A lithium metal battery and a method for preparing the same

By using inorganic nanomaterials and polyvinylidene fluoride-hexafluoropropylene copolymer to prepare nanofiber separators in lithium metal batteries, and combining in-situ polymerization processes to construct polymer solid electrolytes, the problem of interface inhomogeneity in lithium metal batteries is solved. The cycle performance and capacity retention rate of the battery are improved, and high energy density and mechanical stability are achieved.

CN118248957BActive Publication Date: 2024-10-22SVOLT ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410642953.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-23
Publication Date
2024-10-22
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

The original solid electrolyte interface of lithium metal batteries is uneven, resulting in inhomogeneous ion diffusion and lithium dendrites, which affects battery capacity retention and safety. Moreover, the polymer solid electrolyte produced by traditional preparation methods has poor compatibility with the electrode interface, making it difficult to achieve high energy. density.

Method used

Inorganic nanomaterials and polyvinylidene fluoride-hexafluoropropylene copolymer are used to prepare nanofiber separators, combined with in-situ polymerization process to construct polymer solid electrolytes in lithium metal batteries, improve interfacial compatibility and ionic conductivity, and contain Pyrrolidine-based ionic liquids of tetrafluoroborate or hexafluorophosphate achieve homogenization of the lithium deposition path.

Benefits of technology

It significantly improves the cycle performance and capacity retention rate of lithium metal batteries, enhances the mechanical stability and ion transmission efficiency of the battery, achieves the "electrostatic shielding effect", and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_20
    Figure SMS_20
  • Figure QLYQS_1
    Figure QLYQS_1
  • Figure QLYQS_2
    Figure QLYQS_2
Patent Text Reader

Abstract

The present invention relates to the field of battery technology, and in particular to a lithium metal battery and a preparation method thereof. The preparation method of a lithium metal battery comprises the following steps: assembling a battery cell in a manner of stacking a positive electrode sheet, a nanofiber separator and a negative electrode sheet in sequence; the nanofiber separator comprises an inorganic nanomaterial and a polyvinylidene fluoride-hexafluoropropylene copolymer; injecting a polymer precursor solution into the battery cell, and sequentially standing and reacting to obtain a lithium metal battery; the polymer precursor solution comprises an ionic liquid, a plasticizer, a lithium salt and a monomer; the ionic liquid comprises at least one of a pyrrolidyl ionic liquid containing tetrafluoroborate or hexafluorophosphate; the monomer comprises an acrylate crosslinker monomer and / or an epoxy crosslinker monomer. The preparation method enhances the ionic conductivity and mechanical stability of the separator; improves the ionic conductivity, ion migration number and interface compatibility of the electrolyte; helps to uniformly deposit lithium; and thus improves the cycle performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a lithium metal battery and a preparation method thereof. Background Art

[0002] In recent years, lithium metal batteries with lithium metal as the negative electrode have attracted widespread attention. Because lithium metal has an extremely high theoretical specific capacity and a low electrochemical potential, it is very suitable for high-nickel ternary positive electrode LiNi x Co y Mn 1-x-y O 2 The battery composed of (NCM, x ≥ 0.8) combination is expected to provide a high energy density of more than 500Wh / kg and is one of the most promising candidates for the next generation of high-energy batteries.

[0003] Lithium metal is highly reactive and can directly initiate chemical reactions when in contact with the electrolyte, forming a solid electrolyte interface (SEI) at the interface. However, the original SEI layer is heterogeneous and inhomogeneous in composition and structure, which can cause inhomogeneous ion diffusion and initial lithium nucleation, ultimately leading to the so-called lithium dendrites. In addition, the original SEI layer is brittle and its mechanical strength is insufficient to withstand the volume change of the lithium metal anode and the invasion of lithium dendrites, which leads to the formation of a new SEI, causing irreversible loss of battery capacity and a series of safety issues, thus limiting its development.

[0004] Using non-flammable, environmentally friendly, and mechanically sound solid electrolytes to replace traditional electrolytes is an effective solution. Solid electrolytes are generally divided into inorganic solid electrolytes and organic polymer solid electrolytes. Compared with inorganic solid electrolytes, organic polymer solid electrolytes are cheap and easy to obtain, and have great advantages in flexibility, so they show great application potential in lithium metal batteries.

