An isolated mineral insulated fireproof cable material and a preparation method thereof

By adding ingredients such as cobalt-doped magnesium hydroxide to mineral insulated fireproof cable materials, the flame retardant properties of silicone rubber are improved, solving the problems of complex preparation and high cost of existing cable materials, and achieving efficient flame retardant properties and power supply. Time extension.

CN118240379BActive Publication Date: 2024-10-11SHENZHEN LILUTONG TECH IND
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410335291.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-22
Publication Date
2024-10-11
Estimated Expiration
2044-03-22

AI Technical Summary

Technical Problem

The preparation method of existing mineral insulated fireproof cable materials is cumbersome and costly, and the insulation material has a single component, which affects its fire resistance and electrical properties.

Method used

Silicone rubber is used as the matrix, cobalt-doped magnesium hydroxide, hydroxyapatite, kaolin, zinc borate and fillers are added, and cobalt-doped magnesium hydroxide and vulcanizing agent are prepared by hydrothermal treatment to form an isolation mineral with high flame retardant properties. Insulated fireproof cable material.

Benefits of technology

It improves the power supply time and flame retardant performance of cable materials at flame temperature, reduces the expansion rate, simplifies material distribution, and reduces raw material costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118240379B_ABST
    Figure CN118240379B_ABST
Patent Text Reader

Abstract

The present invention discloses an isolated mineral insulated fireproof cable material and a preparation method thereof, wherein the fireproof cable material comprises, by mass, 90 to 120 parts of silicone rubber, 15 to 25 parts of cobalt-doped magnesium hydroxide, 5 to 10 parts of hydroxyapatite, 5 to 15 parts of kaolin, 2 to 5 parts of zinc borate, 10 to 20 parts of filler, and 1 to 3 parts of vulcanizing agent. The fireproof cable material of the present invention expands less when burned, and the dense carbonized layer and hard ceramic matrix produced during burning can support the unburned part, thereby improving the flame retardant properties of the cable material. In addition, the fireproof cable material of the present invention is assembled into a cable, and the power supply time is as high as 180 minutes or more at a flame temperature of 1000°C, and even after aging treatment, a relatively high power supply time can still be maintained. Overall, the cable material of the present invention has a simple distribution, and the raw materials are cheap and easy to obtain, and has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fireproof cables, and in particular to an isolated mineral insulated fireproof cable material and a preparation method thereof. Background Art

[0002] As people's reliance on the power system increases with the acceleration of urban development, power cables are widely used in the construction of industrialization, urbanization and informatization. However, frequent fires have caused significant losses to people's personal safety and property. The key to reducing fire losses is to slow down the spread of flames while ensuring the smooth flow of power, communication lines and escape routes. With the increasing awareness of people's safety in production and life, fire-resistant cables have gradually become a hot topic of research.

[0003] Mineral insulated fireproof cable is a new type of environmentally friendly cable with excellent fireproof and fire-resistant performance. It has been widely used in power supply systems in recent years. At present, the product structure, process and component materials of mineral insulated cables on the market are relatively fixed. Among them, the selection of insulating materials in fireproof cables directly affects the fire resistance and electrical performance of fireproof cables. Therefore, it is necessary to improve the materials of mineral insulated fireproof cables to improve the performance of fireproof cables. There are also some technologies that provide excellent mineral insulated fireproof cable materials. For example, CN114672123A discloses a protective low-smoke halogen-free flame-retardant cable material, which includes the following components by weight: 60-80 parts of olefin copolymer, 24-28 parts of flame-retardant whiskers, 0.2-0.4 parts of antioxidants, 0.8-1.2 parts of lubricants, 8-10 parts of fillers, and 20-24 parts of silicone rubber. The flame-retardant whiskers are made by hydrothermal reaction of a mixture of mineral leachate, aluminosilicate powder and inorganic alkali. The raw materials for preparing the mineral leachate include red mud, dolomite, acidifier and leaching aid; the leaching aid is persulfate; the filler in the cable material formula is phosphogypsum. When this cable material is burned, the expansion pressure brought by water vapor is relatively low, and the unburned part is supported by the carbonized film and ceramic matrix produced during burning, thereby improving the flame retardant performance of the cable material. However, the flame-retardant whiskers of this cable material require hydrothermal preparation and the preparation of mineral leaching solution is also cumbersome, which limits its industrial production.

