Preparation method of V-4Cr-4Ti alloy
By layering vanadium filaments and sponge titanium-chromium particles and pressing them into block-shaped consumable electrodes, the problems of high cost and poor uniformity in the preparation of V-4Cr-4Ti alloys were solved, achieving alloy preparation with lower cost and higher uniformity.
Patent Information
- Application Number
- CN202410333412.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-22
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-03-22
AI Technical Summary
Existing methods for preparing V-4Cr-4Ti alloys are costly and produce poor alloy uniformity, especially with significant uneven distribution of chromium and titanium.
A mixture of vanadium filaments, sponge titanium, and chromium particles is layered and pressed into blocks using a forging press. This mixture is then used as a consumable electrode in a VAR furnace for smelting. The winding structure of the vanadium filaments and the microporous properties of the sponge titanium are used to improve the material bonding tightness and reduce the amount of unmelted slag falling into the molten pool. Combined with electromagnetic stirring, alloy homogeneity is achieved.
It reduced raw material costs, improved the uniformity of V-4Cr-4Ti alloy, especially the uniformity of chromium, and enhanced the quality of the alloy.
Smart Images

Figure CN118222861B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of alloy preparation technology, and in particular to a method for preparing a V-4Cr-4Ti alloy. Background Technology
[0002] Nuclear fusion is an energy generation method whose core principle is to fuse light elements into heavier elements, releasing enormous energy. In nuclear fusion reactors, the fusion blanket structural material is used as the first wall / cladding component, withstanding the impact and radiation damage from high temperatures and high-energy particles. The vanadium-based alloy V-4Cr-4Ti is considered a candidate structural material for the first wall / cladding component due to its low activation, stable high-temperature strength, good compatibility with liquid metals, and resistance to neutron radiation damage. Existing technologies generally employ two methods to prepare V-4Cr-4Ti alloys. One method uses V, Cr, and Ti metal oxides as raw materials, electrolyzing them in molten salt to remove oxygen from the oxides, thus producing the V-4Cr-4Ti alloy. The other method uses elemental V, Cr, and Ti as raw materials to create consumable electrodes, and then prepares the V-4Cr-4Ti alloy in a vacuum arc remelting (VAR) furnace. There are two existing methods for preparing consumable electrodes. One method involves weighing vanadium plates, chromium materials, and titanium materials, pouring them into a crucible, and then preparing the consumable electrode in a melting furnace. For example, the patent application with application number 202011426301.2, entitled "A Vanadium-Chromium-Titanium Alloy and Its Preparation Method," uses this method. However, this method requires melting the materials first, which consumes a lot of energy. The other method involves using isostatic pressing (IOP) to press vanadium powder, chromium powder, and titanium powder into a dense billet under high pressure to form the consumable electrode. This process currently has many problems. On the one hand, the metal powder is relatively expensive, and the IOP process requires high pressure, generally reaching hundreds of megapascals, making the prepared V-4Cr-4Ti alloy costly. On the other hand, due to the poor adhesion of the powder, some unmelted slag easily falls into the molten pool when the billet is melted in the VAR furnace, affecting the strength and uniformity of the alloy after cooling. Summary of the Invention
[0003] Therefore, it is necessary to provide a method for preparing V-4Cr-4Ti alloy with lower cost and more uniform alloy composition.
[0004] A method for preparing a V-4Cr-4Ti alloy includes the following steps:
[0005] Step S1: Arrange vanadium filaments, sponge titanium, and chromium particles in three layers in a predetermined ratio in a material tank. The vanadium filaments are located in the bottom and top layers, while the titanium and chromium particles are located in the middle layer. The thickness of the vanadium filaments is less than or equal to 1 mm, and the width is 2 to 3 mm. The particle size of the sponge titanium is 20 to 50 mm, and the particle size of the chromium particles is 1 to 6 mm.
[0006] Step S2: Use a forging press to press the material in the trough into a block mixture, with a pressure greater than or equal to 40MPa;
[0007] Step S3: Using the block mixture as a consumable electrode, the block mixture is smelted once in a VAR furnace to obtain V-4Cr-4Ti alloy.
