A stamped and welded bridge shell and its preparation method

By optimizing the steel plate composition and hot stamping process of the bridge shell, the problems of "ear" defects and cracks in the stamping process of the welded bridge shell were solved, and a bridge shell with high strength, high plasticity and low anisotropy was achieved, ensuring stability and reliability during service.

CN118222930BActive Publication Date: 2026-11-17XIANGFAN JINNAITE MACHINERY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410619331.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-19
Publication Date
2026-11-17
Estimated Expiration
2044-05-19

AI Technical Summary

Technical Problem

Existing stamped and welded bridge housings are prone to "ear" defects and cracks during the stamping process, resulting in a high scrap rate and poor stability and reliability during service.

Method used

By optimizing the chemical composition of the bridge shell steel plate and controlling the content and ratio of C, Si, Mn, Ti, V, Nb, Al, and Sn, especially ([Al]/27)/([Sn]/119) within the range of 5.7-13.4, and combining it with hot stamping process, the bridge half shell is prepared and welded into a bridge shell, ensuring low anisotropy and excellent strength and plasticity.

Benefits of technology

The obtained bridge housing has no "ear" defects after stamping and is not easy to crack after stamping. It has extremely high stability and reliability during subsequent service, with a yield strength ≥550MPa, tensile strength ≥720MPa, and elongation ≥18%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This invention relates to a stamped and welded bridge housing, characterized in that the stamped and welded bridge housing is formed by welding two bridge halves, the two bridge halves being prepared by hot stamping of steel plates, wherein the chemical composition of the steel plate, by mass percentage, is: C: 0.14-0.22%, Si: 0.25-0.65%, Mn: 1.55-1.95%, P≤0.01%, S≤0.01%, Ti: 0.03-0.07%, V: 0.04-0.08%, Nb: 0.02-0.045%, Al: 0. 22-0.47%, Sn: 0.08-0.26%, with the balance being Fe and unavoidable impurities, and the contents of Al and Sn satisfy ([Al] / 27) / ([Sn] / 119)=5.7-13.4, where [Al] and [Sn] represent the mass percentage content of Al and Sn, respectively. The CEV of the steel plate is below 0.5, and CEV=[C]+[Mn] / 6+[V] / 5, where [C], [Mn], and [V] represent the mass percentage content of C, Mn, and V, respectively.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a stamped and welded bridge housing and its preparation method. In particular, the stamped and welded bridge housing has excellent strength and plasticity, and there is no "ear" defect after stamping. The risk of cracking during the stamping process and during subsequent service is low, and the service stability and reliability are high. Background Technology

[0002] As a load-bearing and force-transmitting component, the axle housing plays a crucial role in ensuring stable vehicle operation. For a long time, axle housings have primarily been manufactured using casting. While cast axle housings offer high strength, they are heavy, making transportation difficult. Furthermore, the manufacturing process is less environmentally friendly, prone to casting defects, resulting in a high scrap rate and a relatively high failure rate. In recent years, another manufacturing method—stamped axle housings—has gained market share. These are lighter, contributing to vehicle weight reduction, and allow for targeted reinforcement of key load-bearing areas. They also have a lower failure rate, and their manufacturing process is more environmentally friendly than casting. Moreover, with improvements in steel properties, stamped axle housings can achieve the same strength levels as cast axle housings.

[0003] In the long run, whether from the perspective of service reliability, lightweighting, or environmental protection, welded bridge housings are likely to replace cast bridge housings.

[0004] As the name suggests, stamped and welded bridge housings require two basic steps: stamping and welding. In actual production, due to the relatively thick steel plates used for the housings, the anisotropy after rolling during the stamping process easily leads to "earing" defects. More seriously, some steel develops cracks after stamping, resulting in a high scrap rate. Alternatively, some stamped and welded bridge housings, due to significant anisotropy, are prone to cracking during subsequent use, leading to service failure. Currently, to avoid anisotropy, the cold rolling reduction rate is usually increased. However, the steel plates used for stamped and welded bridge housings are usually hot-rolled steel plates without a cold rolling step. Anisotropy cannot be effectively controlled during the steel plate preparation stage, making "earing" defects easy to occur during the stamping process and cracking during subsequent service.