[0004] In view of the current problems of single insulation material components, complicated preparation methods and high costs of fire-resistant cables, it is necessary to make corresponding improvements. Summary of the invention

[0005] In order to solve the technical problems existing in the prior art, the present invention provides an isolated mineral insulated fire-resistant cable material, which includes, by mass, 90 to 120 parts of silicone rubber, 15 to 25 parts of cobalt-doped magnesium hydroxide, 5 to 10 parts of hydroxyapatite, 5 to 15 parts of kaolin, 2 to 5 parts of zinc borate, 10 to 20 parts of filler, and 1 to 3 parts of vulcanizing agent.

[0006] The present invention uses silicone rubber as the base of the cable material. Silicone rubber is a straight-chain polysiloxane composed of Si-O-Si bonds. Since it has a silicon-oxygen bond as the main chain, silicone rubber has both organic and inorganic characteristics. The residue after burning will form a ceramic-like material mainly composed of silicon-carbon compounds, which can isolate flames. Therefore, it has better applicability in the field of fire prevention than other rubber materials. However, the interaction force between silicone rubber raw rubber molecules is weak, the molecular chain is extremely unstable, and it is also a flammable substance. In addition, although SiO2 produced after the combustion of silicone rubber can play the role of an insulating layer, it is not strong enough to form a dense porcelain protective layer. Therefore, it is necessary to add reinforcing fillers and other additives to increase the strength and density of the porcelain layer. The present invention uses cobalt-doped magnesium hydroxide, hydroxyapatite and kaolin as flame retardants added to the silicone rubber matrix, calcium carbonate and hydrophobic white carbon black as fillers, and zinc borate as a flux.

[0007] Magnesium hydroxide has been widely used in fireproof cable materials as a clean and non-toxic smoke suppressant, but the conventional addition amount of magnesium hydroxide basically needs to be equal to the matrix, which affects the strength of silicone rubber. Therefore, the present invention first grinds the precursor magnesium oxide through ball milling, then hydrothermally reacts in a weakly alkaline environment provided by sodium acetate, and hydrothermally prepares magnesium hydroxide in a dissolution-crystallization manner under high temperature and high pressure conditions provided by hydrothermal. Cobalt can capture free radicals produced by combustion due to its variable valence, inhibiting the combustion process and the generation of combustible gases. However, the introduction of cobalt will cause partial agglomeration of magnesium hydroxide, reduce its compatibility with silicone rubber, increase the expansion rate after combustion, and reduce the mechanical strength of the combustion products. Therefore, the present invention also introduces sodium benzoate to improve the morphology of cobalt-doped magnesium hydroxide.

[0008] Hydroxyapatite, also known as hydroxyapatite and basic calcium phosphate, is a natural mineralization of calcium apatite (Ca5(PO4)3(OH)) and has the advantages of high biocompatibility, activity, and high heat resistance.

[0009] Kaolin, also known as dolomite or attapulgite, is a natural clay mineral composed of aluminum silicate with a crystal chemical formula of 2SiO2·Al2O3·2H2O.

[0010] Zinc borate is an environmentally friendly non-halogen flame retardant with the characteristics of non-toxicity, low water solubility, high thermal stability, small particle size, low specific gravity, good dispersibility, etc. It has multiple functions such as flame retardancy, carbonization, smoke suppression, smoldering suppression and prevention of molten droplets. Zinc borate can be used as a flux. The silicon dioxide produced by the thermal decomposition of silicone rubber at high temperature reacts with the decomposition products of zinc borate to form a glass phase to promote the ceramicization of silicone rubber.