[0005] The traditional method for preparing polymer solid electrolytes is to cast the polymer precursor solution on a mold, and obtain a polymer solid electrolyte (SPE) membrane with the desired thickness after free radical-induced polymerization; however, the SPE prepared by this process has poor solid-solid interface compatibility with the electrode, and the prepared SPE membrane is too thick to achieve high energy density. Constructing a polymer solid electrolyte inside the battery enhances the interfacial contact between the electrolyte and the electrode to achieve effective lithium ion transmission inside the porous positive electrode; however, in this method, cellulose, glass fiber, polyolefin or similar polymers are used as diaphragms, which are inert and usually do not participate in the ion conduction process, and some monomer-containing liquid electrolytes have poor wettability on these diaphragms. In addition, polymer solid electrolytes constructed based on conventional free radical reactions will leave some unreacted monomers or initiators inside the closed battery. These substances have strong chemical reactivity and are easily affected by voltage, resulting in serious parasitic interface reactions.

[0006] In view of this, this invention is proposed. Summary of the invention

[0007] The first object of the present invention is to provide a method for preparing a lithium metal battery, which enhances the ionic conductivity and mechanical stability of the separator and promotes Li + transport; improved the interfacial compatibility between polymer solid electrolyte and electrode; increased the ionic conductivity and ion migration number of polymer solid electrolyte; helped to homogenize the lithium deposition path and achieve the "electrostatic shielding effect".

[0008] A second object of the present invention is to provide a lithium metal battery having excellent cycle performance.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] The present invention provides a method for preparing a lithium metal battery, comprising the following steps:

[0011] S1. Assemble a battery cell by stacking a positive electrode sheet, a nanofiber separator and a negative electrode sheet in sequence; the nanofiber separator comprises an inorganic nanomaterial and a polyvinylidene fluoride-hexafluoropropylene copolymer;

[0012] S2, injecting a polymer precursor solution into the battery cell, and sequentially allowing the solution to stand and react to obtain the lithium metal battery; the polymer precursor solution includes an ionic liquid, a plasticizer, a lithium salt and a monomer;

[0013] The ionic liquid includes at least one of a pyrrolidinyl ionic liquid containing tetrafluoroborate or hexafluorophosphate;

[0014] The monomer includes at least one of the compounds having a structure as shown in formula (III) or formula (IV);

[0015] (III); (IV); wherein c is an integer between 1 and 9, and d is an integer between 0 and 9.

[0016] Furthermore, the inorganic nanomaterial includes SiO 2 、Al 2 O 3 、ZrO 2 and Li 7 La 3 Zr 2 O 12 At least one of;

[0017] And / or, the mass ratio of the inorganic nanomaterial to the polyvinylidene fluoride-hexafluoropropylene copolymer is (0.5-3): (7-9.5).

[0018] Further, the ionic liquid includes at least one of the compounds having a structure as shown in formula (I) or formula (II);

[0019] (I); (II); wherein a is an integer between 1 and 9, and b is an integer between 1 and 9.

[0020] Further, the plasticizer includes at least one of succinonitrile, acetonitrile, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, ethylene glycol diethyl ether, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate.

[0021] Furthermore, the volume ratio of the ionic liquid to the plasticizer is 1:(1-5).

[0022] Further, the lithium salt includes at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(pentafluoroethanesulfonyl)imide, lithium hexafluorophosphate, lithium difluorooxalatoborate, lithium bis(oxalatoborate), lithium difluorobis(oxalatophosphate) and lithium difluorophosphate;

[0023] And / or, in the polymer precursor solution, the concentration of lithium salt is 0.5-2 mol / L.

[0024] Furthermore, in the polymer precursor solution, the volume percentage of the monomer is 16% to 50%.

[0025] Furthermore, the standing temperature is 20-30°C, and the standing time is 10-24h;

[0026] And / or, the reaction temperature is 60-100° C., and the reaction time is 10-30 min.