[0005] Therefore, how to obtain a bridge shell without "ear" defects and without cracks by stamping has become an important technical problem in this field. Summary of the Invention

[0006] This invention proposes a stamped and welded bridge housing, which not only has excellent strength and plasticity, but also does not produce "ear" defects after stamping and does not crack after stamping, and has good stability and reliability during later service.

[0007] The technical solution of the present invention is as follows.

[0008] This invention provides a stamped and welded bridge housing, characterized in that the stamped and welded bridge housing is welded from two bridge half-shells, the two bridge half-shells being prepared by hot stamping of steel plates, the chemical composition of the steel plate being, by mass percentage: C: 0.14-0.22%, Si: 0.25-0.65%, Mn: 1.55-1.95%, P≤0.01%, S≤0.01%, Ti: 0.03-0.07%, V: 0.04-0.08%, Nb: 0.02-0.045%, Al: 0. 22-0.47%, Sn: 0.08-0.26%, with the balance being Fe and unavoidable impurities, and the contents of Al and Sn satisfy ([Al] / 27) / ([Sn] / 119)=5.7-13.4, where [Al] and [Sn] represent the mass percentage content of Al and Sn, respectively. The CEV of the steel plate is below 0.5, and CEV=[C]+[Mn] / 6+[V] / 5, where [C], [Mn], and [V] represent the mass percentage content of C, Mn, and V, respectively.

[0009] Below, we will first introduce the design principle of the steel plate composition used to prepare the stamped and welded bridge shell of the present invention.

[0010] C: Carbon plays a solid solution strengthening role, and carbon produces a distribution during hot stamping, which can greatly improve the strength of the bridge shell. However, carbon will cause the weldability of the material to deteriorate. Since stamping and welding of bridge shells are required, the carbon content needs to be determined under the premise of balancing strength and weldability. In this invention, the carbon content is controlled at 0.14-0.22%.

[0011] Si: Similar to carbon, silicon is also an element that improves the strength of steel. However, silicon deteriorates the weldability of the material. Therefore, taking into account both strength and weldability, the silicon content of this invention is controlled at 0.30-0.80%.

[0012] Mn: Similar to carbon and silicon mentioned above, manganese also has the effect of increasing strength and worsening weldability. Therefore, taking into account both strength and weldability, the manganese content of the present invention is controlled at 1.55-1.95%.

[0013] Ti: Titanium combines with carbon to form titanium carbide, which precipitates as micron- and nano-sized particles during rolling and hot stamping, exerting a strong precipitation strengthening effect and significantly improving the strength of the steel. Titanium carbide also acts as a pinning agent, effectively inhibiting grain growth and contributing to increased strength. However, excessive titanium content can lead to excessive precipitates, affecting the plasticity of the steel plate and making it prone to defects such as cracks during stamping. Considering both the strength and plasticity requirements of the steel, the titanium content in this invention is controlled at 0.03-0.07%.

[0014] V: Vanadium reacts with carbon to form vanadium carbide during rolling and hot stamping, thereby strengthening the steel through dispersed precipitation and significantly improving its strength. However, excessive vanadium content can lead to a deterioration in the plasticity and toughness of the steel plate. Considering the strength, plasticity and toughness requirements of the steel, the vanadium content of this invention is controlled at 0.04-0.08%.

[0015] Nb: During rolling and hot stamping, niobium reacts with carbon to form micron- and nano-sized niobium carbides, which precipitate into the steel matrix, thus significantly improving the strength of the steel plate. At the same time, niobium carbides have a pinning effect, which can effectively inhibit grain growth, thereby ensuring that the steel plate has excellent strength properties. However, if the niobium content is too high, the plasticity of the steel plate will decrease sharply. Taking into account the strength and plasticity requirements of steel, the niobium content of this invention is controlled at 0.02-0.045%.