[0011] Furthermore, the preparation method of cobalt-doped magnesium hydroxide comprises:

[0012] The magnesium oxide coarse material is wet ball-milled to collect the refined magnesium oxide;

[0013] The refined magnesium oxide is dispersed in a sodium acetate aqueous solution, and then a water-soluble cobalt salt is added and mixed for hydrothermal reaction to obtain cobalt-doped magnesium hydroxide.

[0014] Furthermore, the mass of the water-soluble cobalt salt is 0.05 to 0.1 times that of the refined magnesium oxide;

[0015] After adding the water-soluble cobalt salt, sodium benzoate in an amount of 0.1 to 0.5 times the mass of the water-soluble cobalt salt is also added.

[0016] Furthermore, the particle size of the refined magnesium oxide is 1 to 5 μm.

[0017] Furthermore, the concentration of the sodium acetate aqueous solution is 1 to 3 mol / L;

[0018] The ratio of the refined magnesium oxide to the sodium acetate aqueous solution is 10-30:100-150 g / mL.

[0019] Furthermore, the hydrothermal reaction is continued at 160-200° C. for 3-8 hours.

[0020] Furthermore, the silicone rubber is at least one of methyl silicone rubber, methyl vinyl silicone rubber, and trimethylsiloxymethyl silicone rubber.

[0021] Furthermore, the filler is obtained by mixing calcium carbonate and hydrophobic white carbon black in a mass ratio of 2-5:1-3.

[0022] The vulcanizing agent used in the present invention is a common vulcanizing agent, and illustratively may be at least one of benzoyl peroxide, tert-butyl perbenzoate, di-tert-butyl peroxide, bis(2,4-dimethylbenzene), bis(2,5-dimethylbenzene) and the like.

[0023] The present invention also provides a method for preparing the above-mentioned isolated mineral insulated fireproof cable material, comprising:

[0024] The silicone rubber, cobalt-doped magnesium hydroxide, hydroxyapatite, kaolin, zinc borate and filler are mixed to obtain a rubber compound, and then the rubber compound is thinned to obtain a blank;

[0025] The blank is mixed with a vulcanizing agent, vulcanized, and extruded to obtain an isolated mineral insulated fireproof cable material.

[0026] The present invention also provides a fireproof cable, comprising the above-mentioned isolated mineral insulated fireproof cable material.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The fireproof cable material of the present invention expands less when burned, and the dense carbonized layer and hard ceramic matrix produced during burning can support the unburned part, thereby improving the flame retardant performance of the cable material. In addition, the fireproof cable material of the present invention is assembled into a cable, and the power supply time is as high as more than 180 minutes at a flame temperature of 1000°C, and even after aging treatment, the power supply time can still be maintained at a high level. Overall, the cable material of the present invention has a simple distribution, and the raw materials are cheap and easy to obtain, and has a good application prospect. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 This is a scanning electron microscope image of cobalt-doped magnesium hydroxide in Example 1 of the present invention;

[0030] Figure 2 is a scanning electron microscope image of cobalt-doped magnesium hydroxide in Example 2 of the present invention;

[0031] Figure 3 This is a scanning electron microscope image of magnesium hydroxide in Comparative Example 1 of the present invention;

[0032] Figure 4 This is a scanning electron microscope image of the cable material of Example 1 after burning;

[0033] Figure 5 This is a scanning electron microscope image of the cable material of Example 2 after burning;

[0034] Figure 6 This is a scanning electron microscope image of the cable material of Comparative Example 1 after burning;

[0035] Figure 7 This is a scanning electron microscope image of the cable material of Comparative Example 2 after burning;

[0036] Figure 8 This is a scanning electron microscope image of the cable material of Comparative Example 3 after burning;

[0037] Fig. 9 A schematic diagram of the structure of the assembled cable is shown. DETAILED DESCRIPTION