[0008] Compared to isostatic pressing, which involves extruding mixed powders into blocks for melting V-4Cr-4Ti alloy, this invention uses filamentous vanadium, sponge titanium, and chromium particles to extrude and melt V-4Cr-4Ti alloy, which has the following advantages:
[0009] Firstly, compared to powder, the raw material cost of this invention is lower;
[0010] Secondly, the vanadium filaments of the present invention are intertwined and can wrap around the sponge titanium, and the chromium particles can also enter the gaps in the sponge strips, making the extruded block mixture more tightly bonded, the extrusion process simpler, and the required pressure lower.
[0011] The block mixture prepared by layering and pressing has a more compact structure. During smelting, the intertwined filament structure can effectively reduce the amount of unmelted slag falling into the molten pool, thereby improving the uniformity of the alloy after smelting.
[0012] Instruction manual illustrations
[0013] Figure 1 This is a schematic diagram of the sampling points of the V-4Cr-4Ti alloy of the present invention. Detailed Implementation
[0014] To more clearly illustrate the technical solution of the present invention, the following will provide a detailed description in conjunction with embodiments.
[0015] The preparation method of V-4Cr-4Ti alloy includes the following steps:
[0016] Step S1: Arrange vanadium filaments, sponge titanium, and chromium particles in three layers in a predetermined ratio in a material tank. The vanadium filaments are located in the bottom and top layers, while the titanium and chromium particles are located in the middle layer. The thickness of the vanadium filaments is less than or equal to 1 mm, and the width is 2 to 3 mm. The particle size of the sponge titanium is 20 to 50 mm, and the particle size of the chromium particles is 1 to 6 mm.
[0017] Vanadium raw materials are generally available in powder or ingot form. Vanadium ingots are cheaper to purchase than powdered raw materials. Vanadium filaments can be processed using a planer. Filaments of vanadium have a certain degree of flexibility and can be intertwined, effectively wrapping around sponge ingots and chromium particles, making them less prone to detachment. Simultaneously, the sponge titanium contains numerous micropores, making it even more difficult for chromium particles to separate once they enter the micropores, resulting in a tighter bond during pressing.
[0018] Excessive thickness of the vanadium filaments makes it difficult to achieve a bending effect, while also reducing flexibility and increasing brittleness. This makes them prone to breakage during subsequent pressing. Therefore, the thickness of the vanadium filaments in this invention is less than or equal to 1 mm. Conversely, excessive width of the vanadium filaments leads to poor mixing, while excessively narrow filaments are prone to breakage. Therefore, the width of the vanadium filaments in this invention is 2–3 mm.
[0019] During fabrication, the underlying vanadium filaments intertwine and create numerous pores. Some chromium particles roll into these pores and mix with the vanadium filaments, allowing for better bonding during subsequent pressing. The vanadium filaments and titanium intertwine at their interfaces, resulting in a tighter bond during further pressing.
[0020] Step S2: Use a forging press to press the material in the trough into a block mixture, with a pressure greater than or equal to 40MPa;
[0021] In a preferred embodiment, the feed trough of the forging press is cylindrical, so that the pressed block mixture is cylindrical and has three layers, with the upper and lower layers being vanadium and the middle layer being titanium and chromium.
[0022] Step S3: Use a VAR furnace to perform a single melting of the block mixture to obtain V-4Cr-4Ti alloy.
[0023] In a preferred embodiment, the V-4Cr-4Ti alloy after smelting can be smelted a second time in order to remove or reduce impurities in the alloy.
[0024] The lumpy mixture serves as the consumable electrode in the VAR furnace. During operation, the consumable electrode is held in place by clamps and suspended directly above the molten pool. Upon energization, an arc plasma zone with extremely high temperatures is formed between the lower end of the consumable electrode and the molten pool, melting the end of the lumpy mixture. The bottom layer of the consumable electrode is vanadium, so it melts and falls into the molten pool first. Following this, as the vanadium melts and the consumable electrode descends, the middle layers of titanium and chromium melt into the molten pool, and finally, the upper layer of vanadium melts into the molten pool. The VAR furnace features electromagnetic stirring to ensure uniform mixing of vanadium, chromium, and titanium.
