Silicon carbide epitaxial wafer and preparation method thereof, and semiconductor device
By sequentially growing doped epitaxial layers on the silicon carbide epitaxial wafer substrate and using etching gas to form a low-concentration interface layer, the problem of blurred interfaces of doped epitaxial layers in silicon carbide epitaxial wafers is solved and interface clarity is achieved. improvement and production efficiency.
Patent Information
- Application Number
- CN202410683181.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-30
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-05-30
AI Technical Summary
There is an interface fuzzy problem between epitaxial layers of different doping types in existing silicon carbide epitaxial wafers, resulting in unclear interfaces and affecting device performance. The multi-cavity growth method is costly and difficult to control pollutants.
By sequentially growing a first doped type epitaxial layer and a second doped type epitaxial layer on the substrate, etching the surface of the first doped type epitaxial layer using an etching gas to form a second doped type interface with a low concentration. layer, and grow a silicon carbide layer with a doping concentration lower than the first concentration on the interface layer to suppress the diffusion of doping elements and improve the interface state.
It effectively improves the interface clarity between epitaxial layers of different doping types, reduces costs, improves production efficiency, weakens the background memory effect and the doping element atmosphere in the epitaxial chamber, and improves the quality of the epitaxial layer.
Smart Images

Figure CN118248535B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a silicon carbide epitaxial wafer and a preparation method thereof, and a semiconductor device. Background Art
[0002] Silicon carbide (SiC), as a wide bandgap semiconductor material, has outstanding advantages such as high thermal conductivity, high breakdown electric field, high saturated electron drift velocity and high bonding energy. Its excellent performance can meet the requirements of modern electronic technology for high temperature, high frequency, high power and radiation resistance.
[0003] Among them, for silicon carbide devices, they usually need to be formed by multiple silicon carbide epitaxial layers, especially multiple silicon carbide epitaxial layers with different doping types. However, the interfaces between silicon carbide epitaxial layers with different doping types are easily blurred due to the background memory effect.
[0004] For example, when epitaxially growing an N-type silicon carbide layer on the surface of a substrate, it is generally necessary to introduce a silicon source, a carbon source, and an N-type doping source (e.g., a doping source containing nitrogen elements) to epitaxially grow the N-type silicon carbide layer on the surface of the substrate; and to introduce a silicon source, a carbon source, and a P-type doping source (e.g., a doping source containing trimethylaluminum) to epitaxially grow a P-type silicon carbide layer on the surface of the N-type silicon carbide layer. However, when epitaxially growing a P-type silicon carbide layer, due to the memory effect of the N-type doping background, it is easy for the N-type doping element to diffuse into the P-type silicon carbide layer, affecting the accuracy of the P-type doping concentration in the P-type silicon carbide layer, and also making the interface between the P-type silicon carbide layer and the N-type silicon carbide layer unclear.
[0005] In addition, for the epitaxial chamber for epitaxial growth of N-type silicon carbide layer, a large amount of N-type doping elements (for example, nitrogen) will be attached to the inside of the chamber, so that there is also a serious memory effect of the N-type doping background in the epitaxial chamber, which will also affect the film quality of the subsequently grown P-type epitaxial layer. Therefore, the prior art generally needs to adopt a multi-chamber growth method to perform the growth steps of epitaxial layers of different doping types in different epitaxial chambers. However, this growth method is costly and requires the substrate structure to be transferred between different chambers, which increases the difficulty of controlling pollutants. Summary of the invention
[0006] One of the purposes of the present invention is to provide a method for preparing a silicon carbide epitaxial wafer to solve the problem of interface blur between epitaxial layers of different doping types in the existing silicon carbide epitaxial wafer.
[0007] In order to solve the above technical problems, the present invention provides a method for preparing a silicon carbide epitaxial wafer, comprising: providing a substrate, and sequentially growing a first doping type epitaxial layer and a second doping type epitaxial layer on the substrate. The method for growing the second doping type epitaxial layer comprises: introducing an etching gas to etch the surface of the first doping type epitaxial layer; introducing a second doping type doping source to form a second doping type interface layer with a first concentration on the first doping type epitaxial layer; and introducing a silicon source, a carbon source, and a second doping type doping source to epitaxially grow at least one second doping type silicon carbide layer with a doping concentration lower than the first concentration on the second doping type interface layer.
[0008] Optionally, the method for epitaxially growing the first doping type epitaxial layer includes: introducing a silicon source, a carbon source and a first doping type doping source to epitaxially grow a first doping type silicon carbide layer on the substrate.
[0009] Optionally, the method for epitaxially growing the first doped type epitaxial layer also includes: introducing an etching gas to etch the surface of the first doped type silicon carbide layer; and introducing a silicon source, a carbon source and a first doping type doping source to grow a first doped type interface layer on the first doped type silicon carbide layer, the thickness of the first doped type interface layer being less than the thickness of the first doped type silicon carbide layer.
[0010] Optionally, the thickness of the first doping type silicon carbide layer is 1 μm-3 μm; and / or the thickness of the first doping type interface layer is 10 nm-500 nm.
[0011] Optionally, the etching gas used when growing the first doping type epitaxial layer includes a chlorine-containing gas; and / or the etching gas used when growing the second doping type epitaxial layer includes a chlorine-containing gas.
[0012] Optionally, the method for forming the second doping type interface layer includes: introducing at least one gas containing trimethylaluminum and aluminum hydride to form an aluminum-rich layer to constitute the second doping type interface layer; or, introducing a borane-containing gas to form a boron-rich layer to constitute the second doping type interface layer.
