH value range is usually between 6 and 7.

[0052] The above products can be collectively referred to as silica gel, and it is not that a product is produced by adjusting the pH to a certain value. Therefore, they are referred to as silica series products in this embodiment.

[0053] According to one embodiment of the present invention, the multi-metal ion mixed solution is a multi-metal ion mixed solution rich in iron, aluminum, calcium, manganese, magnesium and titanium.

[0054] According to one embodiment of the present invention, the concentrated acid solution is hydrochloric acid or nitric acid.

[0055] According to one embodiment of the present invention, a mixed solution of multiple metal ions is separated step by step by controlling the pH value to obtain iron, aluminum, calcium, manganese, magnesium and titanium products respectively.

[0056] Furthermore, to achieve the above objectives, the present invention also provides a silicon product prepared by the above method for extracting silicon and multi-metal products from activated red mud.

[0057] Furthermore, to achieve the above objectives, the present invention also provides a plurality of metal products prepared by the above method for extracting silicon and multi-metal products from activated red mud.

[0058] According to the above scheme of the present invention, the present invention realizes the maximum utilization and recycling of resources by synergistically treating gasified slag and red mud and utilizing the synergistic effect between the two. The gasified slag and red mud produce a synergistic effect in the synergistic treatment process, which improves the activity of the red mud. After synergistic thermal activation, the mineral morphology is obviously separated, the monomer minerals increase, the encapsulation phenomenon is not obvious, and the Fe content increases in the elemental composition, wherein the iron-containing phase is transformed into iron element and iron oxide, and the aluminum silicate phase is transformed into nepheline, sodium aluminum silicate, etc. The gasified slag and red mud come from different industrial processes respectively. Through synergistic treatment, the comprehensive utilization of the resources of the two can be achieved, waste emissions can be reduced, and environmental pollution can be reduced. The products after synergistic treatment have new properties and uses, which can expand new product areas and increase added value.

[0059] Example 1

[0060] This embodiment provides a method for extracting silicon and multi-metal products from activated red mud, comprising the following steps:

[0061] S1: red mud, gasification slag and sodium carbonate are mixed evenly in a certain proportion, and the ratio of red mud to gasification slag and sodium carbonate is 1:0.5:0.3;

[0062] S2: crushing and grinding the mixed materials and then performing thermal activation at a temperature of 820°C for 40 minutes;

[0063] S3: crush and grind the activated material, add hot water to dissolve for 10 minutes and filter. The best grinding particle size of the material is 5μm to 74μm;

[0064] S4: filtering to obtain a filtrate as a sodium silicate solution, adjusting the pH value to obtain a silicon series product, and adjusting the pH value to below 6 to obtain a silicon series product.

[0065] S5: filtration after wet magnetic separation, adding concentrated acid solution to the non-magnetic slag to fully mix them, and finally obtaining silica aerogel products and iron, aluminum, calcium, manganese, magnesium, titanium rich multi-metal ion solution, the non-magnetic material and the acid are fully mixed, and the concentrated acid is hydrochloric acid;

[0066] S6: The mixed solution of multiple metal ions can be separated step by step by controlling the pH value to obtain products such as iron, aluminum, calcium, manganese, magnesium, and titanium, which is conducive to subsequent extraction and separation.

[0067] Figure 2 and Figure 3 The SEM morphology and EDS spectrum of the red mud concentrate before activation in Example 1 are shown in FIG. Figure 5 and Figure 6 The SEM morphology and EDS spectrum of the activated red mud in Example 1 are shown in FIG. Figure 8 is the XRD pattern of red mud before activation in Example 1; Fig. 9 This is the XRD diagram of the red mud after activation in Example 1.

[0068] Depend on Figure 2 and Figure 3 It can be seen that the red mud samples after direct crushing and grinding show interlaced distribution of minerals in various forms, mainly in the form of inclusions, rich intergrowths, and fine mineral embedded mixed phases. It is difficult to dissociate the elements, and almost no pure mineral monomers appear, making it difficult to directly separate the elements. It can be clearly seen that the minerals are mainly Fe, Al, Si, Ca, Na, Ti, Mg, and some trace elements V, W, Yb, and Ta. The multi-element mixed ore further proves that the red mud before activation is mainly composed of fine mineral embedded mixed phases, which are difficult to dissociate, have few mineral monomers, and are difficult to sort.

[0069] Depend on Figure 5 and Figure 6 It can be seen that the mineral monomers of the red mud samples after gasification slag activation increased significantly. Figure 2 and Figure 3The mineral inclusions before activation are significantly reduced, the mineral dissociation degree is greatly improved, and the embedding degree is reduced. Combined with the EDS spectrum, it can be clearly seen that each mineral is fully dissociated after activation, and the multi-element mixed ore composed of Fe, Al, Si, Ca, Na, Ti, and Mg is significantly reduced. Figure 8 and Fig. 9 The XRD analysis results further prove that the synergistic activation of gasification slag reduces the chemical stability of minerals, promotes mineral dissociation, crystal transformation to amorphous state, and improves mineral activity. The iron-containing phase is transformed into elemental iron, and the iron oxide and aluminum silicate phase are transformed into nepheline, sodium aluminum silicate, etc.; this also indirectly shows that the synergistic activation of gasification slag is suitable for red mud activation to extract iron and aluminum and the subsequent extraction and separation of various elements.