[0027] Furthermore, the positive electrode material in the positive electrode plate includes at least one of lithium iron phosphate, lithium iron manganese phosphate, lithium manganese oxide and lithium nickel cobalt manganese oxide;

[0028] And / or, the negative electrode plate includes a lithium-copper composite strip with metallic lithium or lithium alloy disposed on both sides.

[0029] The present invention also provides a lithium metal battery, which is prepared by the lithium metal battery preparation method as described above.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] 1. The preparation method of the lithium metal battery of the present invention directly adopts an in-situ polymerization process inside the battery to prepare a polymer solid electrolyte, thereby improving the interface compatibility between the polymer solid electrolyte and the electrode and improving the solid-solid interface contact.

[0032] 2. The present invention uses inorganic nanomaterials and PVDF-HFP as a nanofiber diaphragm prepared by electrospinning, which can promote Li + transport while providing ionic conductivity and mechanical stability.

[0033] 3. The polymer precursor solution of the present invention includes an ionic liquid, a plasticizer, a lithium salt and a monomer, and an in-situ cationic polymerization reaction occurs under heating conditions to generate a polymer solid electrolyte; wherein, the use of a pyrrolidone ionic liquid containing tetrafluoroborate or hexafluorophosphate helps to homogenize the lithium deposition path and achieve an "electrostatic shielding effect"; the plasticizer is beneficial to improving the ionic conductivity and ion migration number of the polymer solid electrolyte.

[0034] 4. The lithium metal battery prepared by the preparation method of the lithium metal battery of the present invention has excellent cycle performance and greatly improves the capacity retention rate. DETAILED DESCRIPTION

[0035] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0036] In some embodiments of the present invention, a method for preparing a lithium metal battery is provided, comprising the following steps:

[0037] S1. Assemble a battery cell by stacking a positive electrode sheet, a nanofiber separator and a negative electrode sheet in sequence; the nanofiber separator includes an inorganic nanomaterial and polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP);

[0038] S2, injecting a polymer precursor solution into a battery cell, and sequentially allowing the solution to stand and react to obtain a lithium metal battery; the polymer precursor solution includes an ionic liquid, a plasticizer, a lithium salt, and a monomer;

[0039] The ionic liquid includes at least one of a pyrrolidinyl ionic liquid containing tetrafluoroborate or hexafluorophosphate;

[0040] The monomer includes at least one of the compounds having a structure as shown in formula (III) or formula (IV);

[0041] (III); (IV); wherein c is an integer between 1 and 9, and d is an integer between 0 and 9.

[0042] In the preparation method of the lithium metal battery of the present invention, an in-situ polymerization process is adopted to directly construct a polymer solid electrolyte inside the battery, which greatly enhances the interface compatibility between the polymer solid electrolyte and the electrode and effectively improves the solid-solid interface contact.

[0043] The nanofiber membrane made of inorganic nanomaterials as active fillers and PVDF-HFP fiber membrane as the matrix is ​​used as the support of the polymer electrolyte; the inorganic nanomaterials can interact with lithium salts through Lewis acid-base interactions, promoting the dissociation of lithium salts and thus promoting Li + transmission; PVDF-HFP fiber membrane serves as a framework for supporting polymer solid electrolytes, which has sufficient electrolyte wetting and absorption capabilities while providing ionic conductivity and mechanical stability.

[0044] The polymer precursor solution includes a pyrrolidino ionic liquid (Py + BF 4 - / Py + PF 6 - ), plasticizer, lithium salt and monomer, which undergo in-situ cationic polymerization to generate a polymer solid electrolyte; during the reaction, Li + Will react with BF in ionic liquids 4 - / PF6 - Decomposition reaction occurs, producing strong Lewis acid BF 3 / PF 5 , inducing the monomer to undergo in situ cationic polymerization; and the pyrrolidine cation Py - It can neutralize the radiation electric field and help to homogenize the lithium deposition path, achieving the "electrostatic shielding effect". - With ratio + A lower reduction potential can ensure the electrochemical stability of the interface.

[0045] Plasticizers are beneficial to increasing the concentration and activity of free lithium ions in polymer solid electrolytes, thereby improving the ionic conductivity and ion transference number of polymer solid electrolytes.