[0013] Optionally, at least two second doped type silicon carbide layers with doping concentrations decreasing from bottom to top are grown on the second doped type interface layer.
[0014] Optionally, the method for growing the at least two second doped type silicon carbide layers includes: adjusting the silicon source and the carbon source so that the carbon-silicon ratio decreases successively, thereby reducing the doping concentration gradient of the grown at least two second doped type silicon carbide layers.
[0015] Optionally, among the at least two layers of the second doped type silicon carbide layers, the bottom layer of the second doped type silicon carbide layer has the smallest thickness.
[0016] Optionally, the first doping type epitaxial layer and the second doping type epitaxial layer are grown in the same epitaxial chamber.
[0017] Another object of the present invention is to provide a silicon carbide epitaxial wafer, comprising: a substrate, a first doping type epitaxial layer and a second doping type epitaxial layer sequentially formed on the substrate. The second doping type epitaxial layer comprises: a second doping type interface layer having a first concentration, the second doping type interface layer is grown on the first doping type epitaxial layer; and at least one second doping type silicon carbide layer, the second doping type silicon carbide layer has a doping concentration lower than the first concentration and is grown above the second doping type interface layer.
[0018] Optionally, the first doped type epitaxial layer includes: a first doped type silicon carbide layer and a first doped type interface layer grown on the first doped type silicon carbide layer, and a thickness of the first doped type interface layer is less than a thickness of the first doped type silicon carbide layer.
[0019] Optionally, the thickness of the first doping type silicon carbide layer is 1 μm-3 μm; and / or the thickness of the first doping type interface layer is 10 nm-500 nm.
[0020] Optionally, the second doping type epitaxial layer includes: at least two second doping type silicon carbide layers whose doping concentration decreases gradually from bottom to top.
[0021] Optionally, among the at least two layers of the second doped type silicon carbide layers, the bottom layer of the second doped type silicon carbide layer has the smallest thickness.
[0022] Another object of the present invention is to provide a semiconductor device, comprising: obtaining a silicon carbide epitaxial wafer using the method described above, or providing a silicon carbide epitaxial wafer described above; and a device structure formed on the silicon carbide epitaxial wafer.
[0023] In the method for preparing the silicon carbide epitaxial wafer provided by the present invention, before growing the silicon carbide layer in the second doping type epitaxial layer, an etching gas is introduced to etch the top surface of the first doping type epitaxial layer, which can not only reduce the doping elements of the first doping type on its surface and weaken the background memory effect, but also remove the surface defects of the first doping type epitaxial layer, so that when epitaxially growing epitaxial layers of different doping types, it is beneficial to improve the interface state between epitaxial layers of different doping types and improve the quality of epitaxial layers grown epitaxially. At the same time, the introduction of etching gas can also reduce the atmosphere of the doping elements of the first doping type in the epitaxial chamber where the substrate is located, weaken the background memory effect caused by the epitaxial chamber, so that even if the first doping type epitaxial layer and the second doping type epitaxial layer are grown in sequence in the same epitaxial chamber, the interface clarity between the epitaxial layers of different doping types can still be effectively improved. That is to say, in the preparation method provided by the present invention, epitaxial layers of different doping types can be allowed to be grown in sequence in the same epitaxial chamber, and the interfaces between the grown epitaxial layers of different doping types are clear, which is beneficial to reducing costs and improving production efficiency.
[0024] In addition, before introducing the silicon source and the carbon source to grow the second doping type silicon carbide layer, the second doping type doping source is preferentially introduced to form a high-concentration second doping type interface layer, so as to utilize the high-concentration second doping type interface layer to suppress the diffusion of the first doping type doping elements underneath it, thereby making the interface between the epitaxial layers of different doping types clearer. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The included drawings are used to provide a further understanding of the embodiments of the present invention, which constitute a part of the specification, are used to illustrate the implementation of the present invention, and together with the text description, explain the principles of the present invention. Obviously, the drawings in the following description are only some embodiments of the present invention.
[0026] Figure 1 The figure is a schematic flow chart of a method for preparing a silicon carbide epitaxial wafer in one embodiment of the present invention.
[0027] Figure 2 Schematic diagram of the structure of a silicon carbide epitaxial wafer in one embodiment of the present invention.
[0028] Figure 3 The present invention is a flowchart of a specific preparation process of a method for preparing a silicon carbide epitaxial wafer in one embodiment of the present invention.
[0029] Among them, the figure markings are as follows: 100-substrate; 110-buffer layer; 200-first doping type epitaxial layer; 210-first doping type silicon carbide layer; 220-first doping type interface layer; 300-second doping type epitaxial layer; 310-second doping type interface layer; 320a / 320b / 320c-second doping type silicon carbide layer. DETAILED DESCRIPTION
[0030] The core idea of the present invention is to provide a silicon carbide epitaxial wafer and a preparation method thereof, which can effectively improve the problem of interface blur between epitaxial layers of different doping types caused by the background memory effect, and is conducive to achieving the purpose of sequentially growing epitaxial layers of different doping types in the same epitaxial chamber.
