A high thermal conductivity and high dispersibility epoxy resin composition and its application
Through the blending of internal and external dispersants, the problem of poor thermal conductivity and filler dispersion in epoxy resin sealants is solved, the thermal conductivity and mechanical properties of the material are improved, and the stability and appearance quality of the product are enhanced.
Patent Information
- Application Number
- CN202410319281.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-20
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-03-20
AI Technical Summary
The problems of poor thermal conductivity and poor dispersion of inorganic fillers in existing epoxy resin sealants lead to poor mechanical and electrical properties of the material, as well as low production efficiency, which affects the stability and appearance of the product.
The internal dispersant and external dispersant are blended and added. The internal dispersant adheres to the surface of the filler to enhance the compatibility between the filler and the resin matrix. The external dispersant reduces the viscosity of the system and improves the uniform distribution and dispersion effect of the filler. Solving the problem Filler build-up and agglomeration issues.
It improves the thermal conductivity and mechanical properties of the material, reduces the expansion coefficient and interface thermal resistance, enhances the stability and appearance quality of the product, and improves the processing performance and anti-cracking effect.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure BDA0004750022370000031
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electronic packaging materials, and in particular to a high-thermal-conductivity and high-dispersibility epoxy resin composition and application thereof. Background Art
[0002] Epoxy molding compound (EMC) is generally composed of fillers, epoxy resins, phenolic resins, curing agents, flame retardants and other additives. Due to its excellent moisture resistance, high thermal conductivity, high reliability, excellent electrical insulation and mechanical properties, EMC has been widely used in the packaging field and has become the mainstream material for semiconductor components and integrated circuit packaging. However, with the miniaturization and integration of semiconductor components, the energy consumption of chips is increasing, and the ambient temperature of chips is getting higher and higher. If the heat generated by power semiconductors is not dissipated in time, its performance will be affected and will cause permanent damage to the components. Therefore, the packaging material is required to have a higher thermal conductivity to meet the heat dissipation requirements of components.
[0003] The method of improving its thermal conductivity mainly relies on the high thermal conductivity filler to form a thermal chain and a thermal network in the epoxy resin matrix. At present, the EMC constructed with filler silica (SiO2) cannot meet the high thermal conductivity requirements, and the high thermal conductivity of the EMC constructed with filler alumina (Al2O3) has become an indispensable packaging material in the electronic packaging industry. However, due to the large surface inertness of Al2O3 and the small number of reactive functional groups, the interface bonding is weak and the dispersion is poor, making it difficult to evenly distribute in the resin matrix, thereby reducing the mechanical strength and adhesion of the epoxy resin itself. For example, the patent technical document CN115286797B provides a thermal conductive filler surface treatment agent, a preparation method and its use. The invention can significantly reduce the viscosity of the composition by adding the thermal conductive filler to the thermal conductive composition after being treated with a surface treatment agent. However, this method will inevitably bring about dispersion problems. Poor dispersion will cause obvious defects in the material, thereby affecting the mechanical properties and electrical properties of the product, and will also have a negative impact on production operability.
[0004] In order to solve the above problems, Al2O3 can be surface modified by a coupling agent, which can improve the mechanical properties of the material to a certain extent. However, the surface tension of the surface-modified Al2O3 is different from that of the resin, and the compatibility with the resin is poor, making it difficult for the resin to wet and disperse on the surface of the Al2O3 particles, so that there are gaps at the interface, which increases the interfacial thermal resistance of the composite material and easily causes Al2O3 to agglomerate in the resin. For example, the patent technical document CN115819845A provides a filler modification method, a modified filler and a filled thermally conductive epoxy resin. The invention improves the thermal conductivity of the epoxy resin by coating polydopamine on the surface of the etched Al2O3, but the process is cumbersome and complicated, and the production efficiency is low in the actual production process. It cannot be directly used in the curing system and has a narrow application field. In the actual production process, the wetting and dispersion of the filler when reinforcing the resin matrix is an indispensable process. The dispersion effect of the filler in the matrix is related to the properties of the filler and the resin, but it is difficult to obtain a stable filler dispersion system relying solely on the interaction between the two.