[0038] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0039] Introduction of some raw materials used in the embodiments of the present invention:

[0040] Methyl vinyl silicone rubber, model DY-V110-2, purchased from Shandong Dayi Chemical Co., Ltd.;

[0041] Magnesium oxide, model TDNH, was purchased from Haicheng Taiding Huaxin Mineral Products Processing Co., Ltd.;

[0042] Hydroxyapatite, model HH8001VAZMJF, was purchased from Wuhan Shuer Biotechnology Co., Ltd.;

[0043] Kaolin, model SX 68A, was purchased from Shanghai Kaiyin Chemical Co., Ltd.;

[0044] Hydrophobic silica, model H2000, was purchased from Shijiazhuang Huijin Mineral Products Co., Ltd.

[0045] Other raw materials not mentioned are common raw materials. The above content is only to help illustrate the present invention and shall not be construed as a strict limitation of the present invention. Those skilled in the art can directly purchase the same / similar raw materials from the market or prepare them by themselves. These contents will not be repeated in the examples.

[0046] The following will be combined with the specific embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] Example 1

[0048] A method for preparing an isolated mineral insulated fireproof cable material, comprising the following steps:

[0049] Step 1, weighing 10kg methyl vinyl silicone rubber, 2kg cobalt-doped magnesium hydroxide, 0.5kg hydroxyapatite, 1kg kaolin, 0.3kg zinc borate, 0.9kg calcium carbonate, 0.6kg hydrophobic white carbon black, and 0.2kg di-2-4;

[0050] Step 2, adding methyl vinyl silicone rubber, cobalt-doped magnesium hydroxide, hydroxyapatite, kaolin, zinc borate, calcium carbonate, and hydrophobic white carbon black into a mixer for mixing to obtain a rubber material, and then thinning the rubber material to obtain a blank;

[0051] Step 3: feeding the obtained blank into a vulcanizer, then adding double 24 and mixing, vulcanizing, and extruding to obtain an isolated mineral insulated fireproof cable material.

[0052] The preparation method of cobalt-doped magnesium hydroxide is as follows:

[0053] S1, placing 20g of magnesium oxide and 100g of 50% by volume ethanol aqueous solution in a ball mill at a speed of 300rpm for ball milling, and then placing the slurry in a constant temperature oven at 100°C to dry to obtain refined magnesium oxide with an average particle size of 3μm;

[0054] S2. 20 g of refined magnesium oxide was stirred at a speed of 350 rpm for 10 min, dispersed in 120 mL of a 2 mol / L sodium acetate aqueous solution, and then 1 g of cobalt nitrate hexahydrate was added and stirred for 15 min. The mixture was then kept at 180 ° C for 5 h for hydrothermal reaction. After natural cooling, the mixture was taken out, the insoluble matter was collected by filtration, washed three times with water and ethanol respectively, and finally dried in a constant temperature oven at 120 ° C to obtain cobalt-doped magnesium hydroxide.

[0055] Example 2

[0056] A method for preparing an isolated mineral insulated fireproof cable material, comprising the following steps:

[0057] Step 1, weighing 10kg methyl vinyl silicone rubber, 2kg cobalt-doped magnesium hydroxide, 0.5kg hydroxyapatite, 1kg kaolin, 0.3kg zinc borate, 0.9kg calcium carbonate, 0.6kg hydrophobic white carbon black, and 0.2kg di-2-4;

[0058] Step 2, adding methyl vinyl silicone rubber, cobalt-doped magnesium hydroxide, hydroxyapatite, kaolin, zinc borate, calcium carbonate, and hydrophobic white carbon black into a mixer for mixing to obtain a rubber material, and then thinning the rubber material to obtain a blank;

[0059] Step 3: feeding the obtained blank into a vulcanizer, then adding double 24 and mixing, vulcanizing, and extruding to obtain an isolated mineral insulated fireproof cable material.