[0031] Specifically, a method for preparing a silicon carbide epitaxial wafer may include: providing a substrate, and sequentially growing a first doping type epitaxial layer and a second doping type epitaxial layer on the substrate. The method for growing the second doping type epitaxial layer includes: introducing an etching gas to etch the surface of the first doping type epitaxial layer; introducing a second doping type doping source to grow a second doping type interface layer with a first concentration on the first doping type epitaxial layer; and introducing a silicon source, a carbon source, and a second doping type doping source to epitaxially grow at least one second doping type silicon carbide layer with a doping concentration lower than the first concentration on the second doping type interface layer.
[0032] That is, in the method for preparing the silicon carbide epitaxial wafer provided by the present invention, when the second doping type epitaxial layer continues to grow on the first doping type epitaxial layer, the etching gas is introduced, which can produce the following beneficial effects:
[0033] 1) The surface of the first doping type epitaxial layer can be etched to reduce the doping elements of the first doping type on the surface and weaken the background memory effect, thereby facilitating the improvement of the interface state between epitaxial layers of different doping types when epitaxially growing epitaxial layers of different doping types;
[0034] 2) When etching the top surface of the first doped type epitaxial layer, stress defects of the first doped type epitaxial layer are also removed, thereby improving the surface flatness of the first doped type epitaxial layer, and on this basis, the film quality of the subsequently grown epitaxial layer can be correspondingly improved;
[0035] 3) The etching gas can also remove the first doping type doping material attached to the inner wall of the epitaxial chamber where the substrate is located, weaken the atmosphere of the first doping type doping element in the epitaxial chamber, and weaken the background memory effect caused by the epitaxial chamber. Therefore, even if the first doping type epitaxial layer and the second doping type epitaxial layer are grown in sequence in the same epitaxial chamber, the interface clarity between the epitaxial layers of different doping types can still be effectively improved.
[0036] In addition, before introducing the silicon source and the carbon source to grow the second doping type silicon carbide layer, the second doping type doping source is preferentially introduced to form a second doping type interface layer with a high concentration, that is, a high concentration second doping type interface layer is preferentially formed on the first doping type epitaxial layer, so as to utilize the high concentration second doping type interface layer to suppress the diffusion of the first doping type doping elements thereunder, thereby making the interface between the epitaxial layers of different doping types clearer.
[0037] Furthermore, the etching gas used may include chlorine-containing gas, which is used in the preparation process of silicon carbide epitaxial wafers, so as to avoid introducing other impurities when etching the first doped type epitaxial layer; at the same time, when the chlorine-containing gas is used to treat the surface of the first doped type epitaxial layer, it is beneficial to consume the doping elements of the first doping type on the surface of the epitaxial layer, and it is also easy to form a chloride film on the surface of the epitaxial layer. The presence of the chloride film layer is also beneficial to inhibiting the diffusion of the doping elements underneath it, further improving the interface clarity between epitaxial layers of different doping types.
[0038] Furthermore, the method for epitaxially growing a first doping type epitaxial layer may include: introducing a silicon source, a carbon source, and a first doping type doping source to epitaxially grow a first doping type silicon carbide layer on a substrate.
[0039] Exemplarily, after growing the first doped type silicon carbide layer, the method further includes: introducing an etching gas to etch the surface of the first doped type silicon carbide layer; then, growing a first doped type interface layer on the first doped type silicon carbide layer, wherein the thickness of the first doped type interface layer is less than the thickness of the first doped type silicon carbide layer. In this example, the top surface of the first doped type silicon carbide layer can also be etched using the etching gas to remove stress defects of the first doped type silicon carbide layer and improve the surface flatness of the film layer. On this basis, the film quality of the first doped type interface layer grown subsequently can be correspondingly improved. In other words, the second doped type epitaxial layer grown subsequently is grown on the high-quality first doped type interface layer, which is conducive to further improving the quality of the second doped type epitaxial layer.
[0040] Furthermore, the second doping type epitaxial layer may specifically include at least two second doping type silicon carbide layers whose doping concentrations decrease from bottom to top, for example, two or more silicon carbide layers whose concentrations decrease gradually. It can be considered that by arranging the second doping type epitaxial layer in a manner in which the concentrations decrease from bottom to top, the silicon carbide layer between the interface layer and the top silicon carbide layer constitutes a concentration buffer, thereby avoiding the formation of a low-concentration silicon carbide layer directly on the high-concentration interface layer.
[0041] The silicon carbide epitaxial wafer, preparation method thereof, and semiconductor device proposed in the present invention are further described in detail below in conjunction with the accompanying drawings. According to the following description, the advantages and features of the present invention will become clearer. It should be noted that the drawings are all in a very simplified form and use non-precise proportions, which are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention. It should be recognized that relative terms such as "above", "below", "top", "bottom", "above" and "below" shown in the drawings can be used to describe the relationship between various elements. These relative terms are intended to cover different orientations of elements other than the orientations depicted in the drawings. For example, if the device is inverted relative to the view in the drawing, an element described as being "above" another element will now be below the element.
[0042] Figure 1 is a schematic flow chart of a method for preparing a silicon carbide epitaxial wafer in one embodiment of the present invention, Figure 2 FIG. 1 is a schematic diagram of the structure of a silicon carbide epitaxial wafer in an embodiment of the present invention. Figure 1 The preparation process shown is used as an example to illustrate the formation of Figure 2 The method for preparing the epitaxial wafer shown in the embodiment is described by taking the example of sequentially growing epitaxial layers of different doping types in the same epitaxial chamber.
[0043] First, execute step S110. Figure 2 As shown, a substrate 100 is provided and placed in an epitaxial chamber. In this embodiment, a chemical vapor deposition process (CVD) or MOCVD process can be used to perform epitaxial growth on the substrate.