[0016] P and S: Phosphorus and sulfur are both common impurity elements in steel, and their content is related to many factors such as raw material conditions and smelting level. The presence of phosphorus and sulfur will deteriorate the performance of steel. Therefore, it is necessary to control the content of phosphorus and sulfur at the lowest possible level. This invention controls both phosphorus and sulfur to below 0.01%. However, the lower the content of phosphorus and sulfur, the higher the cost. Therefore, it is necessary to set the lower limit of phosphorus and sulfur content based on actual cost. While balancing performance and cost, the lower limit of phosphorus and sulfur content can usually be set at 0.002%.

[0017] Al, Sn, and ([Al] / 27) / ([Sn] / 119): The addition of aluminum is beneficial for refining the grain size of the steel plate and can effectively promote carbon distribution during hot stamping, which is crucial for ensuring the excellent strength and plasticity of the steel plate. This invention controls the aluminum content to be 0.22-0.47%. Tin is also beneficial for grain refinement, thus significantly ensuring the strength and plasticity of the steel plate. This invention controls the tin content to be 0.08-0.26%. If the content of aluminum and tin is too high, the plasticity effect will be insufficient, and if the content of aluminum and tin is too low, the strength cannot be guaranteed. In addition, the inventors have found that when aluminum and tin are controlled within the above content range, and the content relationship between the two is further controlled in a synergistic way, an unexpectedly low anisotropy can be obtained, thereby ensuring that there is no "earing" phenomenon in the steel plate during the stamping process and that it is not easy to crack during the stamping process and subsequent use. Through extensive experimental research and summarization, the inventors discovered that when ([Al] / 27) / ([Sn] / 119) is controlled within the range of 5.7-13.4, the anisotropy of the steel plate is particularly low, and the stamping performance is outstanding within ±0.1, thus giving the steel plate excellent strength, plasticity and anisotropy.

[0018] While the exact mechanism by which the addition of Al and Sn, and the control of their content relationship, achieve low anisotropy is not fully understood, it is speculated that the control of the amount and content of Al and Sn can effectively prevent the formation of columnar crystals, thereby enabling the steel sheet to obtain an equiaxed crystal structure. Therefore, the final material exhibits very low anisotropy, making it particularly suitable for hot stamping forming.

[0019] To ensure excellent weldability, this invention limits the CEV of the steel plate to below 0.5, where CEV = [C] + [Mn] / 6 + [V] / 5, and [C], [Mn], and [V] represent the mass percentages of C, Mn, and V, respectively. The lower the CEV of the steel plate, the better the weldability, and the superior the performance and quality of the final welded bridge housing.

[0020] The steel plate with the above-mentioned chemical composition is hot-stamped to obtain a bridge half-shell, and then two bridge half-shells are welded to obtain the bridge shell of the present invention. As mentioned above, the steel plate used in the stamped and welded bridge shell of the present invention has excellent strength and plasticity characteristics, low anisotropy, and good stamping characteristics. Therefore, it can ultimately ensure that the stamped and welded bridge shell has excellent strength and plasticity, and there are no "ear" defects or stamping cracks, resulting in excellent service reliability and service stability.

[0021] This invention optimizes the composition of the bridge shell steel plate, and obtains high strength, high plasticity, and extremely low anisotropy by controlling the content and ratio of Al and Sn. The steel plate exhibits excellent hot stamping performance. Therefore, the bridge shell prepared by this steel plate does not have the "ear" defect after stamping and is not easy to crack after stamping. It has extremely high stability and reliability in subsequent service.

[0022] The stamped and welded bridge housing of the present invention has excellent strength and plasticity, and there is no "ear" defect after stamping. It does not crack after stamping and has extremely high stability and reliability during subsequent service. As a preferred description, the stamped and welded bridge housing of the present invention has a yield strength ≥550MPa, a tensile strength ≥720MPa, and an elongation ≥18%.