[0025] Vanadium, chromium, and titanium have different melting points. Vanadium has a melting point of 1890 degrees Celsius; chromium has a melting point of 1907 degrees Celsius; and titanium has a melting point of 1668 degrees Celsius. Titanium's melting point is significantly lower than vanadium's, while vanadium and chromium have similar melting points.
[0026] The different pressing methods used for vanadium, titanium, and chromium raw materials result in different melting effects when used as electrodes. For example, if titanium and chromium are encased in vanadium to form a consumable electrode, the titanium and chromium inside will fall off the electrode before the vanadium melts. Titanium, with its lower melting point, may melt in the molten pool, but chromium, with its higher melting point, is likely to accumulate in the molten pool, resulting in uneven distribution of the alloy in the molten pool after cooling.
[0027] For example, if vanadium, titanium, and chromium powders are isostatically pressed into electrodes, the formed billet is greatly affected by thermal expansion and contraction after heating. This causes the billet to become loose in certain areas, and some slag falls into the molten pool before melting. If the temperature in the molten pool is insufficient to raise the slag to its melting point, the slag will remain in the molten pool until the pool cools, resulting in an uneven alloy composition.
[0028] The electrode of the V-4Cr-4Ti alloy preparation method of the present invention, i.e. the block mixture, adopts a layered structure and uses filamentous vanadium, sponge titanium and chromium particles. The materials are tightly bonded, the materials are not easy to fall off during the melting process, the materials melt more completely, and the resulting alloy has good uniformity.
[0029] In the V-4Cr-4Ti alloy, vanadium accounts for up to 90% of the mass, while chromium and titanium are present in smaller quantities. During the process of melting vanadium, chromium, and titanium into an alloy, chromium and titanium are more prone to uneven distribution. Although the VAR furnace's molten pool has electromagnetic stirring capabilities, which can help distribute chromium and titanium as evenly as possible in the melt, if unmelted material falls into the pool, it essentially agglomerates at the microscopic level, failing to disperse within the alloy. Chromium, in particular, has a higher melting point than the other two metals and is present in smaller quantities; if it falls into the molten pool unmelted, the alloy's uniformity will be significantly affected.
[0030] The present invention will be described below through specific embodiments.
[0031] Example 1: Preparation of V-4Cr-4Ti alloy using the method of the present invention
[0032] Vanadium plates are planed into 0.9 mm thick and 3 mm wide vanadium filaments using a planer. First, 0.455 tons of vanadium filaments are added to the feed trough below the forging press using a feeding machine. Then, 0.042 tons of sponge titanium and 0.042 tons of chromium particles are added to the vanadium filaments using the feeding machine. The sponge titanium particles have a diameter of 40–45 mm, and the chromium particles have a diameter of 2–3 mm. Next, another 0.455 tons of vanadium filaments are added to the titanium and chromium using a feeding machine. Finally, the material in the feed trough is pressed into a block mixture using a forging press at a pressure of 40 MPa. The block mixture is then transferred to a VAR furnace as a consumable electrode. The tip of the consumable electrode gradually melts into the molten pool under high temperature, and the liquid alloy in the molten pool is stirred evenly under electromagnetic stirring. After cooling, a V-4Cr-4Ti alloy is obtained.
[0033] Example 2:
[0034] 0.91 tons of 200-mesh vanadium powder, 0.042 tons of 200-mesh titanium powder, 0.042 tons of 200-mesh chromium powder, and alcohol were added to a mixer and mixed evenly using a wet mixing method. The mixture was then dried and pressed into blocks using an isostatic pressing machine at a pressure of 200 MPa. The block mixture was then transferred to a VAR furnace as a consumable electrode. The tip of the consumable electrode gradually melted into the molten pool under high temperature, and the liquid alloy in the molten pool was stirred evenly under electromagnetic stirring. After cooling, a V-4Cr-4Ti alloy was obtained.
[0035] The uniformity of the V-4Cr-4Ti alloys obtained after smelting in the two embodiments described above was tested. Please refer to [link / reference needed]. Figure 1 Twelve alloy samples were selected from four points on the upper surface, four points on the middle edge, and four points on the lower surface of the V-4Cr-4Ti alloy. Chemical composition analysis was performed to determine the contents of vanadium, chromium, and titanium. The results are shown in Table 1.