[0070] like Figure 2-Figure 7 As shown, the microscopic morphology of the red mud ore is mainly composed of a porous matrix and individual irregular particles, which are mixed, attached and wrapped with each other. The main elements are Fe, Al, Si, Ca, Na, Ti, Mg from high to low, and there are some trace elements V, W, Yb and Ta.

[0071] After roasting and activation, the mineral morphology is obviously separated, the number of monomer minerals increases, and the inclusion and intergrowth phenomenon is not obvious. In terms of elemental composition, the Fe content increases to 30%, which is the element with the highest content, followed by Al, Na, and Si, with contents of about 5%. There are also small amounts of Ca and Ti, and some trace elements Ga, W, Yb, and Ta. Most of the elements exist mainly in the form of metal oxides, among which the iron-containing phase is transformed into single iron, and the iron oxide and aluminum silicate phases are transformed into nepheline, sodium aluminum silicate, etc.

[0072] like Figure 8 and Fig. 9 As shown in the figure, from the XRD analysis, it is known that the best match of red mud ore is Fe2O3.

[0073] The crystal structure peaks of metal oxides such as γ-AlOOH, γ-FeO(OH), and SiO2 are basically consistent with the results of the energy spectrum analysis. The activated samples are mainly composed of magnetite or hematite, indicating that the main phase of red mud undergoes oxidation and decomposition after activation, mainly forming an iron oxide phase, with very obvious crystal characteristic peaks, high matching degree, high iron oxide content, and complete dissociation.

[0074] Comparative Example 1

[0075] Compared with Example 1, in this comparative example, no gasified slag is added in step S1, and the other processes are the same as in Example 1.

[0076] The substances extracted in this comparative example have many associated impurities and low utilization value. The reason is that the mineral crystals in the red mud are highly stable, and the lack of oxidizing agents to participate in the reaction easily leads to the inability of most minerals to be leached.

[0077] Comparative Example 2

[0078] Compared with Example 1, in this comparative example, gasified slag with twice the red mud content is added in step S1, and the other processes are the same as in Example 1.

[0079] In this comparative example, the activation effect is reduced. Excessive gasification slag changes the chemical reaction conditions during the activation process, thereby reducing the activation effect. At the same time, excessive gasification slag also increases the viscosity of the raw materials or the difficulty of handling, and puts higher requirements on production equipment and processes. Various impurities or organic matter contained in the gasification slag fail to fully react, reducing product quality. In actual applications, the proportion of gasification slag should not be too high.

[0080] Comparative Example 3

[0081] Compared with Example 1, the comparative example is activated at 850° C. in step S2. The other processes are the same as those in Example 1.

[0082] Raising the temperature to 850°C did not significantly improve the activation effect. Therefore, in order to save energy, the temperature is kept below 820°C in actual applications.

[0083] Comparative Example 4

[0084] Compared with Example 1, the comparative example is activated at 500° C. in step S2. The other processes are the same as in Example 1.

[0085] This comparative example is intended to illustrate that temperature has a great influence on activation. The activation effect is not obvious only at low temperature, and the extracted substances are accompanied by more impurities and have low utilization value. The reason is that the mineral crystals in red mud are highly stable, and it is not easy to open the connection between silicon and aluminum at low activation temperature, resulting in most minerals not being dissociated. In actual applications, the temperature should not be lower than 750℃.

[0086] Comparative Example 5

[0087] Compared with Example 1, in step S3, the red mud is crushed and ground to obtain mineral powder with a particle size of 200 mm. The other processes are the same as in Example 1.

[0088] The finished product obtained under this process condition is also of average quality. Due to the large particle size of the minerals, some minerals cannot be dissociated, affecting the final grade and yield. In the actual application process, the red mud should be crushed and ground to less than 74μm as much as possible to facilitate a more thorough reaction.

[0089] Comparative Example 6

[0090] Compared with Example 1, in step S3, the red mud is crushed and ground to obtain mineral powder with a particle size of about 1 μm. The other processes are the same as in Example 1.

[0091] Under this process condition, the quality of the finished product is average. The smaller the particle size of the mineral powder, the higher its surface energy, which is easy to agglomerate and difficult to disperse evenly in the solution. This results in some particles being unable to effectively participate in the reaction during the activation process, reducing the activation efficiency. Although a smaller particle size helps to increase the surface area of ​​the reaction, if the reaction rate is too fast, the reaction will be difficult to control, resulting in uneven activation effects and affecting the quality of the final product. In actual application, red mud should not be crushed and ground to less than 2μm.