[0005] Therefore, in view of the above-mentioned related technologies, it is urgent to develop a high thermal conductivity and high dispersibility epoxy resin composition and its application. Summary of the invention
[0006] In view of this, the purpose of the present invention is to provide a high thermal conductivity and high dispersibility epoxy resin composition and its application to solve the problems of poor thermal conductivity of epoxy resin in epoxy molding compound and poor dispersibility of inorganic filler therein in the prior art.
[0007] Based on the above objectives, the present invention provides a high thermal conductivity and high dispersibility epoxy resin composition and application thereof.
[0008] A high thermal conductivity and high dispersibility epoxy resin composition, the epoxy resin composition is prepared from the following raw materials in parts by weight: 4-10 parts of epoxy resin, 2-10 parts of phenolic resin, 70-95 parts of inorganic filler, 0.1-0.3 parts of colorant, 0.2-0.6 parts of release agent, 0.3-1 parts of coupling agent, 0.05-0.5 parts of curing accelerator, 0.2-1.5 parts of reactive stress modifier, 0.2-1.5 parts of internal dispersant, and 0.2-1.5 parts of external dispersant;
[0009] The structural formula of the internal dispersant is as follows:
[0010]
[0011] The value range of n is 30-50;
[0012] The structural formula of the external dispersant is as follows:
[0013]
[0014] Where x:y=3:7, the value range of x is 10-30;
[0015] Preferably, the epoxy resin is any one of o-cresol-formaldehyde epoxy resin, dicyclopentadiene-formaldehyde epoxy resin, polyaromatic epoxy resin, polyfunctional epoxy resin, biphenyl-formaldehyde epoxy resin, naphthol-formaldehyde epoxy resin and thioether-formaldehyde epoxy resin.
[0016] Preferably, the phenolic resin is any one of phenol ether phenolic resin, o-methyl phenolic resin, biphenyl phenolic resin, polyaromatic phenolic resin and phenol aralkyl phenolic resin.
[0017] Preferably, the inorganic filler is a mixture of alumina and crystalline angular silica in a mass ratio of 77-82:8, the maximum size of the alumina is 70 μm, the maximum size of the crystalline angular silica is 10 μm, and the colorant is carbon black.
[0018] Preferably, the release agent is a wax compound, and more preferably, the release agent is any one of palm wax, montanate wax, polyethylene wax, oxidized polyethylene wax and polyamide wax.
[0019] Preferably, the coupling agent is any one of a mercapto-type siloxane coupling agent, an amino-type siloxane coupling agent and an epoxy-type siloxane coupling agent.
[0020] Preferably, the curing accelerator is any one of an imidazole compound, a tertiary amine compound, and an organic phosphine compound.
[0021] Preferably, the reactive stress modifier is any one of carboxyl silicone oil, amino silicone oil and epoxy silicone oil.
[0022] Preferably, the preparation method of the internal dispersant is as follows:
[0023] P2O5 and toluene are added to a flask, and then methoxy polyethylene glycol and acetone are added. The temperature is raised to 58-62°C and maintained for 1.8-2.2 hours under stirring. The acetone is then evaporated using a distillation device. After adding distilled water, the temperature is raised to 88-92°C and hydrolyzed for 0.8-1.2 hours. Finally, toluene is removed to obtain an internal dispersant.
[0024] The mass ratio of P2O5, toluene, methoxy polyethylene glycol, acetone and distilled water is 0.1-0.2:0.4-0.6-20:35-45:35-45:0.8-1.
[0025] Preferably, the preparation method of the external dispersant is as follows:
[0026] In a nitrogen atmosphere, an initiator and potassium hydroxide are added to a reaction kettle, and then ethylene oxide and propylene oxide are evenly mixed, and the mixture is reacted at 100-110° C. for 8-10 hours. After the reaction is completed, the mixture is neutralized, dehydrated, dried, and filtered to obtain an external dispersant;
[0027] The mass ratio of the initiator, potassium hydroxide and ethylene oxide is 0.24-0.28:0.2-0.3:2-4, and the initiator is any one of 1,2-propylene glycol, n-butanol and n-octanol.
[0028] The invention discloses an application of a high thermal conductivity and high dispersibility epoxy resin composition, wherein the epoxy resin composition is used in the field of chip packaging, semiconductor packaging, electronic devices, and electromechanical product packaging and protection.