[0044] The substrate 100 may be specifically a silicon carbide substrate, and in subsequent steps, a first doping type epitaxial layer 200 and a second doping type epitaxial layer 300 will be sequentially epitaxially grown on the substrate 100. The first doping type epitaxial layer 200 and the second doping type epitaxial layer 300 grown in subsequent steps can be used to further form semiconductor devices, for example, can be used to form a drift region and a well region of a MOSFET device.
[0045] Exemplarily, a buffer layer 110 may be formed on the substrate 100, and the buffer layer 110 may include, for example, at least one silicon carbide buffer layer. Specifically, there are usually many defects in the provided substrate 100, and when epitaxial growth is performed on this basis, the defects in the substrate are easily propagated to the epitaxial layer, so it is difficult to epitaxially grow a high-quality silicon carbide epitaxial layer directly on the substrate 100. At this time, a buffer layer 110 may be preferentially formed on the substrate 100 to prevent the defects in the substrate 100 from extending into the silicon carbide epitaxial layer, thereby improving the quality of the silicon carbide epitaxial layer epitaxially grown in subsequent steps.
[0046] Then execute step S120, and continue to refer to Figure 2 As shown, a first doping type epitaxial layer 200 is epitaxially grown in an epitaxial chamber. In a specific example, the first doping type epitaxial layer 200 is, for example, an N-type epitaxial layer, and the second doping type epitaxial layer 300 formed subsequently is a P-type epitaxial layer; or, the first doping type epitaxial layer 200 is a P-type epitaxial layer, and the second doping type epitaxial layer 300 is an N-type epitaxial layer.
[0047] Before epitaxially growing the first doped type epitaxial layer 200, the process also includes: performing high-temperature cleaning on the substrate 100. The specific cleaning method is, for example, introducing hydrogen (H2) into the epitaxial chamber, and controlling the temperature of the epitaxial chamber to be 1400°C-1700°C, so as to perform high-temperature cleaning and heating baking on the substrate 100, and the baking time can be 1min-50min. During this process, for example, the chamber pressure in the epitaxial chamber can be maintained at 50mbar-400mbar. Afterwards, the first doped type epitaxial layer 200 can be epitaxially grown on the substrate 100.
[0048] Further, the method for growing the first doping type epitaxial layer 200 may include: introducing a silicon source, a carbon source and a doping source of the first doping type (for example, an N-type doping source) into the epitaxial chamber to epitaxially grow the first doping type silicon carbide layer 210 on the substrate 100. Among them, the silicon source used includes, for example, at least one of silane, dichlorosilane, trichlorosilane and tetrachlorosilane. The carbon source used includes, for example, at least one of methane, ethylene, acetylene and propane. And, the first doping type takes N-type doping as an example, then the doping source of the first doping type can be a nitrogen-containing gas, for example, including at least one of nitrogen (N2) and ammonia (NH3). In this process, a carrier gas (for example, hydrogen) can also be introduced into the epitaxial chamber, and the growth pressure of the epitaxial chamber is maintained at 50mbar to 400mbar, and the growth temperature is 1500℃-1700℃. In a specific example, the thickness of the grown first doping type silicon carbide layer 210 may be 1 μm-3 μm, and the doping concentration thereof may be, for example, 5E16 / cm 3 -1E18 / cm 3 .
[0049] For example, Figure 1 and Figure 2As shown, the method for growing the first doping type epitaxial layer 200 may also include: introducing an etching gas into the epitaxial chamber to etch the surface of the first doping type silicon carbide layer 210; then, forming a first doping type interface layer 220 on the first doping type silicon carbide layer 210. The first doping type interface layer 220 may also be a silicon carbide layer, and at this time, a silicon source, a carbon source, and a doping source of the first doping type may be introduced into the epitaxial chamber to grow the first doping type interface layer 220. In addition, the thickness of the first doping type interface layer 220 may be smaller than the thickness of the first doping type silicon carbide layer 210, so as to form an interface layer between the first doping type epitaxial layer 200 and the second doping type epitaxial layer 300 formed subsequently.
[0050] In this example, the first doping type epitaxial layer 200 includes a first doping type silicon carbide layer 210 and a first doping type interface layer 220. Before the first doping type interface layer 220 is epitaxially grown, the surface of the first doping type silicon carbide layer 210 is etched to remove stress defects of the first doping type silicon carbide layer 210 and improve the surface flatness of the first doping type silicon carbide layer 210, so that it is beneficial to improve the crystal quality of the first doping type interface layer 220 further epitaxially grown on the first doping type silicon carbide layer 210. In particular, the thickness of the first doping type interface layer 220 is small, so that the quality of the first doping type interface layer 220 is stable. Taking N-type doping as an example, the first doping type interface layer 220 can form an N-type interface with good crystal quality at this time, providing a high-quality growth environment for the subsequent growth of the second doping type epitaxial layer 300.
[0051] The etching gas used for the surface treatment of the first doped type silicon carbide layer 210 may include a chlorine-containing gas, such as hydrogen chloride gas (HCL), and a carrier gas (such as hydrogen) may be continuously introduced during the process, and the growth pressure of the epitaxial chamber may be maintained at 50 mbar to 400 mbar, the growth temperature may be 1500° C. to 1700° C., and the treatment time using the hydrogen chloride gas may be, for example, 1 min to 50 min. Furthermore, the silicon source, carbon source, and doping source used when growing the first doped type interface layer 220 may be consistent with the silicon source, carbon source, and doping source used when growing the first doped type silicon carbide layer 210.
