A method for preparing highly conductive carbon nanotube powder material for smart wearables

By preparing copper-tin-aluminum-doped carbon nanotube powder by counter-spraying at high temperatures, combined with oxygen plasma activation and electroatomized polyaniline treatment, the problems of low conductivity and easy structural damage are solved, and high conductivity and good properties are achieved. Dispersion, suitable for yarn manufacturing of smart wearable devices.

CN118239477BActive Publication Date: 2024-10-11NANTONG JIEJIAN INTELLIGENT DIGITAL TECH CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202410424690.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-10
Publication Date
2024-10-11
Estimated Expiration
2044-04-10

AI Technical Summary

Technical Problem

Existing conductive fibers in flexible smart wearable devices have problems such as low conductivity, easy oxidation, and structural damage. It is difficult to achieve uniform dispersion of carbon nanotube powder in the fibers, limiting their industrial application.

Method used

The copper-tin-aluminum-doped carbon nanotube powder is prepared by spraying gas phase A and gas phase B at high temperature, and is activated by oxygen plasma and treated with electro-atomized polyaniline to form carbon nanotubes with high conductivity and good dispersion. Powder to ensure uniformity of metal composition and avoid agglomeration.

Benefits of technology

The conductive properties and flexibility of carbon nanotubes are improved to form a conductive network, which is suitable for yarn manufacturing of smart wearable devices. The resistivity is significantly reduced without destroying the original structure.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a method for preparing a highly conductive carbon nanotube powder material for smart wear, and relates to the technical field of conductive carbon nanotubes. The present invention adopts the form of airflow spraying to prepare a fine powder of copper-tin-aluminum-doped carbon nanotubes with dot-shaped protrusions on the surface, which improves the conductivity of the carbon nanotubes without destroying the original structure of the carbon nanotubes, and avoids the influence of the later pulverization treatment on the conductivity of the powder. Then, the activated carbon nanotube powder is electro-atomized with an aniline monomer solution to connect the dot-shaped protrusions into crossed or overlapping strip-shaped protrusions, so that even if the carbon nanotube powder is disorderly arranged inside the fiber, the strip-shaped protrusions on the surface of the powder will be in contact, which is more conducive to the formation of a conductive network, and has good dispersibility, overcoming the disadvantage of the carbon nanotubes in the prior art that they are easy to agglomerate in PBT.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of conductive carbon nanotubes, and in particular to a method for preparing a highly conductive carbon nanotube powder material for smart wear. The material can be used as a conductive filler in the spinning of smart wear fabrics. Background Art

[0002] Although there is a huge market demand for flexible smart wearables, the existing conductive fibers still have many shortcomings. Currently, there are two main types of products that can achieve flexible conduction: one is silver-plated / metal alloy yarn; the second is carbon composite fiber yarn. As a traditional conductive fiber, silver-plated yarn has excellent conductive properties, but it is easy to oxidize, has low elasticity, poor skin affinity, hard feel, and is not soft. Carbon composite fiber is the best choice to replace silver-plated materials, but the carbon composite fiber on the market currently has a major disadvantage - the conductivity is too low, basically around 10. 3 -10 4 Ω / cm, for example, the resistivity of Telxin's carbon black conductive yarn is 10 4 Ω / cm, the resistivity of the carbon nanotube yarn of Under Armour sports T-shirt is 2×10 2 -10 3 Ω / cm.

[0003] Carbon nanotubes are a new type of conductive agent that can act as "wires" in conductive networks. However, due to the strong van der Waals forces between carbon nanotubes, they will entangle and aggregate with each other, thus affecting the conductivity of carbon nanotubes. Therefore, how to prepare a conductive carbon nanotube powder and evenly disperse it in fibers is a major obstacle to its industrial application.

[0004] At present, the solution to the carbon nanotube dispersion problem mainly relies on the strong oxidizing acid treatment method. Although carbon nanotubes with good dispersion performance can be obtained, the strong acid will also destroy the structure of the carbon nanotubes and shorten the carbon nanotubes, thereby affecting the conductivity of the carbon nanotubes and the performance of the carbon nanotubes as a conductive agent. Therefore, the present invention prepares a highly conductive carbon nanotube powder material with good dispersibility in fibers. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a highly conductive carbon nanotube powder material for smart wearables, so as to solve the problems existing in the prior art.

