A carbonization-cured high-toughness fiber cement board, its preparation method and application

By employing carbonization curing technology and a layer-by-layer fiber spreading method, combined with high tensile modulus fibers and additives, the embrittlement problem of fiber cement boards in alkaline environments has been solved, improving strength and durability, reducing water absorption and porosity, and achieving efficient fiber utilization and environmentally friendly production.

CN118221403BActive Publication Date: 2026-11-10WUHAN UNIV OF TECH +3
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410279725.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-12
Publication Date
2026-11-10
Estimated Expiration
2044-03-12

AI Technical Summary

Technical Problem

Existing fiber cement boards become brittle in alkaline environments, resulting in low strength and poor toughness. Furthermore, traditional curing methods can easily lead to deformation, affecting physical properties and durability.

Method used

The fiber cement board employs a carbonization curing process, combined with a production method that involves layer-by-layer fiber forming and spreading. It utilizes high-tensile-modulus organic synthetic fibers and additives, and generates calcium carbonate through the reaction of CO2 with cementing materials, thereby improving the strength and density of the fiber cement board.

Benefits of technology

It improves the flexural and tensile strength of fiber cement boards, reduces water absorption and porosity, improves fiber dispersion and utilization, and reduces resource input and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004737109840000071
    Figure BDA0004737109840000071
  • Figure BDA0004737109840000081
    Figure BDA0004737109840000081
Patent Text Reader

Abstract

This invention discloses a carbonized-cured high-toughness fiber cement board, its preparation method, and its application. The preparation method of the high-toughness fiber cement board includes the following steps: mixing a first fiber, cementitious material, additives, and water to obtain a slurry; forming a slurry layer by sheeting the slurry; laying a second fiber layer on the slurry layer to form a fiber layer; repeating the sheeting and laying process to prepare the slurry layer and fiber layer sequentially until a specified thickness is reached, resulting in a board blank; subjecting the board blank to sequential pressure, pre-curing, and static curing, followed by curing in a CO2 atmosphere. This invention, by employing a layer-by-layer sheeting and fiber-laying method to produce fiber cement board, further improves fiber dispersion, resulting in neat fiber arrangement and high fiber utilization. The carbonization curing method not only fully activates the cementitious material but also reduces resource input and environmental pollution, yielding fiber cement board with higher strength and toughness.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of building materials technology, and in particular relates to a carbonized curing high-toughness fiber cement board, its preparation method and application. Background Technology

[0002] Fiber cement board is a widely used cement-based composite material, favored for its excellent physical properties in interior and exterior decoration materials such as wall panels, insulation boards, partitions, and ceilings. With the ban on asbestos fibers, more and more fiber cement boards are using natural plant fibers as reinforcement. However, plant fibers are brittle and easily become brittle under the alkaline environment and hydration reaction of cement, leading to brittle fracture and exhibiting low strength and poor toughness. Given current usage environments and market demands, the need for high-toughness fiber cement boards is increasing. Therefore, improving the toughness of fiber cement boards is an urgent problem to be solved. Furthermore, fiber cement boards are prone to deformation during traditional autoclaving, severely affecting their physical properties and durability. Summary of the Invention

[0003] To address the shortcomings of existing technologies, the present invention aims to provide a carbonized curing high-toughness fiber cement board, its preparation method, and its application.

[0004] The objective of this invention is achieved through the following technical solution:

[0005] A method for preparing a carbonation-cured high-toughness fiber cement board includes the following steps:

[0006] (1) Mix the first fiber, cementitious material, additives and water to obtain a slurry. The slurry is then sheeted to form a slurry layer. A second fiber is then laid flat on the slurry layer to form a fiber layer. The sheeting and laying are repeated to prepare the slurry layer and fiber layer in sequence until the specified thickness is reached to obtain the slab.

[0007] (2) The slab is subjected to pressure, pre-curing and static treatment in sequence, and then cured in CO2 atmosphere to obtain high toughness fiber cement board.

[0008] Preferably, in step (1), the mass ratio of the first fiber, the cementitious material, and the additive is (3.5-7):(89-94):(0.5-1.5).