[0023] As a non-limiting description, the thickness of the stamped and welded bridge shell of the present invention can be 10-20mm, and the thickness of the stamped and welded bridge shell is not limited to this. The thickness of the stamped and welded bridge shell can be reasonably selected and determined according to the requirements of the actual application scenario.

[0024] As another objective of the present invention, the present invention also provides a preparation process for the above-mentioned stamped and welded bridge shell, comprising the following steps: S1: melting to obtain the corresponding composition and casting to obtain a slab; S2: homogenizing the slab; S3: hot rolling the homogenized slab; S4: laminar cooling after rolling; S5: air cooling to room temperature after coiling to obtain a hot-rolled plate; S6: heating the hot-rolled plate; S7: hot stamping the heated hot-rolled plate to obtain a bridge half shell; S8: welding the two bridge half shells after the bridge half shells have cooled to obtain a bridge shell.

[0025] Preferably, the homogenization temperature in step S2 is 1200-1280℃, and the homogenization time is 2-5 hours. Suitable homogenization temperature and time have a significant impact on obtaining high-performance steel plates. If the homogenization temperature is too low, sufficient and effective solution cannot be achieved, resulting in decreased strength; if the homogenization temperature is too high, overheating is likely, and significant grain coarsening occurs, leading to insufficient strength; if the homogenization time is too long, the material will also overheat, resulting in grain coarsening and decreased strength; if the homogenization time is too short, sufficient and effective solution cannot be achieved, and sufficient strength cannot be guaranteed.

[0026] As an optional technical solution, the initial rolling temperature of the S3 hot rolling is 950-1000℃, and the final rolling temperature is 850-910℃. A suitable rolling temperature is beneficial for obtaining a good microstructure, thereby further improving the strength and plasticity of the steel plate and reducing anisotropy. If the rolling temperature is too high, the tendency for grain coarsening becomes obvious; if the rolling temperature is too low, the rolling energy consumption is too high and defects such as rolling cracks are easily generated.

[0027] As a further preferred technical solution, the cooling rate of S4 post-rolling laminar flow cooling is controlled at 10-40℃ / s. A suitable cooling rate is beneficial for refining the microstructure and effectively improving the strength, plasticity, and hot stamping forming characteristics of the steel plate.

[0028] As a further preferred technical solution, controlling the winding temperature of S5 within a suitable range is beneficial for obtaining a good balance between strength and plasticity. If the winding temperature is too high, the strength decreases significantly, making it impossible to guarantee the acquisition of high strength characteristics; if the winding temperature is too low, the elongation is insufficient, and the plasticity deteriorates. Therefore, this invention controls the winding temperature at 580-640℃, which is beneficial for obtaining steel plates that combine strength and plasticity.

[0029] As a further preferred technical solution, after S5 is coiled, it is cooled to room temperature to obtain hot-rolled steel sheet, and the cooling method can be air cooling.

[0030] As a further preferred technical solution, the heating temperature of S6 is 720-800℃, and the hot stamping forming temperature of S7 is 700-780℃; the holding time is 0.2-3 minutes. If the heating and stamping temperatures are too high, austenite will grow significantly, reducing the deformation resistance of the steel plate, but also decreasing the plasticity and hot working performance. Furthermore, the austenite structure will coarsen, affecting the structure and properties of the stamped axle half-shell. If the heating and stamping temperatures are too low, the deformation resistance during hot stamping will increase, which is not conducive to the long-term operation of the stamping equipment, and cracking is prone to occur during the stamping process. Holding pressure plays a role in determining the length and shape. If the holding time is too short, springback in size and shape is likely to occur. If the holding time is too long, it is not conducive to improving production efficiency.

[0031] The present invention has the following beneficial effects.

[0032] This invention optimizes the composition of the bridge shell steel plate, and obtains a steel plate with high strength, high plasticity, and extremely low anisotropy by controlling the content and ratio of Al and Sn. The steel plate exhibits excellent hot stamping performance. Therefore, the bridge shell of this invention prepared by this steel plate does not have the "ear" defect after stamping and is not easy to crack after stamping. It has extremely high stability and reliability in subsequent service. Detailed Implementation

[0033] To enable those skilled in the art to fully understand the technical solution and beneficial effects of the present invention, the following detailed explanation is provided in conjunction with specific experimental examples.