[0006] In order to solve the above technical problems, the present invention provides the following technical solution: a highly conductive carbon nanotube powder material for smart wearables, comprising the following preparation steps:

[0007] (1) introducing gas phase A, hydrogen, and argon into the vent, and introducing gas phase B into the nozzle, with the nozzle and the vent being arranged opposite to each other, and simultaneously spraying the gases into the reaction chamber at 1100° C., with the argon flow rate being 300 to 400 sccm, the hydrogen flow rate being 1000 to 1400 sccm, the gas phase A flow rate being 2 to 20 sccm, the gas phase B flow rate being 10 to 35 sccm, and the nozzle pressure being 0.5 to 2 MPa, to obtain copper-tin-aluminum-doped carbon nanotube powder;

[0008] (2) After activation treatment, the copper-tin-aluminum doped carbon nanotube powder is placed in a reactor with a stirring device, and the stirring is turned on. Aniline and sulfuric acid with a mass fraction of 20% are mixed in a ratio of 2g:100mL. After stirring evenly, the mixture is injected into an electrospray device at a rate of 15-30μL / min. The distance between the nozzle of the device and the activated carbon nanotubes is 30-50mm, the applied voltage is 5-15kV, the atomization time is 5-20min, and the mixture is dried to a constant weight to obtain a highly conductive carbon nanotube powder material.

[0009] Furthermore, the gas phase A in step (1) is obtained by mixing a carbon source, a sulfur source, and a nickel source in a molar ratio of 100:0.1-3:0.3-5, stirring and dissolving, and then evaporating and vaporizing.

[0010] Furthermore, the carbon source is one of methanol, benzene or toluene.

[0011] Furthermore, the sulfur source is one of sulfur powder, thiophene or thiourea.

[0012] Furthermore, the nickel source is nickelocene.

[0013] Furthermore, the preparation method of the gas phase B in step (1) is as follows: after stirring and dissolving stannous chloride and 12 mol / L hydrochloric acid in a ratio of 0.5 g:2.5 mL, water is added to a stannous chloride concentration of 0.1 mol / L, and then 0.5 to 1.2 times the mass of stannous chloride and 0.1 to 0.9 times the mass of stannous chloride are added. After stirring and dissolving, the mixture is evaporated and vaporized.

[0014] Furthermore, the activation treatment in step (2) is as follows: placing the copper-tin-aluminum doped carbon nanotube powder in a plasma reaction chamber and evacuating the chamber to a vacuum of 2.0×10 -4 ~5.0×10 -4 After Pa, argon gas was introduced at a rate of 15-30 mL / min for 20-25 min, and discharge treatment was performed for 8-13 min at an oxygen flow rate of 15-30 mL / min and a power of 70 W.

[0015] Furthermore, the stirring speed in step (2) is 60 to 100 rpm.

[0016] Furthermore, the drying temperature in step (2) is 80°C.

[0017] Furthermore, the highly conductive carbon nanotube powder material can be used in the manufacture of PBT yarn for smart wearable devices.

[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:

[0019] The present invention selects gaseous carbon source, nickel source and sulfur source as gas phase A, gaseous copper source, tin source and aluminum source as gas phase B, and sprays the two gas phases with high-temperature airflow in a closed space. The gaseous nickel source and carbon source can catalyze and induce carbon atoms to grow into carbon nanotubes, while the gaseous copper source, tin source and aluminum source are transformed into metal copper, tin, aluminum and three-phase alloy at high temperature, and are assembled with carbon nanotubes to obtain copper-tin-aluminum-doped carbon nanotubes. In addition, during the preparation process, a gas phase B with a relatively high gas flow rate and pressurized gas phase B is selected to drive the carbon source gas to flow rapidly, so that some metal element atoms cannot participate in the joint assembly in time, thereby carbon nanotubes are The nanotube wall is doped with a small amount of copper, tin, and aluminum, which improves the conductivity without destroying the original structure of the carbon nanotube. The copper, tin, and aluminum on the tube wall can serve as a seed layer, and some metal elements that fail to participate are transformed into metal particles. With the movement of airflow and high temperature, they adhere to the surface of the carbon nanotube to form a dot-like protrusion structure. The present invention adopts gas phase mixing to ensure the uniformity of the metal component and avoid the agglomeration of metal elements in the carbon nanotube in the prior art. The airflow sprays against each other to create particle collision and form a grinding effect, so that the product is directly in the form of metal-carbon nanotube powder, which can reduce the influence of subsequent crushing treatment on conductivity.