[0060] The preparation method of cobalt-doped magnesium hydroxide is as follows:

[0061] S1, placing 20g of magnesium oxide and 100g of 50% by volume ethanol aqueous solution in a ball mill at a speed of 300rpm for ball milling, and then placing the slurry in a constant temperature oven at 100°C to dry to obtain refined magnesium oxide with an average particle size of 3μm;

[0062] S2. 20 g of refined magnesium oxide was stirred at a speed of 350 rpm for 10 min, dispersed in 120 mL of a 2 mol / L sodium acetate aqueous solution, and then 1 g of cobalt nitrate hexahydrate and 0.5 g of sodium benzoate were added and continued to stir and mix for 15 min, and then kept at 180 ° C for 5 h for hydrothermal reaction. After natural cooling, the solution was taken out, the insoluble matter was collected by filtration, washed three times with water and ethanol respectively, and finally dried in a constant temperature oven at 120 ° C to obtain cobalt-doped magnesium hydroxide.

[0063] Comparative Example 1

[0064] A method for preparing an isolated mineral insulated fireproof cable material, comprising the following steps:

[0065] Step 1, weigh 10kg methyl vinyl silicone rubber, 2kg magnesium hydroxide, 0.5kg hydroxyapatite, 1kg kaolin, 0.3kg zinc borate, 0.9kg calcium carbonate, 0.6kg hydrophobic white carbon black, and 0.2kg di-2-4;

[0066] Step 2, adding methyl vinyl silicone rubber, magnesium hydroxide, hydroxyapatite, kaolin, zinc borate, calcium carbonate, and hydrophobic white carbon black into a mixer for mixing to obtain a rubber material, and then thinning the rubber material to obtain a blank;

[0067] Step 3: feeding the obtained blank into a vulcanizer, then adding double 24 and mixing, vulcanizing, and extruding to obtain an isolated mineral insulated fireproof cable material.

[0068] The preparation method of magnesium hydroxide is:

[0069] S1, placing 20g of magnesium oxide and 100g of 50% by volume ethanol aqueous solution in a ball mill at a speed of 300rpm for ball milling, and then placing the slurry in a constant temperature oven at 100°C to dry to obtain refined magnesium oxide with an average particle size of 3μm;

[0070] S2. 20 g of refined magnesium oxide was stirred at a speed of 350 rpm for 10 min, dispersed in 120 mL of a 2 mol / L sodium acetate aqueous solution, and then stirred for 15 min to mix, and then kept at 180 ° C for 5 h for hydrothermal reaction. After natural cooling, the solution was taken out, the insoluble matter was collected by filtration, washed with water and ethanol three times each, and finally dried in a constant temperature oven at 120 ° C to obtain magnesium hydroxide.

[0071] Comparative Example 2

[0072] A method for preparing an isolated mineral insulated fireproof cable material, comprising the following steps:

[0073] Step 1, weighing 10kg methyl vinyl silicone rubber, 2.5kg cobalt-doped magnesium hydroxide, 1kg kaolin, 0.9kg calcium carbonate, 0.3kg zinc borate, 0.6kg hydrophobic white carbon black, and 0.2kg bis(2,4-dimethyl-2,4-bis(2,4-di-)-1,4-di-1,4-di-1;

[0074] Step 2, adding methyl vinyl silicone rubber, cobalt-doped magnesium hydroxide, kaolin, zinc borate, calcium carbonate, and hydrophobic white carbon black into a mixer for mixing to obtain a rubber material, and then thinning the rubber material to obtain a blank;

[0075] Step 3: feeding the obtained blank into a vulcanizer, then adding double 24 and mixing, vulcanizing, and extruding to obtain an isolated mineral insulated fireproof cable material.

[0076] Wherein, the preparation method of cobalt-doped magnesium hydroxide is the same as that in Example 2.