[0029] Beneficial effects of the present invention:
[0030] When the internal dispersant and the external dispersant provided by the present invention are blended and added, the two additives have a synergistic effect. The external dispersant has low viscosity, good fluidity, and high lipophilicity, and can quickly disperse and flow in the system, thereby reducing the viscosity of the entire system, so that more fillers can be filled into a unit volume of resin, reducing costs, and improving processing performance in the later stage molding process. In addition, under the action of the external dispersant, the internal dispersant can adhere to the surface of the filler, thereby enhancing the compatibility between the filler particles and the resin matrix, so that the filler can be evenly distributed inside the resin, and the comprehensive performance of the product is greatly improved.
[0031] When the internal dispersant provided by the present invention is coated on the surface of the filler particles, the surface will be transformed from a solid-gas interface to a solid-liquid interface. Therefore, the internal dispersant has a certain defoaming effect, which can effectively solve the pore problem caused by improper stacking of fillers in the final product during processing. In addition, the strong interface affinity can effectively reduce stratification and overflow in the actual packaging process, and can also appropriately reduce the expansion coefficient. The anti-cracking effect can be improved during the hot and cold cycle process, thereby improving product stability.
[0032] The internal dispersant provided by the present invention also has a good dispersing effect on the colorant carbon black, which can effectively solve the problem of surface defects caused by mold flow marks caused by the easy agglomeration of carbon black during the packaging process, so that the product appearance has no color difference, no dirt, adds gloss, and improves leveling. DETAILED DESCRIPTION
[0033] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments.
[0034] The sources or properties of the raw materials used in the examples and comparative examples of the present invention are as follows:
[0035] Methoxypolyethylene glycol was purchased from Haian Petrochemical Plant in Jiangsu Province, model MPEG-350.
[0036] Embodiment 1: A method for preparing a high thermal conductivity and high dispersibility epoxy resin composition, comprising the following steps:
[0037] S1. Add 0.1g P2O5 and 0.4g toluene into a flask, add 35g methoxy polyethylene glycol and 35g acetone, raise the temperature to 58°C and keep for 1.8h under stirring, then use a distillation device to evaporate the acetone, add 0.8g distilled water and raise the temperature to 88°C for hydrolysis for 0.8h, and finally remove the toluene to obtain an internal dispersant;
[0038] S2. 0.24 g of 1,2-propylene glycol and 0.2 g of potassium hydroxide were added to a reactor under a nitrogen atmosphere, and then 2 g of ethylene oxide and 6.15 g of propylene oxide were added and mixed uniformly, and the mixture was reacted at 100 ° C for 8 h. After the reaction was completed, the mixture was neutralized, dehydrated, dried, and filtered to obtain an external dispersant;
[0039] S3. Add 5g of o-cresol epoxy resin NPCN-702, 3g of phenol ether phenolic resin, 77g of alumina with a maximum size of 70μm, 8g of crystalline silica with a maximum size of 10μm, 0.2g of palm wax, 0.2g of oxidized polyethylene wax, 0.3g of alkyl silane, 0.05g of 2,4-diamino-6-[2-(2-methyl-1-imidazole)ethyl]-1,3,5-triazine, 0.2g of carboxyl silicone oil, 0.1g of carbon black, 0.2g of internal dispersant and 0.2g of external dispersant into a high-speed mixer in sequence, mix well, melt-knead on an open rubber mixer at 95°C, remove the evenly mixed material from the open rubber mixer, cool and crush to obtain a powdery material, and finally preform into a cake material to obtain an epoxy resin composition.