[0036] Table 1: Percentage of vanadium, chromium, and titanium content at different locations in the V-4Cr-4Ti alloy.
[0037]
[0038]
[0039] In Table 1, the average percentage of chromium content in Example 1 is 4.05%, and the average percentage of chromium content in Example 2 is 4.07%. The chromium content in both examples is close, with no significant difference. However, the variance of the percentage of chromium content in Example 1 is 0.002, compared to 0.018 in Example 2. The variances of elemental chromium and elemental titanium content in Example 1 are on the same order of magnitude, indicating that the chromium content variation at each sampling point in Example 1 is smaller, while the variation is larger in Example 2, suggesting better uniformity of chromium in the alloy of Example 1. The average percentage of titanium content in Example 1 is 4.02%, and the average percentage of titanium content in Example 2 is 4.01%. The titanium content in both examples is close, with no significant difference. Meanwhile, the variance of the percentage of titanium content in Example 1 is 0.002, and the variance is 0.004 in Example 2, indicating small differences in titanium content at each sampling point in both examples.
[0040] The above results demonstrate that the preparation method of V-4Cr-4Ti alloy of the present invention can effectively improve the uniformity of V-4Cr-4Ti alloy, especially the uniformity of chromium in V-4Cr-4Ti alloy, and the prepared V-4Cr-4Ti alloy has better quality.
[0041] It should be noted that there are various methods for preparing consumable electrodes, but Example 2 is already a relatively superior preparation method in the existing technology. Other methods have many problems. For example, preparing consumable electrodes by melting vanadium, chromium, and titanium raw materials is very energy-intensive and is not suitable from a cost perspective. Another example is welding vanadium plates, chromium plates, and titanium plates together to use as consumable electrodes. The internal cavity of existing VAR furnaces is cylindrical, while the welded plates are cubic, making it difficult to place the plates into the VAR furnace and impossible to clamp the plates.
[0042] Besides the VAR furnace method, other methods exist for preparing V-4Cr-4Ti alloys from elemental metals. For example, mixing various metal powders, isostatically pressing them, and then sintering them in a vacuum sintering furnace. This method requires high uniformity in metal mixing and precise particle size control. However, the cost of preparing V-4Cr-4Ti alloys using this invention is lower. Furthermore, the aforementioned methods are essentially solid-to-solid mixtures, while this invention involves liquid-to-liquid mixing, which generally results in better uniformity than solid-to-liquid mixing.
[0043] The above-disclosed embodiments are merely preferred embodiments of the present invention and should not be construed as limiting the scope of the invention. Those skilled in the art will understand that implementing all or part of the above-described embodiments and making equivalent changes in accordance with the claims of the present invention are still within the scope of the invention.
Claims
1. A method for preparing a V-4Cr-4Ti alloy, characterized in that, Includes the following steps: Step S1: Arrange vanadium filaments, sponge titanium, and chromium particles in three layers in a predetermined ratio in a material tank. The vanadium filaments are located in the bottom and top layers, while the titanium and chromium particles are located in the middle layer. The thickness of the vanadium filaments is less than or equal to 1 mm, and the width is 2-3 mm. The particle size of the sponge titanium is 20-50 mm, and the particle size of the chromium particles is 1-6 mm. Step S2: Use a forging press to press the material in the trough into a block mixture, with a pressure greater than or equal to 40MPa; Step S3: Using the block mixture as a consumable electrode, the block mixture is smelted once in a VAR furnace to obtain V-4Cr-4Ti alloy.
2. The method for preparing the V-4Cr-4Ti alloy as described in claim 1, characterized in that: In step S1, the thickness of the vanadium filaments is 0.7 to 1 mm.
3. The method for preparing the V-4Cr-4Ti alloy as described in claim 1, characterized in that: In step S2, the pressing pressure of the block mixture is 40 MPa.
Citation Information
Patent Citations
Vanadium-chromium-titanium alloy and preparation method thereof
CN113481393A
Novel helium ion sputtering-resistant vanadium alloy and preparation method thereof
CN105506428A
High-strength high-toughness vanadium alloy and preparation method thereof
CN106435318A