[0009] Preferably, in step (1), the ratio of the mass of water to the total mass of the first fiber, cementing material and additives is 10:1.

[0010] In step (1), the first fiber is at least one of leaf pulp fiber, sulfate pulp fiber and cellulose fiber.

[0011] Preferably, in step (1), the length of the first fiber is 2 to 3 mm.

[0012] Preferably, in step (1), the cementing material is at least one of calcium silicate mineral powder, steel slag powder rich in calcium silicate mineral phase, and magnesium slag powder rich in calcium silicate mineral phase, and the average particle size of the cementing material is <50μm.

[0013] Preferably, the calcium silicate mineral powder includes at least one of γ-C2S, C3S2, and CS.

[0014] The mineral phase composition of steel slag powder rich in calcium silicate mineral phase preferably includes γ-type dicalcium silicate, RO phase, calcium ferrite, tricalcium silicate, free calcium oxide and free magnesium oxide, wherein the total mass content of dicalcium silicate and tricalcium silicate is preferably >40%.

[0015] The mineral phase composition of magnesium slag powder rich in calcium silicate mineral phase preferably includes γ-type dicalcium silicate, β-type dicalcium silicate and magnesium oxide, wherein the total mass content of dicalcium silicate is preferably >50%.

[0016] Preferably, in step (1), the additive is at least one of hydroxypropyl cellulose, hydroxymethyl cellulose, sodium hexametaphosphate and organosilicon coupling agent.

[0017] Preferably, in step (1), the thickness of a single layer of slurry is 175-350 μm, more preferably 250-280 μm.

[0018] Preferably, in step (1), the second fiber is at least one of PP fiber, PVA fiber and PAN fiber.

[0019] Preferably, in step (1), the length of the second fiber is 6 to 12 mm.

[0020] Preferably, the mass ratio of the first fiber to the second fiber is (2-13):1.

[0021] Preferably, in step (1), the thickness of the single layer of fiber is 16-40 μm, more preferably 25-35 μm.

[0022] Preferably, in step (2), the pressurization method is: the peak pressure is 20-30 MPa and the pressure holding time is 2-3 min.

[0023] Preferably, in step (2), the pre-curing temperature is 40-50℃, the relative humidity is ≤50%, and the time is 20-30min.

[0024] Preferably, in step (2), the standing time is 10 to 20 minutes at room temperature.

[0025] Preferably, in step (2), the curing parameters in the CO2 atmosphere are: CO2 pressure of 0.1-0.3 MPa, time of 2-48 h, volume concentration of ≥30%, temperature of 5-90 °C, and relative humidity of 30-80%.

[0026] The source of CO2 gas used in the CO2 atmosphere is preferably CO2-rich industrial kiln exhaust gas, or preferably high-concentration CO2 gas enriched from various industrial waste gases.

[0027] Preferably, in step (2), after curing in a CO2 atmosphere, the product is subjected to a water saturation treatment for 1 to 3 days.

[0028] The high-toughness fiber cement board prepared by the above-mentioned carbonization curing method is a high-toughness fiber cement board.

[0029] The above-mentioned high-toughness fiber cement board is used as an indoor and outdoor decorative material.

[0030] The mechanisms involved in this invention include:

[0031] To address the issues of low strength and poor toughness in traditional fiber cement boards, this invention improves the formulation and process by incorporating organic synthetic fibers with high tensile modulus to enhance the flexural and tensile strength of the fiber cement board. PP fibers, PVA fibers, and PAN fibers possess excellent hydrophobic properties, which can significantly reduce the water absorption rate of the fiber cement board, thereby improving its strength and durability.

[0032] To address the problem of poor fiber dispersibility, this invention introduces an additive. This additive ionizes in water to form anions and possesses surface activity. Large particles have pores or carry a positive charge on their surface, allowing them to adsorb anions. Consequently, the solid particles are separated by electrostatic repulsion, achieving dispersion. Furthermore, the addition of the additive increases the viscosity of the slurry, making the slurry suspension less prone to aggregation.

[0033] This invention produces fiber cement board by using a layer-by-layer fiber-laying method. Compared with traditional processes, this process further improves the dispersion of fibers, prevents the organic synthetic fibers from agglomerating, and results in neat fiber arrangement and high fiber utilization.