[0020] The present invention activates copper, tin and aluminum doped carbon nanotube powder with oxygen plasma, then electro-atomizes aniline monomer solution toward the surface of the carbon nanotube, regulates voltage, polymerizes and deposits a small amount of polyaniline on the surface of the carbon nanotube, and connects the dot-shaped protrusions on the surface of the carbon nanotube to form crossed or overlapping strip-shaped protrusions, so that even if the carbon nanotube powder is disorderly arranged inside the fiber, the strip-shaped protrusions on the surface of the powder will be in contact with each other, which is more conducive to the formation of a conductive network. The presence of polyaniline overcomes the disadvantage of the prior art that carbon nanotubes are easy to agglomerate in PBT. At the same time, the carbon nanotube powder prepared by the present invention has good flexibility, can be bent and folded arbitrarily, and can be used in the manufacture of yarn for smart wear. DETAILED DESCRIPTION

[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] (1) Benzene, sulfur powder and nickelocene are mixed in a molar ratio of 100:0.1:1.8, stirred and dissolved, and evaporated to obtain gas phase A; stannous chloride and 12 mol / L hydrochloric acid are stirred and dissolved in a ratio of 0.5 g:2.5 mL, water is added to a stannous chloride concentration of 0.1 mol / L, and then copper chloride of 1 times the mass of the stannous chloride and aluminum chloride of 0.1 times the mass of the stannous chloride are added, stirred and dissolved, and evaporated to obtain gas phase B; gas phase A, hydrogen and argon are introduced into a vent, gas phase B is introduced into a nozzle, the nozzle and the vent are arranged oppositely, and gases are sprayed into a reaction chamber at 1100° C. at the same time, the argon flow rate is 300 sccm, the hydrogen flow rate is 1000 sccm, the gas phase A flow rate is 2 sccm, the gas phase B flow rate is 10 sccm, and the nozzle pressure is 0.5 MPa, thereby obtaining carbon nanotube powder doped with copper, tin and aluminum;

[0024] (2) Place the copper, tin, and aluminum-doped carbon nanotube powder in a plasma reaction chamber and evacuate the chamber to a vacuum of 2.0×10 -4 After Pa, argon was introduced at 15 mL / min for 25 min, and the discharge treatment was performed for 13 min at an oxygen flow rate of 15 mL / min and a power of 70 W to obtain activated carbon nanotubes;

[0025] (3) The activated carbon nanotubes were placed in a reactor with a stirring device, and the stirring was turned on at a speed of 60 rpm. Aniline and 20% sulfuric acid were mixed in a ratio of 2 g: 100 mL. After stirring evenly, the mixture was injected into an electrospray device at a rate of 15 μL / min. The distance between the nozzle of the device and the activated carbon nanotubes was 30 mm. The applied voltage was 5 kV. The atomization time was 18 min. The mixture was dried at 80°C until constant weight was obtained to obtain a highly conductive carbon nanotube powder material.

[0026] (4) Highly conductive carbon nanotube powder material and PBT are melt-spun, with the carbon nanotube powder accounting for 20% of the fiber mass and the resistance being 15Ω / cm.

[0027] Example 2

[0028] (1) Toluene, thiophene and nickelocene were mixed in a molar ratio of 100:1.8:2.1, stirred and dissolved, and evaporated to obtain gas phase A; stannous chloride and 12 mol / L hydrochloric acid were stirred and dissolved in a ratio of 0.5 g:2.5 mL, water was added to a stannous chloride concentration of 0.1 mol / L, and then copper chloride with a mass of 1.2 times that of the stannous chloride and aluminum chloride with a mass of 0.4 times that of the stannous chloride were added, stirred and dissolved, and evaporated to obtain gas phase B; gas phase A, hydrogen and argon were introduced into a vent, gas phase B was introduced into a nozzle, the nozzle and the vent were arranged opposite each other, and gases were sprayed into a reaction chamber at 1100° C. at the same time, the argon flow rate was 350 sccm, the hydrogen flow rate was 1200 sccm, the gas phase A flow rate was 10 sccm, the gas phase B flow rate was 30 sccm, and the nozzle pressure was 1.1 MPa, thereby obtaining carbon nanotube powder doped with copper, tin and aluminum;