[0040] Embodiment 2: A method for preparing a high thermal conductivity and high dispersibility epoxy resin composition, comprising the following steps:
[0041] S1. Add 0.13g P2O5 and 0.47g toluene into a flask, add 38g methoxy polyethylene glycol and 38g acetone, raise the temperature to 59°C and keep for 1.9h under stirring, then distill off the acetone using a distillation apparatus, add 0.87g distilled water and raise the temperature to 89°C for hydrolysis for 1.0h, and finally remove the toluene to obtain an internal dispersant;
[0042] S2. 0.26 g of n-butanol and 0.23 g of potassium hydroxide were added to the reactor under a nitrogen atmosphere, and then 2.7 g of ethylene oxide and 8.3 g of propylene oxide were added and mixed, and the mixture was reacted at 103 ° C for 8.7 h. After the reaction was completed, the mixture was neutralized, dehydrated, dried, and filtered to obtain an external dispersant;
[0043] S3. Add 6g of biphenyl epoxy resin BNPE-3501LL, 5g of o-methylphenolic resin, 79g of alumina with a maximum size of 70μm, 8g of crystalline silica with a maximum size of 10μm, 0.3g of palm wax, 0.3g of oxidized polyethylene wax, 0.5g of aminosilane, 0.2g of 2,4-diamino-6-[2-(2-methyl-1-imidazole)ethyl]-1,3,5-triazine, 0.6g of aminosilicone oil, 0.2g of carbon black and 0.3g of internal dispersant and 0.3g of external dispersant into a high-speed mixer in sequence, mix well, melt-knead on an open rubber mixer at 90°C, remove the evenly mixed material from the open rubber mixer, cool and crush to obtain a powdery material, and finally preform into a cake material to obtain an epoxy resin composition.
[0044] Embodiment 3: A method for preparing a high thermal conductivity and high dispersibility epoxy resin composition, comprising the following steps:
[0045] S1. Add 0.16g P2O5 and 0.54g toluene into a flask, add 42g methoxy polyethylene glycol and 42g acetone, raise the temperature to 61°C and keep for 2.1h under stirring, then use a distillation device to evaporate the acetone, add 0.94g distilled water and raise the temperature to 91°C for hydrolysis for 1.1h, and finally remove the toluene to obtain an internal dispersant;
[0046] S2. 0.27 g of n-octanol and 0.26 g of potassium hydroxide were added to the reactor under a nitrogen atmosphere, and then 3.4 g of ethylene oxide and 10.46 g of propylene oxide were added and mixed, and the reaction was carried out at 106 ° C for 9.4 h. After the reaction was completed, it was neutralized, dehydrated, dried, and filtered to obtain an external dispersant;
[0047] S3. Add 8g of bisphenol A epoxy resin E-12, 8g of biphenyl phenolic resin, 81g of alumina with a maximum size of 70μm, 8g of crystalline silica with a maximum size of 10μm, 0.4g of palm wax, 0.1g of oxidized polyethylene wax, 0.1g of phenyl silane, 0.35g of 2,4-diamino-6-[2-(2-methyl-1-imidazole)ethyl]-1,3,5-triazine, 1.0g of epoxy silicone oil, 0.25g of carbon black, 0.5g of internal dispersant and 0.5g of external dispersant into a high-speed mixer in sequence, mix well, melt-knead on an open rubber mixer at 105°C, remove the evenly mixed material from the open rubber mixer, cool and crush to obtain a powdery material, and finally preform into a cake material to obtain an epoxy resin composition.
[0048] Embodiment 4: A method for preparing a high thermal conductivity and high dispersibility epoxy resin composition, comprising the following steps:
[0049] S1. Add 0.2g P2O5 and 0.6g toluene into a flask, add 45g methoxy polyethylene glycol and 45g acetone, raise the temperature to 62°C and keep for 2.2h under stirring, then use a distillation device to evaporate the acetone, add 1g distilled water and raise the temperature to 92°C for hydrolysis for 1.2h, and finally remove the toluene to obtain an internal dispersant;
[0050] S2. 0.28 g of n-octanol and 0.3 g of potassium hydroxide were added to the reactor under a nitrogen atmosphere, and then 4 g of ethylene oxide and 12.3 g of propylene oxide were added and mixed uniformly, and the reaction was carried out at 110 ° C for 10 h. After the reaction was completed, it was neutralized, dehydrated, dried, and filtered to obtain an external dispersant;
[0051] S3. 10g of o-cresol epoxy resin NPCN-702, 10g of phenol ether phenolic resin, 82g of alumina with a maximum size of 70μm, 8g of crystalline silica with a maximum size of 10μm, 0.5g of palm wax, 0.1g of oxidized polyethylene wax, 1.0g of mercaptosilane, 0.5g of 2,4-diamino-6-[2-(2-methyl-1-imidazole)ethyl]-1,3,5-triazine, 1.5g of epoxy silicone oil, 0.3g of carbon black and 0.75g of internal dispersant and 0.75g of external dispersant are added to a high-speed mixer in sequence, mixed evenly, melt-kneaded on an open rubber mixer at 100°C, the evenly mixed material is removed from the open rubber mixer, cooled and crushed to obtain a powdery material, and finally preformed into a cake material to obtain an epoxy resin composition.