[0034] This invention employs carbonation curing for post-curing. The cementitious component used in this invention has carbonation activity, reacting with CO2 to generate calcium carbonate, a carbonation product that provides strength to the fiber cement board. Carbonation curing not only fully activates the activity of the cementitious material but also reduces resource input and environmental pollution. With traditional autoclaving, fiber cement boards using cement as the cementing material are prone to deformation, and cement hydration products can easily cause fiber embrittlement in the later stages, affecting the service life of the fiber cement board. However, for fiber cement boards cured with carbonation, the carbonation process significantly increases the density of the fiber cement board, improving its durability. High strength can be achieved within 2 hours of curing, and even higher strength and toughness can be obtained after 12 hours.

[0035] Compared with the prior art, the beneficial effects of the present invention include:

[0036] (1) The fiber cement board prepared by the present invention exhibits high flexural strength and tensile strength, low water absorption and low porosity.

[0037] (2) The present invention produces fiber cement board by using a layer-by-layer papering and flat fiber laying method. Compared with the traditional process, the fiber dispersion is further improved, the organic synthetic fiber will not agglomerate, the fiber is neatly arranged, and the fiber utilization rate is high.

[0038] (3) Carbonation curing can not only fully activate the activity of cementitious materials, but also reduce resource input and environmental pollution. Detailed Implementation

[0039] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0040] In Examples 1-3 and Comparative Examples 1-8, the average particle size of the cementitious materials used was <50 μm; the length of the first fiber was 2 mm, and the length of the second fiber was 6 mm. The chemical composition of the steel slag powder, by mass percentage, was: CaO 41.77%, MgO 10.73%, SiO2 9.8%, Al2O3 2.55%, and Fe2O3 29.24%; the chemical composition of the magnesium slag powder was: SiO2 28.87%, Fe2O3 8.17%, CaO 53.86%, and MgO 7.24%.

[0041] Example 1 (γ-C2S)

[0042] 93 parts of cementitious material (specifically γ-C2S in calcium silicate mineral powder), 6 parts of first fiber (specifically sulfate pulp fiber), 1 part of second fiber (specifically polyacrylonitrile fiber), and 1 part of additive (specifically Kh550).

[0043] A method for preparing a high-toughness fiber cement board with carbonation curing, comprising the following steps:

[0044] (1) According to the proportion, add the weighed cementitious material, first fiber, additive and 1000 parts of water to the mixing device and stir for 15 minutes to fully mix to form a slurry;

[0045] (2) Transfer the slurry into a papermaking wire mesh box and paper the slurry to form a slurry layer (single layer thickness is 250μm); lay a second fiber on the slurry layer to form a fiber layer (single layer thickness is 30μm); repeat the papermaking and laying to prepare the slurry layer and fiber layer in sequence until the specified thickness (specifically 7mm) is reached to obtain a slab; transfer the formed slab to a pressure mold and pressurize it with a pressure of 20MPa and a holding time of 2min;

[0046] (3) Remove the pressurized fiber cement board and place it in a curing box for pre-curing. The pre-curing conditions are 40℃, relative humidity below 50%, and curing time of 30min. The fiber cement board is pre-cured until the mass ratio of water to solid is 0.2:1.

[0047] (4) After pre-curing, the obtained fiber cement board is placed in a reactor and cured in a CO2 atmosphere at a temperature of 40°C, a relative humidity of 50%, a gas pressure of 0.2 MPa, and a time of 12 h. The CO2 gas is a high-concentration CO2 gas enriched from industrial waste gas with a CO2 volume concentration of 99%. After curing, a carbonized high-toughness fiber cement board is obtained. The carbonized high-toughness fiber cement board is saturated with water for 1 day and then its performance is tested.

[0048] Example 2 (Magnesium Slag)

[0049] Based on Example 1, the cementing material was replaced with magnesium slag, while the raw material ratio remained unchanged.

[0050] A method for preparing a high-toughness fiber cement board with carbonization curing, the steps are as follows: same as in Example 1.

[0051] Example 3 (Steel Slag)

[0052] Based on Example 1, the cementing material was replaced with steel slag, while the raw material ratio remained unchanged.