[0046] In some embodiments of the present invention, the inorganic nanomaterial comprises SiO 2 、Al 2 O 3 、ZrO 2 and Li 7 La 3 Zr 2 O 12 At least one of the following:

[0047] In some embodiments of the present invention, the particle size of the inorganic nanomaterial is ≥100 nm and <1000 nm.

[0048] In some embodiments of the present invention, the mass ratio of the inorganic nanomaterial and the polyvinylidene fluoride-hexafluoropropylene copolymer is (0.5~3):(7~9.5); typically but not limitatively, for example, the mass ratio of the inorganic nanomaterial and the polyvinylidene fluoride-hexafluoropropylene copolymer can be 0.5:9.5, 1:9, 1.5:8.5, 2:8, 2.5:7.5, 3:7 or a range of any two thereof.

[0049] If the content of inorganic nanomaterials in the nanofiber separator is too much, particle agglomeration will occur, resulting in reduced ion conductivity and reduced flexibility and adhesion of the polymer; if the content of inorganic nanomaterials is too little, the effect will be weak and the shear modulus of the polymer will be low, making it difficult to block lithium dendrites.

[0050] In some embodiments of the present invention, the thickness of the nanofiber membrane is 15-50 μm; typically but not limiting, for example, the thickness of the nanofiber membrane can be 15 μm, 25 μm, 35 μm, 45 μm, 50 μm or a range of any two thereof.

[0051] In some embodiments of the present invention, the method for preparing the nanofiber membrane comprises electrospinning.

[0052] In some embodiments of the present invention, a method for preparing a nanofiber membrane comprises the following steps:

[0053] The spinning solution containing inorganic nanomaterials and polyvinylidene fluoride-hexafluoropropylene copolymer is subjected to electrostatic spinning, and then dried and hot-pressed in sequence to obtain a nanofiber separator.

[0054] In some embodiments of the present invention, the mass percentage of the polyvinylidene fluoride-hexafluoropropylene copolymer in the spinning solution is 15% to 25%.

[0055] In some embodiments of the present invention, the solvent in the spinning solution includes at least one of N,N-dimethylformamide, N-methylpyrrolidone, dimethylacetamide and acetone.

[0056] In some embodiments of the present invention, the parameters of electrospinning are: voltage of 10~30kV, distance between the receiving tube and the needle of 10~30cm, inner diameter of the needle of 0.2~1mm, flow rate of spinning solution of 0.01~0.2mL / min, and rotation speed of the receiving tube of 300~1000rpm.

[0057] In some embodiments of the present invention, the drying temperature is 70-90°C.

[0058] In some embodiments of the present invention, the temperature of hot pressing is 100-150° C. and the pressure is 0.1-0.5 MPa.

[0059] In some embodiments of the present invention, the ionic liquid includes at least one of the compounds having a structure as shown in formula (I) or formula (II);

[0060] (I); (II); wherein a is an integer between 1 and 9, and b is an integer between 1 and 9.

[0061] In some embodiments of the present invention, the ionic liquid comprises at least one of the following compounds;

[0062] (CAS No.: 117947-85-0); (CAS No.: 327022-59-3); (CAS No.: 345974-11-4); (CAS No.: 327022-58-2); (CAS No.: 330671-29-9).

[0063] In some embodiments of the present invention, the plasticizer includes at least one of succinonitrile, acetonitrile, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, ethylene glycol diethyl ether, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate.

[0064] In some embodiments of the present invention, the volume ratio of the ionic liquid to the plasticizer is 1:(1-5); typically but not limiting, for example, the volume ratio of the ionic liquid to the plasticizer can be 1:1, 1:2, 1:3, 1:4, 1:5 or a range of any two thereof.

[0065] Li in polymer precursor solution system + Will be with BF on ionic liquid 4 - / PF 6 - Decomposition reaction occurs, producing strong Lewis acid BF 3 / PF 5 , inducing the monomer to undergo in situ cationic polymerization. If the content is low, it will lead to incomplete monomer polymerization; and if the content is high, it will lead to lower ionic conductivity of the polymer electrolyte.