[0052] In addition, the doping concentration of the first doping type interface layer 220 may be slightly lower than the doping concentration of the first doping type silicon carbide layer 210. For example, the doping concentration of the first doping type interface layer 220 may be 5E15-1E18cm 3 Furthermore, the thickness of the first doping type interface layer 220 is less than the thickness of the first doping type silicon carbide layer 210 . For example, the growth thickness of the first doping type interface layer 220 is 10 nm-500 nm.
[0053] Then execute step S130, and continue to refer to Figure 2 As shown, the second doping type epitaxial layer 300 is epitaxially grown in the epitaxial chamber. That is, in this embodiment, the first doping type epitaxial layer 200 and the second doping type epitaxial layer 300 of different doping types are sequentially grown in the same epitaxial chamber.
[0054] The method for epitaxially growing the second doping type epitaxial layer 300 may include: epitaxially growing a second doping type interface layer 310 having a first concentration and at least one second doping type silicon carbide layer having a doping concentration lower than the first concentration (for example, Figure 2 In the example of FIG. 3 , three layers of second doped type silicon carbide layers 320a / 320b / 320c are illustrated). That is, before growing the second doped type silicon carbide layer, a high-concentration second doped type interface layer 310 is preferentially formed, so that the high-concentration second doped type interface layer 310 can be used to suppress the diffusion of the first doped type doping element thereunder (for example, the diffusion of nitrogen element can be suppressed), thereby improving the interface clarity between epitaxial layers of different doping types.
[0055] In a specific example, the method of epitaxially growing the second doping type epitaxial layer 300 may include the following steps.
[0056] In the first step, an etching gas (e.g., chlorine-containing gas) is introduced into the epitaxial chamber to process the surface of the epitaxial chamber and the first doping type epitaxial layer 200, so as to reduce the first doping type doping element (e.g., nitrogen element) attached to the epitaxial chamber, and reduce the first doping type doping element (e.g., nitrogen element) on the surface of the first doping type epitaxial layer 200, and reduce the diffusion movement of the first doping type doping element (e.g., nitrogen element), thereby improving the diffusion of the first doping type doping element into the second doping type epitaxial layer formed subsequently. In addition, when the surface of the first doping type epitaxial layer 200 is processed using a chlorine-containing etching gas, a chloride film is easily formed on the surface of the epitaxial layer, and the presence of the chloride film is also conducive to inhibiting the diffusion of the doping element.
[0057] The etching gas used in this step includes, for example, hydrogen chloride gas (HCL), and a carrier gas (such as hydrogen) can be continuously introduced during this process. At the same time, the growth pressure of the epitaxial chamber can be maintained at 50mbar~400mbar, the growth temperature is 1500℃-1700℃, and the time for introducing the etching gas can be controlled to be 1 min-50min.
[0058] In the second step, a doping source of a second doping type (for example, a doping source of a P-type doping) is introduced to form a second doping type interface layer 310 having a first concentration on the first doping type epitaxial layer 200. In this embodiment, the second doping type interface layer 310 is specifically grown on the first doping type interface layer 220. It should be noted that in this step, a high-concentration doping source of a second doping type is introduced, for example, only a doping source of a second doping type and a carrier gas may be introduced without introducing a silicon source and a carbon source, so as to form a high-concentration second doping type interface layer 310.
[0059] For example, in this step, at least one gas containing trimethylaluminum (TMAL) and aluminum hydride can be introduced to form an aluminum-rich second doping type interface layer 310, wherein the aluminum hydride is, for example, aluminum hydride (AlH), aluminum dihydride (AlH2) and / or aluminum trihydride (AlH3). The second doping type interface layer 310 is a P-rich interface, which effectively inhibits the diffusion of nitrogen atoms, for example. Alternatively, in this step, a borane-containing gas can be introduced to form a boron-rich second doping type interface layer 310, constituting a P-rich interface. In this process, a carrier gas (such as hydrogen) can also be introduced, and the growth pressure of the epitaxial chamber is maintained at 50mbar to 400mbar, and the growth temperature is 1500℃-1700℃.
[0060] In the third step, a silicon source, a carbon source, and a second doping type doping source are introduced to epitaxially grow at least one second doping type silicon carbide layer (for example, Figure 2 The three layers of second doped type silicon carbide layers 320a / 320b / 320c are shown.
[0061] In a specific example, at least two layers of second doping type silicon carbide layers with doping concentrations decreasing from bottom to top may be sequentially grown on the second doping type interface layer 310. Figure 2 In the example, a second doped type silicon carbide layer 320a, a second doped type silicon carbide layer 320b and a second doped type silicon carbide layer 320c with gradually decreasing concentrations are grown in sequence. By setting the doping concentration in a gradient, a concentration buffer can be formed from the second doped type interface layer 310 to the top layer of the second doped type silicon carbide layer 320c, thereby avoiding the direct formation of a low-concentration silicon carbide layer on the high-concentration interface layer.