[0053] A method for preparing a high-toughness fiber cement board with carbonization curing, the steps are as follows: same as in Example 1.

[0054] Comparative Example 1 (Cement)

[0055] Based on Example 1, the cementitious material was replaced with cement (ordinary Portland cement, P·O 42.5), while the raw material ratio remained unchanged.

[0056] A method for preparing fiber cement board, comprising the following steps:

[0057] (1) According to the proportion, add the weighed cementitious material, first fiber, additive and 1000 parts of water to the mixing device and stir for 15 minutes to fully mix to form a slurry;

[0058] (2) Transfer the slurry into a papermaking wire mesh box and paper the slurry to form a slurry layer (single layer thickness is 250μm); lay a second fiber on the slurry layer to form a fiber layer (single layer thickness is 30μm); repeat the papermaking and laying to prepare the slurry layer and fiber layer in sequence until the specified thickness (specifically 7mm) is reached to obtain a slab; transfer the formed slab to a pressure mold and pressurize it with a pressure of 20MPa and a holding time of 2min;

[0059] (3) Remove the pressurized fiber cement board and pre-cur it at 20-25℃ for 4 hours. After pre-curing, perform autoclaving. The autoclaving regime is as follows: increase temperature and pressure for 3 hours, raise the temperature from room temperature to 180℃ to enter the pressure holding period, hold the pressure for 10 hours, and after the pressure holding period, enter the depressurization period for 3 hours. After curing, the autoclaved fiber cement board is obtained. The fiber cement board is saturated with water for 1 day, and then its performance is tested.

[0060] Comparative Example 2

[0061] Based on Example 1, the following were used: 93 parts of cementitious material (specifically γ-C2S in calcium silicate mineral powder), 6.9 parts of first fiber (specifically sulfate pulp fiber), 0.1 parts of second fiber (specifically polyacrylonitrile fiber), and 1 part of additive (specifically Kh550).

[0062] The preparation method is the same as in Example 1.

[0063] Comparative Example 3

[0064] Based on Example 1, the following were used: 93 parts of cementitious material (specifically γ-C2S in calcium silicate mineral powder), 4 parts of first fiber (specifically sulfate pulp fiber), 3 parts of second fiber (specifically polyacrylonitrile fiber), and 1 part of additive (specifically Kh550).

[0065] The preparation method is the same as in Example 1.

[0066] Comparative Example 4 (without the second fiber)

[0067] Based on Example 1, 93 parts of cementitious material (specifically γ-C2S in calcium silicate mineral powder), 7 parts of first fiber (specifically sulfate pulp fiber), and 1 part of additive (specifically Kh550).

[0068] The preparation method is the same as in Example 1.

[0069] Comparative Example 5 (without additives)

[0070] Based on Example 1, 93 parts of cementitious material (specifically γ-C2S in calcium silicate mineral powder), 6 parts of first fiber (specifically sulfate pulp fiber), and 1 part of second fiber (specifically polyacrylonitrile fiber) were used.

[0071] The preparation method is the same as in Example 1.

[0072] Comparative Example 6 (without second fiber and additives)

[0073] Based on Example 1, 93 parts of cementitious material (specifically γ-C2S in calcium silicate mineral powder) and 7 parts of first fiber (specifically sulfate pulp fiber) were used.

[0074] The preparation method is the same as in Example 1.

[0075] Comparative Example 7 (Slurry Method)

[0076] 93 parts of cementitious material (specifically γ-C2S in calcium silicate mineral powder), 6 parts of first fiber (specifically sulfate pulp fiber), 1 part of second fiber (specifically polyacrylonitrile fiber), and 1 part of additive (specifically Kh550).

[0077] A method for preparing fiber cement board, comprising the following steps:

[0078] (1) According to the proportion, add the weighed cementitious material, first fiber, additive and 1000 parts of water to the mixing device and stir for 15 minutes to fully mix to form a slurry;

[0079] (2) Pour the slurry into a vacuum filtration device for dewatering. The vacuum degree is 0.1 MPa. Filter until the green body is a whole and there is no obvious water flow. Transfer the formed slab to a pressure mold and apply pressure at 20 MPa for 2 minutes.