[0052] Comparative Example 1:
[0053] Compared with Example 1, the internal dispersant and the external dispersant were not added during the preparation of the epoxy resin composition in this comparative example, and the remaining steps and parameters were the same, which will not be repeated in this comparative example. Finally, the epoxy resin composition was prepared.
[0054] Comparative Example 2:
[0055] Compared with Example 1, this comparative example did not add an internal dispersant during the preparation of the epoxy resin composition, and the remaining steps and parameters were the same, which will not be repeated in this comparative example. Finally, an epoxy resin composition was prepared.
[0056] Comparative Example 3:
[0057] Compared with Example 1, this comparative example did not add an external dispersant during the preparation of the epoxy resin composition, and the remaining steps and parameters were the same, which will not be repeated in this comparative example. Finally, an epoxy resin composition was prepared.
[0058] Comparative Example 4: A method for preparing an epoxy composition, comprising the following steps:
[0059] S1. Add 0.1g P2O5 and 0.4g toluene into a flask, add 35g methoxy polyethylene glycol and 35g acetone, raise the temperature to 58°C and keep for 1.8h under stirring, then use a distillation device to evaporate the acetone, add 0.8g distilled water and raise the temperature to 88°C for hydrolysis for 0.8h, and finally remove the toluene to obtain an internal dispersant;
[0060] S2. 0.24 g of 1,2-propylene glycol and 0.2 g of potassium hydroxide were added to a reactor under a nitrogen atmosphere, and then 6.15 g of ethylene oxide and 2 g of propylene oxide were added and mixed, and the mixture was reacted at 100 ° C for 8 h. After the reaction was completed, the mixture was neutralized, dehydrated, dried, and filtered to obtain an external dispersant;
[0061] S3. Add 4g of o-cresol epoxy resin NPCN-702, 2g of phenol ether phenolic resin, 77g of alumina with a maximum size of 70μm, 8g of crystalline silica with a maximum size of 10μm, 0.2g of palm wax, 0.2g of oxidized polyethylene wax, 0.3g of alkyl silane, 0.05g of 2,4-diamino-6-[2-(2-methyl-1-imidazole)ethyl]-1,3,5-triazine, 0.2g of carboxyl silicone oil, 0.1g of carbon black, 0.2g of internal dispersant and 0.2g of external dispersant into a high-speed mixer in sequence, mix well, melt-knead on an open rubber mixer at 100°C, remove the evenly mixed material from the open rubber mixer, cool and crush to obtain a powdery material, and finally preform into a cake material to obtain an epoxy resin composition.
[0062] Performance Test:
[0063] Referring to GB / T40564-2021 "Test Method for Epoxy Molding Materials for Electronic Packaging", the spiral flow length, gelation time, flash, viscosity, bending strength, hot hardness, appearance inspection and thermal conductivity of the epoxy resin compositions prepared in Examples 2-6 and Comparative Examples 1-2 were measured;
[0064] TCT test: The epoxy resin compositions prepared in Examples 2-6 and Comparative Examples 1-2 were pressed into products with a height of 50 mm, an inner diameter of 25 mm, and an outer diameter of 30 mm by a molding machine, and the mold temperature was 175 ± 2 ° C and the injection pressure was 80 ± 2 kg / cm 2 The molded product was post-cured at 175±2℃ for 6h, then taken out and cooled at room temperature, and then placed in a hot and cold cycle shock test box from -35℃ to 130℃, 2h cycle once, for 300 cycles, to check the cracking of the product. The results are shown in Table 1 below:
[0065] Table 1 Summary of experimental results
[0066]
[0067] Data Analysis:
[0068] As can be seen from Table 1, from Comparative Examples 2 and 3, when the internal dispersant and the external dispersant are added separately, the additives cannot wet the filler surface well, which is manifested as a short flow length, excessive flash, low strength at room temperature, and high brittleness of the product. In the later stage of packaging, the flash is too large to be removed, which will affect the electroplating effect, and there is also a risk of breakage during mold opening and application. Compared with conventional product formulas, the overall performance is not good.