[0062] Among them, when epitaxially growing each second doped type silicon carbide layer, the same type of silicon source, carbon source and second doped type doping source can be used, and the ratio of silicon source and carbon source, the flow rate of doping source, etc. can be adjusted accordingly according to the specific concentration requirements of each silicon carbide layer. In a specific example, the silicon source and the carbon source can be adjusted so that the carbon-silicon ratio is gradually reduced, thereby forming a multi-layer silicon carbide layer with a gradually decreasing doping concentration from bottom to top. Taking the growth of a P-type doped silicon carbide epitaxial layer as an example, when the carbon-silicon ratio is relatively large, it is more conducive to the doping of P-type doping ions in the silicon carbide layer to form a P-type doped silicon carbide layer with a higher concentration; conversely, when the carbon-silicon ratio is smaller, the doping amount of P-type doping ions can be lower, thereby forming a silicon carbide epitaxial layer with a lower concentration. Also, among the at least two layers of second doped type silicon carbide layers, the thickness of the bottom second doped type silicon carbide layer can be the smallest, and the thickness of the upper second doped type silicon carbide layer can be the same or different. For example Figure 2 In the example, the thickness of the bottom second doped type silicon carbide layer 320a is the smallest, and the thicknesses of the second doped type silicon carbide layer 320b and the second doped type silicon carbide layer 320c may be the same or different.
[0063] In order to make the method for preparing the silicon carbide epitaxial wafer provided by the present disclosure clearer, the following is combined with Figure 2 and Figure 3 A specific example is used to further illustrate a preparation process of a silicon carbide epitaxial wafer, and the preparation process includes the following steps.
[0064] Step S210, introducing a silicon source, a carbon source, and an N-type doping source, such as at least one of nitrogen (N2) and ammonia (NH3), to grow an N-type silicon carbide layer (e.g., Figure 2 In this process, a carrier gas (such as hydrogen) may be introduced into the epitaxial chamber, and the thickness of the grown N-type silicon carbide layer may be 1 μm-3 μm, and the doping concentration may be, for example, 5E16 / cm 3 -1E18 / cm 3 .
[0065] Step S220, introducing etching gas, such as hydrogen chloride (HCl), to etch the surface of the N-type silicon carbide layer. During this process, a carrier gas (such as hydrogen) may be continuously introduced, and the treatment time of the hydrogen chloride gas may be, for example, 1 min to 50 min.
[0066] Step S230, introducing a silicon source, a carbon source, and an N-type doping source, such as at least one of nitrogen (N2) and ammonia (NH3), to grow an N-type interface layer (e.g., Figure 2The thickness of the N-type interface layer is less than the thickness of the N silicon carbide layer, for example, the growth thickness of the N-type interface layer is 10nm-500nm; the doping concentration of the N-type interface layer can also be lower than the doping concentration of the N silicon carbide layer, for example, the concentration of the N-type interface layer is 5E15 / cm 3 -1E18 / cm 3 .
[0067] Step S240, introducing etching gas, such as hydrogen chloride gas (HCl), to etch the surface of the N-type interface layer and weaken the N-type doping atmosphere in the epitaxial chamber. During this process, a carrier gas (such as hydrogen) can be continuously introduced, and the time for introducing the etching gas can be controlled to be 1 min-50 min.
[0068] Step S250, introducing a P-type doping source to grow a P-type interface layer (eg, Figure 2 The second doping type interface layer 310 shown in FIG. 1 ) may be specifically introduced with a gas containing trimethylaluminum (TMAL) to form an aluminum-rich P-type interface layer.
[0069] Step S260, introducing a silicon source, a carbon source, and a P-type doping source, such as a gas containing trimethylaluminum (TMAL), and adjusting the gas flow rates of the silicon source and the carbon source so that the carbon-silicon ratio C / SI is 1-1.5, and epitaxially growing a high-concentration P-type silicon carbide layer (e.g., Figure 2 In this process, hydrogen (H2) can be introduced as a carrier gas, and the growth thickness of the high-concentration P-type silicon carbide layer can be controlled to be 5nm-100nm, and the doping concentration is 1E17 / cm 3 -1E19 / cm 3 .
[0070] Step S270, adjusting the gas flow rates of the silicon source and the carbon source to reduce the carbon-silicon ratio C / SI, for example, the carbon-silicon ratio C / SI can be 0.8-1.3, and continuously introducing a P-type doping source (for example, TMAL) to epitaxially grow a medium-concentration P-type silicon carbide layer (for example, Figure 2 The second doping type silicon carbide layer 320b shown in FIG. 3 can be formed, and the growth thickness of the medium concentration P-type silicon carbide layer can be controlled to be 50nm-1000nm, and the doping concentration thereof can be 1E17 / cm2 relative to the high concentration P-type silicon carbide layer. 3 -1E19 / cm 3 within the range of .
[0071] Step S280, adjusting the gas flow rates of the silicon source and the carbon source to further reduce the carbon-to-silicon ratio C / SI, for example, to reduce the carbon-to-silicon ratio C / SI within the range of 0.8-1.3, and continuously introducing a P-type doping source (for example, TMAL) to epitaxially grow a low-concentration P-type silicon carbide layer (for example, Figure 2 The second doped type silicon carbide layer 320c shown in FIG. 3 has a growth thickness of, for example, 50 nm to 1000 nm, and a doping concentration of 1E17 / cm2 relative to the medium concentration P-type silicon carbide layer. 3 -1E19 / cm 3 within the range of .
[0072] In this embodiment, when epitaxially growing the P-type silicon carbide layer, no nitrogen-containing gas (for example, no ammonia gas and nitrogen gas) is introduced, thereby preventing the nitrogen element from diffusing in the P-type silicon carbide layer.