[0080] (3) Remove the pressurized fiber cement board and place it in a curing box for pre-curing. The pre-curing conditions are 40℃, relative humidity below 50%, and curing time of 30min. The fiber cement board is pre-cured until the mass ratio of water to solid is 0.2:1.

[0081] (4) After pre-curing, the obtained fiber cement board is placed in a reactor and cured in a CO2 atmosphere at a temperature of 40°C, relative humidity of 50%, gas pressure of 0.2MPa, and time of 12h. The CO2 gas is a high-concentration CO2 gas enriched from industrial waste gas with a CO2 volume concentration of 99%. After curing, a carbonized high-toughness fiber cement board is obtained. The carbonized high-toughness fiber cement board is saturated with water for 1 day and then its performance is tested.

[0082] Comparative Example 8 (Copying Method)

[0083] 93 parts of cementitious material (specifically γ-C2S in calcium silicate mineral powder), 6 parts of first fiber (specifically sulfate pulp fiber), 1 part of second fiber (specifically polyacrylonitrile fiber), and 1 part of additive (specifically Kh550).

[0084] A method for preparing fiber cement board, comprising the following steps:

[0085] (1) According to the proportion, add the weighed cementitious material, first fiber, second fiber, additive and 1000 parts of water to the mixing device and stir for 15 minutes to fully mix to form a slurry;

[0086] (2) Transfer the slurry into the forming wire mesh box for forming, and transfer the formed slab (7mm thick) into the pressure mold for pressing. The pressure is 20MPa and the holding time is 2min.

[0087] (3) Remove the pressurized fiber cement board and place it in a curing box for pre-curing. The pre-curing conditions are 40℃, relative humidity below 50%, and curing time of 30min. The fiber cement board is pre-cured until the mass ratio of water to solid is 0.2:1.

[0088] (4) After pre-curing, the obtained fiber cement board is placed in a reactor and cured in a CO2 atmosphere at a temperature of 40°C, relative humidity of 50%, gas pressure of 0.2MPa, and time of 12h. The CO2 gas is a high-concentration CO2 gas enriched from industrial waste gas with a CO2 volume concentration of 99%. After curing, a carbonized high-toughness fiber cement board is obtained. The carbonized high-toughness fiber cement board is saturated with water for 1 day and then its performance is tested.

[0089] The physical properties of the fiber cement boards prepared in Examples 1-3 and Comparative Examples 1-8 were tested. Bending strength, water absorption and porosity were tested according to GB / T7019-2014, and tensile strength was tested according to JCT2461-2018. Bending strength and tensile strength were the bending strength and tensile strength of the samples before and after water saturation, respectively. The test results are shown in Table 1.

[0090] Table 1. Summary of Physical Properties of Fiber Cement Board

[0091]

[0092]

[0093] The results of Examples 1-3 show that the present invention exhibits high flexural strength and tensile strength within a given formulation range. The fiber cement board with low water absorption and low porosity was obtained through the carbonization curing process. It also shows a consistent pattern for γ-C2S, magnesium slag or steel slag.

[0094] The results of Comparative Example 1 and Examples 1-3 show that, taking traditional fiber cement board and its curing process as an example, the curing process is relatively complicated, requires a lot of energy, takes a long time, and the fiber cement board has low strength and poor toughness after curing.

[0095] The results from Comparative Examples 2-3 and Example 1 show that outside the given formulation range, reducing or increasing the proportion of the second fiber affects the strength and toughness of the fiber cement board, and the fiber cement board does not perform as well as the fiber cement board within the formulation range.

[0096] The results from Comparative Examples 4-6 and Example 1 show that, for the control groups without the second fiber, without the additive, and without both the second fiber and the additive, the group without the second fiber exhibits better flexural strength and tensile strength before saturation, but after saturation, it has a high strength loss rate and high water absorption rate, making it unsuitable for high humidity environments. The group without the additive, whose main function is to disperse the fiber and increase viscosity, shows that Comparative Example 5 exhibits lower performance than Example 1, indicating that the additive plays a crucial role in the formulation and process of this invention. If neither the second fiber component nor the additive is incorporated, even worse physical and mechanical properties are observed.