[0077] Comparative Example 3

[0078] A method for preparing an isolated mineral insulated fireproof cable material, comprising the following steps:

[0079] Step 1, weighing 10kg methyl vinyl silicone rubber, 2.3kg cobalt-doped magnesium hydroxide, 0.5kg hydroxyapatite, 1kg kaolin, 0.9kg calcium carbonate, 0.6kg hydrophobic silica, and 0.2kg bis(2,4-dioxadiene);

[0080] Step 2, adding methyl vinyl silicone rubber, cobalt-doped magnesium hydroxide, hydroxyapatite, kaolin, calcium carbonate, and hydrophobic white carbon black into a mixer for mixing to obtain a rubber material, and then thinning the rubber material to obtain a blank;

[0081] Step 3: feeding the obtained blank into a vulcanizer, then adding double 24 and mixing, vulcanizing, and extruding to obtain an isolated mineral insulated fireproof cable material.

[0082] Wherein, the preparation method of cobalt-doped magnesium hydroxide is the same as that in Example 2.

[0083] Referring to the standard GB / T 2408-2021 "Determination of the combustion performance of plastics by horizontal and vertical methods", the fire-resistant cable materials of the embodiments and comparative examples were made into test specimens of 125mm×13mm×10mm, and the limiting oxygen index was tested. Referring to the standard GB / T 9341-2008 "Determination of the bending properties of plastics", the fire-resistant cable materials of the embodiments and comparative examples were made into test specimens of 80mm×10mm×4mm and placed in a muffle furnace at 1000℃ for 30min, and the bending strength of the specimens after burning was tested according to the three-point bending test. The fire-resistant cable materials of the embodiments and comparative examples were also made into test specimens of 100mm×100mm×10mm and placed in a muffle furnace at 1000℃ for 30min, and the thickness before and after was measured to calculate the expansion rate. These results are shown in Table 1. Generally speaking, the larger the limiting oxygen index, the better the flame retardant properties of the material, and a limiting oxygen index higher than 27% is considered to be flame retardant; the greater the mechanical strength of the burning product, the more stable the vitrified structure formed; the smaller the expansion rate, the smaller the volume change, which will not cause a major impact on the cable as a whole.

[0084] Table 1 Flexural strength and expansion rate results

[0085] Limiting oxygen index (%) Bending strength(MPa) Expansion rate (%) Example 1 33.8 0.8 43 Example 2 34.9 1.5 32 Comparative Example 1 32.1 1.2 39 Comparative Example 2 28.3 0.5 52 Comparative Example 3 27.8 0.3 65

[0086] It can be seen that both the examples and the comparative examples have good flame retardant effects, which is attributed to the characteristics of methyl vinyl silicone rubber and the good flame retardant effects of hydroxyapatite, kaolin, cobalt-doped magnesium hydroxide or magnesium hydroxide. Especially in Examples 1 and 2 where cobalt-doped magnesium hydroxide is added, this is because the cobalt doping catalyzes the formation of the carbon layer, captures the free radicals generated by combustion, and inhibits the combustion process. However, the bending strength and expansion rate of Example 1 are both poor. From Figure 1 to Figure 3 It can be seen that the magnesium hydroxide prepared without cobalt doping in Comparative Example 1 presents irregular flakes, while the cobalt-doped magnesium hydroxide after adding cobalt in Example 1 still has a flake structure as a whole but with obvious agglomeration. In Example 2, sodium benzoate is added during the reaction to obtain cobalt-doped magnesium hydroxide with uniform dispersion, uniform particle size and significantly reduced agglomeration. Figures 4 to 6 It can be seen that the uniform structure is conducive to forming a more stable porcelain structure during firing. The bending strength of Comparative Examples 2 and 3 after firing decreased more significantly and the expansion rate was greater. Figure 7 and Figure 8 This is because phosphorus in hydroxyapatite can react with aluminum in kaolin at high temperature to generate low melting point aluminum phosphate with bonding effect, and zinc borate promotes the formation of a large amount of liquid phase substances at high temperature, which can connect the residues more evenly. The fireproof cable material of Example 2 of the present invention expands less when burned, and the dense carbonized layer and hard ceramic matrix produced during burning can support the unburned part, thereby improving the flame retardant performance of the cable material.