[0034] The molten steel was smelted according to the composition in Table 1, with P and S controlled at 0.008% ± 0.001%. The molten steel was then continuously cast to obtain a slab with a thickness of 200 mm and a width of 1000 mm. The slab was subjected to a homogenization heat treatment at 1230℃ for 3.5 h, followed by hot rolling at an initial rolling temperature of 960℃ and a final rolling temperature of 870℃ to obtain a 20 mm thick hot-rolled slab. The hot-rolled slab was then subjected to laminar flow cooling at a cooling rate of 25℃ / s. After cooling to 600℃, the slab was coiled and air-cooled to room temperature. The slab was then heated to 770℃ and held for 5 min before being transferred to a stamping die within 30 s. Hot stamping was performed at 750℃ and held for 90 s. After demolding, the slab was air-cooled to room temperature to obtain a 16 mm thick bridge half-shell. In Table 1, F1 = ([Al] / 27) / ([Sn] / 119) and CEV = [C] + [Mn] / 6 + [V] / 5, where [Al], [Sn], [C], [Mn], and [V] represent the mass percentages of Al, Sn, C, Mn, and V, respectively.

[0035] The dimensions of the bridge half shell were measured to determine whether there was a "ear" defect. Then, magnetic particle testing was performed to determine whether there was a crack. After that, the bridge half shell was cut and its strength and elongation were tested. The elongation, tensile strength and yield strength at room temperature were tested in accordance with GB / T228.1-2021 "Metallic materials - Tensile testing - Part 1: Test method at room temperature" and the test results were recorded in Table 2.

[0036] Table 1 Chemical composition of each bridge half-shell (by mass percentage, balance Fe).

[0037] Table 2 Performance test results of each bridge half-shell.

[0038]

[0039] The following analysis will be conducted in conjunction with Tables 1 and 2.

[0040]

[0041] The bridge half-shells in test numbers 1-6 of Table 1 all meet the composition requirements of this invention. The yield strength, tensile strength, and elongation of the final bridge half-shells all meet the requirements of this invention, exhibiting high strength and high plasticity. The steel plates used to prepare the bridge half-shells in tests 1-6 demonstrate good stamping characteristics. After hot stamping, the bridge half-shells do not exhibit "earing" defects, and magnetic particle testing shows no crack defects after stamping. The composition and properties of the bridge half-shells in tests 1-6 all meet the requirements of this invention; therefore, they are embodiments of this invention.

[0042] In Table 1, at least one of the components of Al, Sn, and ([Al] / 27) / ([Sn] / 119) in the bridge half-shell composition of tests 7-14 does not meet the requirements of this invention. Consequently, at least one of their strength, elongation, "earing" defects, and crack defects fails to meet the requirements of this invention. Therefore, tests 7-14 are all comparative examples of this invention.

[0043] The following is a detailed analysis of each comparative example.

[0044] Comparative Example 7 is a comparative example of Example 1. Under the premise that other components are the same, the Al content was adjusted. The adjusted Al content is still within the range required by this invention, but ([Al] / 27) / ([Sn] / 119) no longer meets the requirements of the invention. The test results in Table 2 confirm that the bridge half-shell has poor hot stamping forming performance, exhibiting an "earing" phenomenon after stamping, and the bridge half-shell has crack defects after stamping, failing to meet the requirements of the invention. Therefore, controlling ([Al] / 27) / ([Sn] / 119) within a suitable range is beneficial for obtaining a hot-stamped bridge half-shell without "earing" defects and without cracks.