[0029] (2) Place the copper, tin, and aluminum-doped carbon nanotube powder in a plasma reaction chamber and evacuate the chamber to a vacuum of 2.0×10 -4 After Pa, argon gas was introduced at 20 mL / min for 22 min, and the discharge treatment was performed for 10 min at an oxygen flow rate of 20 mL / min and a power of 70 W to obtain activated carbon nanotubes;

[0030] (3) placing the activated carbon nanotubes in a reactor with a stirring device, starting stirring at a speed of 80 rpm, mixing aniline and 20% sulfuric acid in a ratio of 2 g:100 mL, stirring evenly, and injecting into an electrospray device at a rate of 20 μL / min, with the nozzle of the device at a distance of 40 mm from the activated carbon nanotubes, applying a voltage of 10 kV, and atomizing for 15 min. Drying at 80°C to a constant weight to obtain a highly conductive carbon nanotube powder material;

[0031] (4) Highly conductive carbon nanotube powder material and PBT are melt-spun, with the carbon nanotube powder accounting for 20% of the fiber mass and the resistance being 10Ω / cm.

[0032] Example 3

[0033] (1) Toluene, thiourea and nickelocene are mixed in a molar ratio of 100:1.6:3.6, stirred and dissolved, and evaporated to obtain gas phase A; stannous chloride and 12 mol / L hydrochloric acid are stirred and dissolved in a ratio of 0.5 g:2.5 mL, water is added to a stannous chloride concentration of 0.1 mol / L, and then copper chloride with a mass of 1.2 times that of the stannous chloride and aluminum chloride with a mass of 0.9 times that of the stannous chloride are added, stirred and dissolved, and evaporated to obtain gas phase B; gas phase A, hydrogen and argon are introduced into a vent, gas phase B is introduced into a nozzle, the nozzle and the vent are arranged oppositely, and gases are sprayed into a reaction chamber at 1100° C. at the same time, the argon flow rate is 400 sccm, the hydrogen flow rate is 1400 sccm, the gas phase A flow rate is 20 sccm, the gas phase B flow rate is 35 sccm, and the nozzle pressure is 2 MPa, thereby obtaining carbon nanotube powder doped with copper, tin and aluminum;

[0034] (2) Place the copper, tin, and aluminum-doped carbon nanotube powder in a plasma reaction chamber and evacuate the chamber to a vacuum of 5.0×10 -4 After Pa, argon was introduced at 30 mL / min for 20 min, and the discharge treatment was performed at an oxygen flow rate of 30 mL / min and a power of 70 W for 8 min to obtain activated carbon nanotubes;

[0035] (3) placing the activated carbon nanotubes in a reactor with a stirring device, starting stirring at a speed of 100 rpm, mixing aniline and 20% sulfuric acid in a ratio of 2 g: 100 mL, stirring evenly, and injecting into an electrospray device at a rate of 30 μL / min, with the nozzle of the device at a distance of 50 mm from the activated carbon nanotubes, applying a voltage of 15 kV, and atomizing for 8 min, and drying at 80°C until constant weight to obtain a highly conductive carbon nanotube powder material;

[0036] (4) Highly conductive carbon nanotube powder material and PBT are melt-spun, with the carbon nanotube powder accounting for 20% of the fiber mass and the resistance being 15Ω / cm.

[0037] Comparative Example 1

[0038] The difference between Comparative Example 1 and Example 2 is that step (1) is different. Step (1) is changed to: carbon nanotubes, stannous chloride, cupric chloride and aluminum chloride are mixed in a mass ratio of 100:1:1.2:0.4, calcined at 1000°C for 1h, and ground to obtain copper-tin-aluminum-doped carbon nanotube powder; the remaining steps are the same as Example 2.

[0039] The highly conductive carbon nanotube powder material is melt-spun with PBT. The carbon nanotube powder accounts for 20% of the fiber mass and the resistance is 2×10 2 Ω / cm.