[0069] It can be seen from Example 1, Comparative Example 1 and Comparative Example 4 that the internal dispersant and the external dispersant and their dosage relationship play a key role in the comprehensive performance of the final product, which is manifested in that when the internal dispersant and the external dispersant are not added to the system and the addition amounts of ethylene oxide and propylene oxide are changed, the comprehensive performance of the final product is poor.
[0070] As can be seen from Examples 2 to 4, when the internal dispersant and the external dispersant are blended and added, the two additives have a synergistic effect. The external dispersant has poor compatibility with the matrix, quickly disperses and flows in the system, reduces the viscosity of the entire system, and improves processing performance during the later stage of molding. Under the action of the external dispersant, the internal dispersant can adhere to the surface of the filler, thereby enhancing the compatibility between the filler particles and the resin matrix, so that the filler can be evenly distributed inside the resin, and the comprehensive performance of the product is greatly improved, which is manifested in an increase in flow length, an extension of curing time, a reduction in flash, a decrease in modulus while the strength increases, an increase in hardness when hot, and an increase in thermal conductivity. In addition, due to the strong interfacial affinity of the wetting dispersant, the expansion coefficient can be appropriately reduced in product applications, and the anti-cracking effect can be improved during the hot and cold cycle process. The surface is free of cracks when observed under a microscope, which can improve product stability, so it can pass the TCT test.
[0071] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.
[0072] The present invention is intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.
Claims
1. A high thermal conductivity and high dispersibility epoxy resin composition, characterized in that: The epoxy resin composition is prepared from the following raw materials in parts by weight: 4-10 parts of epoxy resin, 2-10 parts of phenolic resin, 70-95 parts of inorganic filler, 0.1-0.3 parts of colorant, 0.2-0.6 parts of release agent, 0.3-1 parts of coupling agent, 0.05-0.5 parts of curing accelerator, 0.2-1.5 parts of reactive stress modifier, 0.2-1.5 parts of internal dispersant, and 0.2-1.5 parts of external dispersant; The structural formula of the internal dispersant is as follows: The value range of n is 30-50; The structural formula of the external dispersant is as follows: Where x:y=3:7, and the value range of x is 10-30.
2. The high thermal conductivity and high dispersibility epoxy resin composition according to claim 1, characterized in that: The epoxy resin is any one of o-cresol epoxy resin, dicyclopentadiene epoxy resin, polyaromatic epoxy resin, polyfunctional epoxy resin, biphenyl epoxy resin, naphthol phenolic epoxy resin and thioether epoxy resin.
3. The high thermal conductivity and high dispersibility epoxy resin composition according to claim 1, characterized in that: The phenolic resin is any one of phenolic ether phenolic resin, o-methyl phenolic resin, biphenyl phenolic resin and polyaromatic phenolic resin.
4. The high thermal conductivity and high dispersibility epoxy resin composition according to claim 1, characterized in that: The inorganic filler is obtained by mixing aluminum oxide and crystalline angular silica in a mass ratio of 77-82:
8. The maximum size of the aluminum oxide is 70 μm, the maximum size of the crystalline angular silica is 10 μm, and the colorant is carbon black.
5. The high thermal conductivity and high dispersibility epoxy resin composition according to claim 1, characterized in that: The release agent is any one of palm wax, montanate wax, polyethylene wax, oxidized polyethylene wax and polyamide wax.
6. The high thermal conductivity and high dispersibility epoxy resin composition according to claim 1, characterized in that: The coupling agent is any one of a mercapto-type siloxane coupling agent, an amino-type siloxane coupling agent and an epoxy-type siloxane coupling agent.
7. The high thermal conductivity and high dispersibility epoxy resin composition according to claim 1, characterized in that: The curing accelerator is any one of imidazole compounds, tertiary amine compounds, and organic phosphine compounds, and the reactive stress modifier is one or more of carboxyl silicone oil, amino silicone oil, and epoxy silicone oil.
8. An application of the high thermal conductivity and high dispersibility epoxy resin composition according to any one of claims 1 to 7, characterized in that: The epoxy resin composition is used in the field of packaging and protection of electromechanical products.