[0045] Comparative Example 8 is a comparative example of Example 2. Under the premise that other components are the same, the Sn content was adjusted. The adjusted Sn content is still within the range required by this invention, but ([Al] / 27) / ([Sn] / 119) no longer meets the requirements of the invention. The test results in Table 2 confirm that the bridge half-shell has poor hot stamping forming performance, exhibiting an "earing" phenomenon after stamping, and the bridge half-shell has crack defects after stamping, failing to meet the requirements of the invention. Therefore, controlling ([Al] / 27) / ([Sn] / 119) within a suitable range is beneficial for obtaining a hot-stamped bridge half-shell without "earing" defects and without cracks.

[0046] Comparative Example 9 is a comparative example of Example 3. Under the premise that other components are the same, the Sn content was adjusted. The adjusted Sn content is still within the range required by this invention, but ([Al] / 27) / ([Sn] / 119) no longer meets the requirements of the invention. The test results in Table 2 confirm that the bridge half-shell has poor hot stamping forming performance, exhibiting an "earing" phenomenon after stamping, and the bridge half-shell has crack defects after stamping, failing to meet the requirements of the invention. Therefore, controlling ([Al] / 27) / ([Sn] / 119) within a suitable range is beneficial for obtaining a hot-stamped bridge half-shell without "earing" defects and without cracks.

[0047] Comparative Example 10 is a comparative example of Example 4. Under the premise that other components are the same, the Al content was adjusted. The adjusted Al content is still within the range required by the present invention, but ([Al] / 27) / ([Sn] / 119) no longer meets the requirements of the invention. The test results in Table 2 confirm that the bridge half-shell has poor hot stamping forming performance, exhibiting an "earing" phenomenon after stamping, and the bridge half-shell has crack defects after stamping, failing to meet the requirements of the invention. Therefore, controlling ([Al] / 27) / ([Sn] / 119) within a suitable range is beneficial for obtaining a hot-stamped bridge half-shell without "earing" defects and without cracks.

[0048] Comparative Example 11 is a comparative example of Example 5. With other components remaining the same, the Sn content was adjusted. The adjusted Sn content exceeded the Sn content range required by this invention and no longer met the requirements. The test results in Table 2 confirm that although the yield strength and tensile strength of this bridge half-shell were improved, the elongation decreased and the plasticity deteriorated, failing to meet the requirements of the invention. Therefore, controlling Sn within a suitable range is beneficial for achieving excellent plasticity in the bridge half-shell.

[0049] Comparative Example 12 is a comparative example of Example 6. With other components remaining the same, the Al content was adjusted. The adjusted Al content exceeded the Al content range required by this invention, and therefore no longer met the requirements of the invention. The test results in Table 2 confirm that although the yield strength and tensile strength of this bridge half-shell were improved, the elongation decreased, and the plasticity deteriorated, failing to meet the requirements of the invention. It is evident that controlling Al within a suitable range is beneficial for achieving excellent plasticity in the bridge half-shell.

[0050] Comparative Example 13 is a comparative example of Example 1. With other components remaining the same, the Al content was adjusted. The adjusted Al content is below the Al content range required by this invention and no longer meets the requirements of the invention. The test results in Table 2 confirm that although the elongation of the bridge half-shell was improved, the yield strength and tensile strength decreased, and the strength deteriorated significantly, failing to meet the requirements of the invention. Therefore, controlling Al within a suitable range is beneficial for achieving excellent strength in the bridge half-shell.

[0051] Comparative Example 14 is a comparative example of Example 2. Under the premise that other components are the same, the Sn content was adjusted. The adjusted Sn content is lower than the Sn content range required by this invention, and ([Al] / 27) / ([Sn] / 119) no longer meets the requirements of the invention. The test results in Table 2 confirm that although the elongation of the bridge half-shell is improved, the yield strength and tensile strength decrease, and the strength deteriorates significantly, failing to meet the requirements of the invention. Simultaneously, the hot stamping forming performance of the bridge half-shell is poor, with "earing" defects and cracks appearing after stamping, failing to meet the requirements of the invention. Therefore, controlling Sn within a suitable range is beneficial for obtaining excellent strength in the bridge half-shell, and controlling ([Al] / 27) / ([Sn] / 119) within a suitable range is beneficial for obtaining a hot-stamped bridge half-shell without "earing" defects and without cracks.