[0040] Comparative Example 2

[0041] The difference between Comparative Example 2 and Example 2 is that step (1) is different, and step (1) is changed to: toluene, thiophene, and nickelocene are mixed in a molar ratio of 100:1.8:2.1, stirred to dissolve, and evaporated to obtain gas phase A; stannous chloride and 12 mol / L hydrochloric acid are stirred to dissolve in a ratio of 0.5 g:2.5 mL, water is added to a stannous chloride concentration of 0.1 mol / L, and then 1.2 times the mass of stannous chloride and 0.4 times the mass of stannous chloride are added. Aluminum chloride is stirred and dissolved, and then evaporated to obtain gas phase B; gas phase A, hydrogen and argon are introduced into the vent, and gas phase B is introduced into the nozzle. The nozzle and the vent are arranged opposite to each other, and the gas is sprayed into the reaction chamber at 1100°C at the same time. The argon flow rate is 350sccm, the hydrogen flow rate is 1200sccm, the gas phase A flow rate is 10sccm, the gas phase B flow rate is 5sccm, and the nozzle pressure is 1.1MPa to obtain copper-tin-aluminum-doped carbon nanotube powder; the remaining steps are the same as those in Example 2.

[0042] Highly conductive carbon nanotube powder material and PBT are melt-spun, with the carbon nanotube powder accounting for 20% of the fiber mass and the resistance being 50Ω / cm.

[0043] Comparative Example 3

[0044] The difference between Comparative Example 3 and Example 2 is that step (1) is changed to: toluene, thiophene and nickelocene are mixed in a molar ratio of 100:1.8:2.1, stirred and dissolved, and evaporated to obtain gas phase A; stannous chloride and 12 mol / L hydrochloric acid are stirred and dissolved in a ratio of 0.5 g:2.5 mL, water is added to a stannous chloride concentration of 0.1 mol / L, and then copper chloride with a mass of 1.2 times that of stannous chloride and 0.4 times that of stannous chloride are added. Aluminum chloride is stirred and dissolved, and then evaporated to obtain gas phase B; gas phase A, hydrogen and argon are introduced into the vent, and gas phase B is introduced into the nozzle. The nozzle and the vent are arranged opposite to each other, and the gas is sprayed into the reaction chamber at 1100°C at the same time. The argon flow rate is 350sccm, the hydrogen flow rate is 1200sccm, the gas phase A flow rate is 10sccm, the gas phase B flow rate is 40sccm, and the nozzle pressure is 1.1MPa to obtain copper, tin and aluminum doped carbon nanotube powder; the remaining steps are the same as those in Example 2.

[0045] The highly conductive carbon nanotube powder material is melt-spun with PBT, and the carbon nanotube powder accounts for 20% of the fiber mass, with a resistance of 10 2 Ω / cm.

[0046] Comparative Example 4

[0047] The difference between Comparative Example 4 and Example 2 is that step (1) is different, and step (1) is changed to: toluene, thiophene, and nickelocene are mixed in a molar ratio of 100:1.8:2.1, stirred and dissolved, and evaporated to obtain gas phase A; stannous chloride and 12 mol / L hydrochloric acid are stirred and dissolved in a ratio of 0.5 g:2.5 mL, water is added to a stannous chloride concentration of 0.1 mol / L, and then copper chloride (1.2 times the mass of stannous chloride) and stannous chloride (0.05 times the mass of stannous chloride) are added. .4 times of aluminum chloride is stirred and dissolved, and then evaporated to obtain gas phase B; gas phase A, hydrogen and argon are introduced into the vent, gas phase B is introduced into another vent, the two vents are arranged opposite to each other, and gases are sprayed into the reaction chamber at 1100°C at the same time, with the argon flow rate of 350sccm, the hydrogen flow rate of 1200sccm, the gas phase A flow rate of 10sccm, and the gas phase B flow rate of 30sccm to obtain copper, tin and aluminum doped carbon nanotube powder; the remaining steps are the same as those in Example 2.

[0048] Highly conductive carbon nanotube powder material and PBT are melt-spun, with the carbon nanotube powder accounting for 20% of the fiber mass and the resistance being 20Ω / cm.

[0049] Comparative Example 5

[0050] The difference between Comparative Example 5 and Example 2 is that there is no step (2), and step (3) is changed to: placing the copper, tin and aluminum doped carbon nanotube powder in a reactor with a stirring device, turning on the stirring, the stirring speed is 80 rpm, aniline and 20% sulfuric acid with a mass fraction are mixed in a ratio of 2g:100mL, after stirring evenly, injected into the electrospray device at 20μL / min, the distance between the nozzle of the device and the activated carbon nanotubes is 40mm, the applied voltage is 10kV, the atomization time is 15min, and drying at 80°C to constant weight to obtain a highly conductive carbon nanotube powder material; the remaining steps are the same as Example 2.

[0051] The highly conductive carbon nanotube powder material was melt-spun with PBT. The carbon nanotube powder accounted for 20% of the fiber mass and the resistance was 3×10 2 Ω / cm.