[0073] The present disclosure also provides a silicon carbide epitaxial wafer, on which a first doping type epitaxial layer and a second doping type epitaxial layer are formed, and a clear interface is provided between the first doping type epitaxial layer and the second doping type epitaxial layer.
[0074] For details, please refer to Figure 2 As shown, the silicon carbide epitaxial wafer includes: a substrate 100, a first doping type epitaxial layer 200 and a second doping type epitaxial layer 300 sequentially formed on the substrate 100. The second doping type epitaxial layer 300 includes: a second doping type interface layer 310 having a first concentration, the second doping type interface layer 310 is grown on the first doping type epitaxial layer 200; and at least one second doping type silicon carbide layer (e.g. Figure 2 In the embodiment, there are three second doped type silicon carbide layers 320a / 320b / 320c), and the doping concentration of the second doped type silicon carbide layers is lower than the first concentration.
[0075] That is, the second doping type interface layer 310 has a higher concentration, so that the interface layer can effectively block the first doping type doping element (for example, nitrogen element) thereunder from diffusing upward, so that there is a clear interface between the first doping type epitaxial layer 200 and the second doping type epitaxial layer 300. In a specific example, the second doping type epitaxial layer 300 is, for example, a P-type epitaxial layer, and the second doping type interface layer 310 is, for example, an aluminum-rich layer or a boron-rich layer.
[0076] Furthermore, at least two layers of second doped type silicon carbide layers may be grown on the second doped type interface layer 310, and the doping concentration decreases from bottom to top, so as to form a concentration buffer from high doping to low doping. The doping concentration of at least two layers of second doped type silicon carbide layers may be 1E17 / cm 3 -1E19 / cm3 The gradient decreases within the region.
[0077] In a specific example, the thickness of the second doped type silicon carbide layer at the bottom layer may be the smallest. Figure 2 For example, a high-concentration second doped type silicon carbide layer 320a, a medium-concentration second doped type silicon carbide layer 320b and a low-concentration second doped type silicon carbide layer 320c are sequentially grown on the second doped type interface layer 310, wherein the high-concentration second doped type silicon carbide layer 320a has the smallest thickness, for example, the high-concentration second doped type silicon carbide layer 320a can have a thickness of 5nm-100nm, and the medium-concentration second doped type silicon carbide layer 320b and the low-concentration second doped type silicon carbide layer 320c can have a thickness of 50nm-1000nm.
[0078] Continue to refer Figure 2 As shown, the first doping type epitaxial layer 200 includes: a first doping type silicon carbide layer 210 and a first doping type interface layer 220 grown on the first doping type silicon carbide layer 210, and the thickness of the first doping type interface layer 220 is less than the thickness of the first doping type silicon carbide layer 210. The thickness of the first doping type silicon carbide layer 210 is, for example, 1 μm-3 μm, and the thickness of the first doping type interface layer 220 is, for example, 10 nm-500 nm.
[0079] Specifically, the lattice quality of the first doping type interface layer 220 is higher than the lattice quality of the first doping type silicon carbide layer 210, and the film quality of the epitaxial layer grown on the interface layer can be correspondingly improved. In addition, the first doping type interface layer 220 can be an interface layer after chlorination treatment, so that a chloride film is easily generated on the first doping type interface layer 220, so as to use the chloride film layer to suppress the diffusion of the doping elements thereunder, and further improve the interface clarity between the epitaxial layers of different doping types.
[0080] In summary, in the silicon carbide epitaxial wafer and the preparation method thereof provided by the present disclosure, before epitaxially growing epitaxial layers of different doping types, the surface of the front epitaxial layer is etched with an etching gas. In this process, the etching gas can also weaken the doping atmosphere formed by the previous doping in the epitaxial chamber, weaken the background memory effect, effectively improve the interface clarity between the epitaxial layers of different doping types grown epitaxially, and effectively improve the quality of the epitaxially grown film layer. In addition, based on the preparation method provided by the present disclosure, epitaxial layers of different doping types can also be allowed to grow in the same epitaxial chamber, which is conducive to reducing costs and improving production efficiency.
[0081] The present disclosure also provides a semiconductor device (e.g., a silicon carbide device), which includes the silicon carbide epitaxial wafer as described above, or a silicon carbide epitaxial wafer formed by the method as described above; and a device structure is also formed on the silicon carbide epitaxial wafer. Since the silicon carbide epitaxial wafer has a high quality, the device performance of the semiconductor device can be optimized accordingly.
[0082] It should be noted that the various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments, and the same and similar parts between the various embodiments can be referred to each other. Also, although the present invention has been disclosed as above with preferred embodiments, the above embodiments are not intended to limit the present invention. For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments of equivalent changes. Therefore, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of protection of the technical solution of the present invention.
[0083] It should also be recognized that, unless otherwise specified or indicated, the terms "first", "second", "third", etc. in the specification are only used to distinguish between various components, elements, steps, etc. in the specification, and are not used to indicate the logical relationship or sequential relationship between various components, elements, steps, etc. It should also be understood that the singular forms "a" and "an" used herein and in the appended claims include plural references unless the context clearly indicates otherwise. For example, a reference to "a step" or "a device" means a reference to one or more steps or devices, and may include secondary steps and secondary devices.