[0087] Please refer to Fig. 9 The fireproof cable materials of the embodiment and the comparative example are also assembled into cables. The other components of the cable are conventional fireproof cable materials, the filling material is porous flame-retardant polyolefin, and the glass fiber cloth tape and low-smoke halogen-free flame-retardant polyolefin sheath are used. Referring to the standard GB / T 19216.21-2003 "Line integrity test for cables or optical cables under flame conditions Part 21: Test procedures and requirements for cables with rated voltages of 0.6 / 1.0 kV and below", and referring to the standard GB / T 16422.2-2022 "Plastic laboratory light source exposure test method Part 2: Xenon arc lamp", the fireproof cable materials of the embodiment and the comparative example are measured again after aging for 1000 hours, and the results are shown in Table 2.

[0088] Table 2 Power supply time under combustion

[0089]

[0090]

[0091] From the test results in Table 2, it can be seen that the fireproof cable material of Example 2 of the present invention can continuously supply power for up to 192 minutes at a flame temperature of 1000° C., and the power supply time does not show a significant decrease even after aging for 1000 hours.

[0092] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An isolated mineral insulated fireproof cable material, characterized in that: The composition comprises, by weight, 90 to 120 parts of silicone rubber, 15 to 25 parts of cobalt-doped magnesium hydroxide, 5 to 10 parts of hydroxyapatite, 5 to 15 parts of kaolin, 2 to 5 parts of zinc borate, 10 to 20 parts of filler, and 1 to 3 parts of vulcanizing agent; The preparation method of cobalt-doped magnesium hydroxide comprises: The magnesium oxide coarse material is wet ball-milled to collect the refined magnesium oxide; Dispersing refined magnesium oxide in a sodium acetate aqueous solution, then adding a water-soluble cobalt salt and mixing them for hydrothermal reaction to obtain cobalt-doped magnesium hydroxide; The mass of the water-soluble cobalt salt is 0.05 to 0.1 times that of the refined magnesium oxide; After adding the water-soluble cobalt salt, sodium benzoate in an amount of 0.1 to 0.5 times the mass of the water-soluble cobalt salt is also added.

2. The isolated mineral insulated fireproof cable material according to claim 1, characterized in that: The particle size of the refined magnesium oxide is 1-5 μm.

3. The isolated mineral insulated fireproof cable material according to claim 1, characterized in that: The concentration of the sodium acetate aqueous solution is 1-3 mol / L; The ratio of the refined magnesium oxide to the sodium acetate aqueous solution is 10-30:100-150 g / mL.

4. The isolated mineral insulated fireproof cable material according to claim 1, characterized in that: The hydrothermal reaction is continued at 160-200° C. for 3-8 hours.

5. The isolated mineral insulated fireproof cable material according to claim 1, characterized in that: The silicone rubber is at least one of methyl silicone rubber, methyl vinyl silicone rubber, and trimethylsiloxymethyl silicone rubber.

6. The isolated mineral insulated fireproof cable material according to claim 1, characterized in that: The filler is obtained by mixing calcium carbonate and hydrophobic white carbon black in a mass ratio of 2-5:1-3.

7. A method for preparing the isolated mineral insulated fireproof cable material according to any one of claims 1 to 6, characterized in that: include, The silicone rubber, cobalt-doped magnesium hydroxide, hydroxyapatite, kaolin, zinc borate and filler are mixed to obtain a rubber compound, and then the rubber compound is thinned to obtain a blank; The blank is mixed with a vulcanizing agent, vulcanized, and extruded to obtain an isolated mineral insulated fireproof cable material.

8. A fireproof cable, characterized in that: The invention comprises the isolated mineral insulated fireproof cable material as described in any one of claims 1 to 6.