[0066] In some embodiments of the present invention, the lithium salt includes at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(pentafluoroethanesulfonyl)imide, lithium hexafluorophosphate, lithium difluorooxalatoborate, lithium bis(oxalatoborate), lithium difluorobis(oxalatophosphate) and lithium difluorophosphate.

[0067] In some embodiments of the present invention, the concentration of the lithium salt in the polymer precursor solution is 0.5~2 mol / L; typically but not limitatively, for example, the concentration of the lithium salt in the polymer precursor solution can be 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L or a range of any two thereof.

[0068] In some embodiments of the present invention, the monomers include acrylate crosslinking agent monomers and / or epoxy crosslinking agent monomers; and the monomers are capable of undergoing cationic polymerization.

[0069] In some embodiments of the present invention, the monomer comprises at least one of the following compounds;

[0070] (CAS No.: 2274-11-5);

[0071] (CAS No.: 4074-88-8);

[0072] (CAS No.: 1680-21-3);

[0073] (CAS No.: 2238-07-5);

[0074] (CAS No.: 2224-15-9);

[0075] (CAS No.: 4206-61-5).

[0076] In some embodiments of the present invention, the volume percentage of the monomer in the polymer precursor solution is 16% to 50%; typically but not limitatively, for example, the volume percentage of the monomer in the polymer precursor solution can be 16%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range of any two thereof.

[0077] In some embodiments of the present invention, the method for preparing a polymer precursor solution comprises the following steps:

[0078] In an anhydrous and oxygen-free environment, a lithium salt, an ionic liquid and a plasticizer are mixed to obtain a composite electrolyte; a monomer is added to the composite electrolyte to obtain a polymer precursor solution; the volume ratio of the composite electrolyte to the monomer is (1-5):1; typically but not restrictively, for example, the volume ratio of the composite electrolyte to the monomer can be 1:1, 2:1, 3:1, 4:1, 5:1 or a range of any two of them.

[0079] In some embodiments of the present invention, the standing temperature is 20-30° C., and the standing time is 10-24 h.

[0080] In some embodiments of the present invention, the reaction temperature is 60-100°C, and the reaction time is 10-30 min; typically but not limiting, for example, the reaction temperature can be 60°C, 70°C, 80°C, 90°C, 100°C or a range of any two thereof.

[0081] In the preparation method of the lithium metal battery of the present invention, a polymer precursor solution is injected into a battery cell assembled in a stacked manner of a positive electrode plate, a nanofiber separator, and a negative electrode plate. After uniform infiltration, the monomer is subjected to a cationic polymerization reaction under heating conditions to obtain an in-situ self-polymerized all-solid-state polymer lithium metal battery. The in-situ self-polymerized all-solid-state polymer lithium metal battery prepared by this method has improved cyclability and safety simultaneously.

[0082] In some embodiments of the present invention, the positive electrode material in the positive electrode plate is not limited to at least one of lithium iron phosphate, lithium manganese iron phosphate, lithium manganese oxide and lithium nickel cobalt manganese oxide; the present invention does not strictly limit the type of positive electrode material, and the positive electrode material can be selected from commonly used positive electrode materials publicly known in the art;

[0083] The negative electrode plate includes a lithium-copper composite strip with metallic lithium or lithium alloy disposed on both sides.

[0084] In some embodiments of the present invention, a lithium metal battery is also provided, which is prepared using the above-mentioned method for preparing a lithium metal battery.

[0085] The lithium metal battery prepared by the preparation method of the lithium metal battery of the present invention has excellent cycle performance and greatly improves the capacity retention rate.

[0086] In some embodiments of the present invention, a lithium metal battery includes a polymer solid electrolyte and a nanofiber separator carrying the polymer solid electrolyte;

[0087] Polymer solid electrolytes are mainly obtained by in-situ polymerization initiated by cations from lithium salts, ionic liquids, plasticizers and monomers;

[0088] The nanofiber membrane is mainly obtained by electrospinning inorganic nanomaterials and polyvinylidene fluoride-hexafluoropropylene copolymer.