Claims
1. A method for preparing a silicon carbide epitaxial wafer, characterized in that: include: Providing a substrate, and sequentially growing a first doping type epitaxial layer and a second doping type epitaxial layer on the substrate, wherein the first doping type epitaxial layer is an N-type epitaxial layer, and the second doping type epitaxial layer is a P-type epitaxial layer; Wherein, the method for growing the second doping type epitaxial layer includes: Passing a chlorine-containing etching gas to etch the surface of the first doping type epitaxial layer and form a chloride film on the surface of the first doping type epitaxial layer, wherein the chloride film is used to inhibit diffusion of doping elements below the chloride film; A second doping type doping source is introduced to form a second doping type interface layer having a first concentration on the first doping type epitaxial layer, wherein the second doping type doping source is a P-type doping doping source, and the second doping type interface layer is an aluminum-rich P-type interface layer, and the second doping type interface layer is used to suppress the diffusion of the doping element of the first doping type epitaxial layer; and At least one second doping type silicon carbide layer having a doping concentration lower than the first doping concentration is epitaxially grown on the second doping type interface layer.
2. The method for preparing a silicon carbide epitaxial wafer according to claim 1, characterized in that: The method for epitaxially growing the first doping type epitaxial layer comprises: A silicon source, a carbon source and a doping source of a first doping type are introduced to epitaxially grow a first doping type silicon carbide layer on the substrate.
3. The method for preparing a silicon carbide epitaxial wafer according to claim 2, characterized in that: The method for epitaxially growing the first doping type epitaxial layer further includes: introducing an etching gas to etch the surface of the first doped type silicon carbide layer; and, A silicon source, a carbon source and a first doping type doping source are introduced to grow a first doping type interface layer on the first doping type silicon carbide layer, wherein the thickness of the first doping type interface layer is less than the thickness of the first doping type silicon carbide layer.
4. The method for preparing a silicon carbide epitaxial wafer according to claim 3, characterized in that: The thickness of the first doping type silicon carbide layer is 1 μm-3 μm; and / or the thickness of the first doping type interface layer is 10 nm-500 nm.
5. The method for preparing a silicon carbide epitaxial wafer according to claim 3, characterized in that: The etching gas used when growing the first doping type epitaxial layer includes chlorine-containing gas.
6. The method for preparing a silicon carbide epitaxial wafer according to claim 1, characterized in that: The method for forming the second doping type interface layer includes: introducing at least one gas containing trimethylaluminum and aluminum hydride to form an aluminum-rich layer to constitute the second doping type interface layer.
7. The method for preparing a silicon carbide epitaxial wafer according to claim 1, characterized in that: At least two second doped type silicon carbide layers with doping concentrations decreasing from bottom to top are grown on the second doped type interface layer.
8. The method for preparing a silicon carbide epitaxial wafer according to claim 7, characterized in that: The method for growing the at least two second doped type silicon carbide layers comprises: adjusting the silicon source and the carbon source so that the carbon-silicon ratio decreases successively, so that the doping concentration gradient of the at least two second doped type silicon carbide layers grown decreases.
9. The method for preparing a silicon carbide epitaxial wafer according to claim 7, characterized in that: Among the at least two second-doped type silicon carbide layers, the second-doped type silicon carbide layer of the bottom layer has the smallest thickness.
10. The method for preparing a silicon carbide epitaxial wafer according to any one of claims 1 to 9, characterized in that: The first doping type epitaxial layer and the second doping type epitaxial layer are grown in the same epitaxial chamber.
11. A silicon carbide epitaxial wafer, characterized in that: include: A substrate, a first doping type epitaxial layer and a second doping type epitaxial layer sequentially formed on the substrate, wherein the first doping type epitaxial layer is an N-type epitaxial layer, and the second doping type epitaxial layer is a P-type epitaxial layer; Wherein, a chloride film is formed on the surface of the first doping type epitaxial layer, and the chloride film is used to suppress the diffusion of the doping element under the chloride film; The second doping type epitaxial layer comprises: A second doping type interface layer having a first concentration, the second doping type interface layer is grown on the first doping type epitaxial layer, the second doping type interface layer is an aluminum-rich P-type interface layer, and the second doping type interface layer is used to suppress the diffusion of the doping element of the first doping type epitaxial layer; At least one second doping type silicon carbide layer, wherein the doping concentration of the second doping type silicon carbide layer is lower than the first concentration and is grown on the second doping type interface layer.
12. The silicon carbide epitaxial wafer according to claim 11, characterized in that: The first doping type epitaxial layer includes: a first doping type silicon carbide layer and a first doping type interface layer grown on the first doping type silicon carbide layer, and the thickness of the first doping type interface layer is smaller than the thickness of the first doping type silicon carbide layer.
13. The silicon carbide epitaxial wafer according to claim 12, characterized in that: The thickness of the first doping type silicon carbide layer is 1 μm-3 μm; and / or the thickness of the first doping type interface layer is 10 nm-500 nm.
14. The silicon carbide epitaxial wafer according to claim 11, characterized in that: The second doping type epitaxial layer includes: at least two second doping type silicon carbide layers whose doping concentration decreases gradually from bottom to top.
15. The silicon carbide epitaxial wafer according to claim 14, characterized in that: Among the at least two second-doped type silicon carbide layers, the second-doped type silicon carbide layer of the bottom layer has the smallest thickness.
16. A semiconductor device, characterized in that: include: Obtaining a silicon carbide epitaxial wafer by the method according to any one of claims 1 to 10, or providing a silicon carbide epitaxial wafer according to any one of claims 11 to 15; as well as, A device structure is formed on the silicon carbide epitaxial wafer.