[0052] Comparative Example 6

[0053] The difference between Comparative Example 6 and Example 2 is that there is no step (3), and the remaining steps are the same as Example 2.

[0054] Highly conductive carbon nanotube powder material and PBT are melt-spun, with the carbon nanotube powder accounting for 20% of the fiber mass and the resistance being 40Ω / cm.

[0055] The carbon nanotube powder prepared by the present invention has high conductivity and good dispersibility inside the fiber, thereby being able to form a conductive network inside the fiber, further enhancing the conductivity of the fiber. The carbon nanotube powder prepared by the present invention can give the fiber good flexibility, can be bent and folded arbitrarily, and can be used in the manufacture of yarn for smart wearables.

[0056] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.

Claims

1. A highly conductive carbon nanotube powder material for smart wearables, It is characterized in that The method comprises the following preparation steps: (1) Passing gas phase A, hydrogen and argon into the vent, passing gas phase B into the nozzle, the nozzle and the vent are arranged opposite to each other, and simultaneously spraying the gases into the reaction chamber at 1100° C., the argon flow rate is 300-400 sccm, the hydrogen flow rate is 1000-1400 sccm, the gas phase A flow rate is 2-20 sccm, the gas phase B flow rate is 10-35 sccm, and the nozzle pressure is 0.5-2 MPa to prepare copper-tin-aluminum doped carbon nanotube powder; the gas phase A is composed of a carbon source , sulfur source, and nickel source are mixed in a molar ratio of 100:0.1~3:0.3~5, stirred to dissolve, and then evaporated to obtain; the preparation method of the gas phase B is: stannous chloride and 12mol / L hydrochloric acid are stirred to dissolve in a ratio of 0.5g:2.5mL, water is added to the concentration of stannous chloride to be 0.1mol / L, and then 0.5~1.2 times the mass of stannous chloride and 0.1~0.9 times the mass of aluminum chloride are added, stirred to dissolve, and then evaporated; (2) Place the copper, tin, and aluminum-doped carbon nanotube powder in a plasma reaction chamber and evacuate the chamber to a pressure of 2.0×10 -4 ~5.0×10 -4 Pa, introduce argon at 15-30 mL / min for 20-25 min, discharge for 8-13 min at an oxygen flow rate of 15-30 mL / min and a power of 70 W to obtain activated carbon nanotubes, place them in a reactor with a stirring device, start stirring, mix aniline and 20% sulfuric acid in a ratio of 2g:100 mL, stir evenly, inject into an electrospray device at 15-30 μL / min, the distance between the nozzle of the device and the activated carbon nanotubes is 30-50 mm, the applied voltage is 5-15 kV, the atomization time is 5-20 min, and dry to constant weight to obtain a highly conductive carbon nanotube powder material.

2. The highly conductive carbon nanotube powder material for smart wearable according to claim 1, It is characterized in that The carbon source in step (1) is one of methanol, benzene or toluene.

3. The highly conductive carbon nanotube powder material for smart wearable according to claim 1, It is characterized in that The sulfur source in step (1) is one of sulfur powder, thiophene or thiourea.

4. The highly conductive carbon nanotube powder material for smart wearable according to claim 1, It is characterized in that The nickel source in step (1) is nickelocene.

5. The highly conductive carbon nanotube powder material for smart wearable according to claim 1, It is characterized in that The stirring speed in step (2) is 60-100 rpm.

6. The highly conductive carbon nanotube powder material for smart wearable according to claim 1, It is characterized in that The drying temperature in step (2) is 80°C.

7. The highly conductive carbon nanotube powder material for smart wearable according to claim 1, It is characterized in that The highly conductive carbon nanotube powder material can be used in the manufacture of PBT yarn for smart wearable devices.

Citation Information

Patent Citations

  • Preparation method of carbon nano tube reinforced Al-Cu alloy based composite material

    CN104141062A

  • Foam metal-carbon nanotube composite material, and preparation method and application thereof

    CN104868134A

  • Aluminum / copper / CNTs-tin / graphite multilayer-structured lithium ion battery negative electrode material and preparation method therefor

    CN105609729A

  • Method for preparing carbon-nanotube composite powder material

    CN107096535A

  • Graphene carbon nano tube hybrid reinforced aluminum bearing material and preparation method thereof

    CN110331307A