[0052] The comparison of the above embodiments and comparative examples clearly demonstrates that the present invention, through optimized formulation of the bridge shell steel plate, and by controlling the Al and Sn contents and their ratios, obtains a steel plate with high strength, high plasticity, and extremely low anisotropy. The steel plate exhibits excellent hot stamping performance. The bridge shell of the present invention prepared from this steel plate does not have "ear" defects after stamping, is not prone to cracking after stamping, and demonstrates extremely high stability and reliability during subsequent service. The above description of the embodiments is only for the purpose of helping to understand the method and core ideas of the present invention. It should be noted that those skilled in the art can make several improvements and modifications to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the protection scope of the claims of the present invention.

[0053] The above description of the disclosed embodiments enables those skilled in the art to make or use the invention. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the invention. Therefore, the invention is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A stamped and welded bridge housing, characterized in that, The welded bridge shell is formed by welding two bridge halves, which are prepared by hot stamping of steel plates. The chemical composition of the steel plate, by mass percentage, is: C: 0.14-0.22%, Si: 0.25-0.65%, Mn: 1.55-1.95%, P≤0.01%, S≤0.01%, Ti: 0.03-0.07%, V: 0.04-0.08%, Nb: 0.02-0.045%, Al: 0.22-0.47%, Sn: 0.08-0.26%, with the balance being Fe and unavoidable impurities. The Sn content satisfies ([Al] / 27) / ([Sn] / 119)=5.7-13.4, where [Al] and [Sn] represent the mass percentages of Al and Sn, respectively. The CEV of the steel plate is below 0.5, and CEV=[C]+[Mn] / 6+[V] / 5, where [C], [Mn], and [V] represent the mass percentages of C, Mn, and V, respectively. The bridge half shell obtained by hot stamping of the steel plate is free from "ear" defects and cracks. The yield strength of the stamped and welded bridge shell is ≥550MPa, the tensile strength is ≥720MPa, and the elongation is ≥18%.

2. The stamped and welded bridge housing according to claim 1, characterized in that, The thickness of the welded bridge shell is 10-20mm.

3. The manufacturing process of the stamped and welded bridge housing according to any one of claims 1-2, characterized in that, Includes the following steps: S1: Melt to obtain the corresponding composition and cast to obtain a slab; S2: Homogenize the slab; S3: Hot rolling of homogenized slabs; S4: Laminar flow cooling after rolling; S5: After coiling, air-cool to room temperature to obtain hot-rolled sheet; S6: Heating the hot-rolled plate; S7: The heated hot-rolled plate is hot-stamped to form a bridge half-shell; S8: After the bridge half-shell has cooled, weld the two bridge half-shells together to obtain the bridge shell.

4. The manufacturing process of the stamped and welded bridge shell according to claim 3, characterized in that, The homogenization temperature in S2 is 1200-1280℃, and the homogenization time is 2-5h.

5. The manufacturing process of the stamped and welded bridge housing according to any one of claims 3-4, characterized in that, The initial rolling temperature of the S3 hot rolling is 950-1000℃, and the final rolling temperature is 850-910℃.

6. The manufacturing process of the stamped and welded bridge housing according to any one of claims 3-4, characterized in that, The post-rolling laminar flow cooling of S4 has a cooling rate of 10-40℃ / s.

7. The manufacturing process of the stamped and welded bridge housing according to any one of claims 3-4, characterized in that, The winding temperature of S5 is 580-640℃.

8. The manufacturing process of the stamped and welded bridge housing according to any one of claims 3-4, characterized in that, The heating temperature of S6 is 720-800℃, the hot stamping forming temperature of S7 is 700-780℃, and the holding time is 0.2-3min.

Citation Information

Patent Citations

  • 700MPa-grade thermal forming axle housing steel and preparation method thereof

    CN112195403A

  • High-strength molten-zinc-plated steel plate excellent in deposit adhesion and suitability for press forming and process for producing the same

    CN1483090A