[0097] The results of Comparative Examples 7-8 and Example 1 show that the paper-making and flat-laying production process provided by the present invention has good fiber dispersion, high fiber utilization, and good homogeneity of fiber cement board. Compared with the flow-forming method, the fiber cement board produced by the flow-forming method has poor performance and high water absorption, mainly due to its poor uniformity; compared with the traditional paper-making method, the fiber component dispersion is poor, and the performance of the fiber cement board after curing is not as good as that of Example 1.

[0098] The specific embodiments of the present invention described above do not constitute a limitation on the scope of protection of the present invention. Any other corresponding changes and modifications made in accordance with the technical concept of the present invention should be included within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a high-toughness fiber cement board with carbonation curing, characterized in that, Includes the following steps: (1) Mix the first fiber, cementitious material, additives and water to obtain slurry, and form a slurry layer by forming the slurry layer; lay a second fiber on the slurry layer to form a fiber layer; repeat forming and laying to prepare the slurry layer and fiber layer in sequence until the specified thickness is reached to obtain the slab. Step (1) The first fiber is a cellulose fiber; Step (1) The second fiber is at least one of PP fiber, PVA fiber and PAN fiber; (2) The slab is subjected to pressure, pre-curing and static treatment in sequence, and then cured in CO2 atmosphere to obtain the high toughness fiber cement board.

2. The method for preparing the high-toughness fiber cement board with carbonation curing according to claim 1, characterized in that, In step (1), the mass ratio of the first fiber, cementitious material, and additive is 3.5~7: 89~94: 0.5~1.5; The ratio of the mass of water in step (1) to the total mass of the first fiber, cementing material and additives is 10:1; The mass ratio of the first fiber to the second fiber is 2~13:

1.

3. The method for preparing high-toughness fiber cement board with carbonation curing according to claim 1, characterized in that, Step (1) The length of the first fiber is 2~3mm; Step (1) The length of the second fiber is 6~12mm.

4. The method for preparing high-toughness fiber cement board with carbonation curing according to claim 1 or 2, characterized in that, The cementing material in step (1) is at least one of calcium silicate mineral powder, steel slag powder rich in calcium silicate mineral phase, and magnesium slag powder rich in calcium silicate mineral phase, and the average particle size of the cementing material is <50μm. The additive in step (1) is at least one of hydroxypropyl cellulose, hydroxymethyl cellulose, sodium hexametaphosphate and organosilicon coupling agent.

5. The method for preparing high-toughness fiber cement board with carbonation curing according to claim 1, characterized in that, The thickness of a single layer of slurry in step (1) is 175~350μm; The thickness of the fiber layer in step (1) is 16~40μm.

6. The method for preparing high-toughness fiber cement board with carbonation curing according to claim 1 or 2, characterized in that, The pressurization method described in step (2) is as follows: the peak pressure is 20~30MPa, and the pressure holding time is 2~3min; The pre-curing temperature in step (2) is 40~50℃, the relative humidity is ≤50%, and the time is 20~30min; The step (2) involves letting the food stand at room temperature for 10-20 minutes.

7. The method for preparing high-toughness fiber cement board with carbonation curing according to claim 6, characterized in that, The parameters for curing in a CO2 atmosphere in step (2) are as follows: CO2 pressure is 0.1~0.3MPa, time is 2~48h, volume concentration is ≥30%, temperature is 5~90℃, and relative humidity is 30~80%; The source of the CO2 atmosphere is CO2-rich industrial kiln exhaust gas; Step (2) involves curing in a CO2 atmosphere followed by water saturation treatment, with a saturation time of 1-3 days.

8. The high-toughness fiber cement board prepared by the method of carbonization curing according to any one of claims 1 to 7.

9. The application of the high-toughness fiber cement board according to claim 8 as an indoor and outdoor decorative material.

Citation Information

Patent Citations

  • Hydrated and carbonized composite fiber cement board as well as preparation method and application thereof

    CN114368940A

  • Multi-layer process and apparatus for producing high strength fiber-reinforced structural cementitious panels with enhanced fiber content

    US20070110970A1