[0092] Comparative Example 7

[0093] Compared with Example 1, in step S5, the concentrated sulfuric acid solution is added to the non-magnetic slag to make it fully mixed. The other processes are the same as those in Example 1.

[0094] Concentrated sulfuric acid solution has a selective dissolving effect on the components in red mud, but has no effect on other components, resulting in uneven activation effect. Concentrated sulfuric acid solution has poor solubility for silicates and will not have a significant dissolving effect on the silicate components in red mud. In actual application, concentrated sulfuric acid should be avoided.

[0095] According to the above scheme of the present invention, the present invention provides a method for extracting silicon and multi-metal products by synergistically activating red mud with gasification slag, firstly, red mud, gasification fine slag and sodium carbonate are mixed and then heat-roasted and activated; then crushed and ground; then dissolved in hot water for 10 minutes; finally put into a vacuum filter. Through low-temperature thermal activation, certain minerals in the gasification slag and different elements in the red mud minerals are recombined under the action of the activator sodium carbonate, which can promote chemical reactions in the raw materials and increase the release of active substances, thereby enhancing the reaction efficiency of subsequent steps, reducing the chemical stability of the minerals, and causing a crystal transformation to an amorphous state to increase activity. The main activation mechanisms are:

[0096] 1. Element rearrangement and reorganization: Minerals in gasified slag and red mud may rearrange and reorganize under the action of heat, causing the originally stable structure to change, forming new chemical bonds and lattice structures, thereby increasing their activity.

[0097] 2. Dissolution and migration: Low temperature thermal activation may cause the dissolution of some minerals and the migration of elements. These dissolved substances can react with other minerals to form new active substances and promote the reactions in subsequent steps.

[0098] 3. Crystal transformation: Through low-temperature thermal activation, some minerals may undergo crystal transformation from crystalline to amorphous or amorphous. This transformation will make the structure of the mineral more unstable and increase its activity and reactivity.

[0099] 4. Surface activity enhancement: Activators increase the active sites on the mineral surface and promote the reaction.

[0100] In summary, synergistic activation can promote the phase transformation of minerals in red mud, change the mineral microstructure, achieve element reorganization, and make metal elements easier to extract in subsequent processing steps. At the same time, the synergistic thermal activation method also improves the magnetic properties of iron-containing minerals in red mud, combining the two processes of roasting activation modification and magnetic separation purification, focusing on the goals of green, low carbon, and low energy consumption, to maximize product added value and continuously optimize solid waste resource utilization technology.

[0101] Finally, it should be noted that the above embodiments are only preferred embodiments, which are only used to illustrate the technical solutions of the present invention rather than to limit them. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A method for extracting silicon and multi-metal products from activated red mud, characterized in that: include: Mix red mud, gasification slag and sodium carbonate evenly according to proportion; The mixed materials are crushed and ground and then thermally activated; The activated material is crushed and ground into powder, dissolved in hot water and then filtered; Filtering to obtain a sodium silicate solution and filter residue, and adjusting the pH value of the sodium silicate solution to obtain a silicon product; The filter residue is subjected to wet magnetic separation, and then filtered, and the non-magnetic residue obtained by filtration is mixed with a concentrated acid solution to obtain a mixed solution of silica aerogel and multi-metal ions; The mixed solution of multiple metal ions is separated step by step by controlling the pH value to obtain multiple metal products; The red mud, the gasified slag and the sodium carbonate are mixed in a ratio of 1:0.5:0.3; The thermal activation temperature is 800-820°C and the thermal activation time is 40 minutes; The activated material is crushed and ground, and then dissolved in hot water and filtered to obtain: The activated material is crushed and ground to a particle size of 5 μm to 74 μm, then dissolved in hot water for 10 minutes and filtered; Adjusting the pH of the sodium silicate solution to below 6 to obtain a silicon series product; The concentrated acid solution is hydrochloric acid or nitric acid.

2. The method for extracting silicon and multi-metal products from activated red mud according to claim 1, characterized in that: The mixed material is crushed and ground and then thermally activated, including the following reaction processes: .

3. The method for extracting silicon and multi-metal products from activated red mud according to claim 1, characterized in that: The multi-metal ion mixed solution is a multi-metal ion mixed solution rich in iron, aluminum, calcium, manganese, magnesium and titanium.

4. The method for extracting silicon and multi-metal products from activated red mud according to any one of claims 1 to 3, characterized in that: The mixed solution of multiple metal ions is separated step by step by controlling the pH value to obtain iron, aluminum, calcium, manganese, magnesium and titanium products respectively.

5. A silicon product prepared by the method for extracting silicon and multi-metal products from activated red mud as claimed in claim 1.

6. A plurality of metal products prepared by the method for extracting silicon and multi-metal products from activated red mud according to any one of claims 1 to 4.