[0089] Example 1

[0090] The method for preparing a lithium metal battery provided in this embodiment comprises the following steps:

[0091] S1, SiO 2 and PVDF-HFP in a mass ratio of 1:9 and dispersed in a mixed solvent of N,N-dimethylformamide and acetone in a volume ratio of 7:3, wherein the mass percentage of PVDF-HFP is 18%, and magnetic stirring is performed at 60°C for 12 hours to form a uniform spinning solution; the spinning solution is electrospun on an electrospinning machine, the voltage of the electrospinning is 20 kV, a grounded aluminum foil is used as the receiving end, and the distance between the receiving tube and the needle is controlled to be 15 cm, the inner diameter of the needle is 0.2 mm, the spinning solution flow rate is 0.03 mL / min, and the speed of the receiving tube is 500 rpm, and then vacuum dried at 80°C in a vacuum oven for 12 hours, and hot pressed at 120°C and 0.3 MPa to obtain a nanofiber diaphragm with a thickness of 20 μm;

[0092] The positive electrode sheet, the nanofiber separator, and the negative electrode sheet are sequentially stacked to obtain a battery electrode group, which is assembled in an aluminum-plastic film and dried in a vacuum oven to obtain a battery cell.

[0093] S2. In a glove box, 2.81 g of lithium salt (lithium bis(trifluoromethylsulfonyl)imide), 5 mL of ionic liquid (N-ethyl-N-methylpyrrolidine tetrafluoroborate, CAS No. 117947-85-0) and 5 mL of plasticizer (succinonitrile) were stirred evenly to form a composite electrolyte; then 5 mL of monomer (ethylene glycol diacrylate, CAS No. 2274-11-5) was added and stirred evenly to obtain a polymer precursor solution;

[0094] The polymer precursor solution was injected into the battery cell, vacuum sealed and allowed to stand at 25°C for 12 hours, and then placed in an oven at 80°C for reaction for 20 minutes to obtain an in-situ self-polymerized all-solid-state polymer lithium metal battery.

[0095] Example 2

[0096] The preparation method of the lithium metal battery provided in this embodiment refers to that in embodiment 1, the only difference is that in step S1, SiO 2 Replaced by Li 7 La 3 Zr 2 O 12 .

[0097] Example 3

[0098] The preparation method of the lithium metal battery provided in this embodiment refers to that in embodiment 1, the only difference is that in step S1, SiO 2 The mass ratio of PVDF-HFP to PVDF-HFP is 3:7.

[0099] Example 4

[0100] The preparation method of the lithium metal battery provided in this embodiment refers to that in embodiment 1, except that in step S2, the ionic liquid is N-butyl-N-methylpyrrolidino hexafluorophosphate, with a CAS number of 330671-29-9.

[0101] Example 5

[0102] The preparation method of the lithium metal battery provided in this embodiment refers to that in embodiment 1, except that in step S2, the monomer is ethylene glycol diglycidyl ether, with a CAS number of 2224-15-9.

[0103] Example 6

[0104] The preparation method of the lithium metal battery provided in this embodiment refers to Example 1, except that, in step S2, 2.81 g of lithium salt (lithium bis(trifluoromethylsulfonyl)imide), 2 mL of ionic liquid (N-ethyl-N-methylpyrrolidine tetrafluoroborate, CAS No. 117947-85-0) and 8 mL of plasticizer (succinonitrile) are stirred evenly to form a composite electrolyte.

[0105] Example 7

[0106] The preparation method of the lithium metal battery provided in this embodiment refers to Example 1, except that in step S2, the volume of the monomer (ethylene glycol diacrylate, CAS No. 2274-11-5) is 3 mL.

[0107] Example 8

[0108] The method for preparing a lithium metal battery provided in this embodiment comprises the following steps:

[0109] S1, Al 2 O 3 and PVDF-HFP in a mass ratio of 2:8 and dispersed in a mixed solvent of N,N-dimethylformamide and acetone in a volume ratio of 7:3, wherein the mass percentage of PVDF-HFP is 20%, and magnetic stirring is performed at 60°C for 12 hours to form a uniform spinning solution; the spinning solution is electrospun on an electrospinning machine, the voltage of the electrospinning is 20kV, a grounded aluminum foil is used as the receiving end, and the distance between the receiving tube and the needle is controlled to be 15cm, the inner diameter of the needle is 0.2mm, the spinning solution flow rate is 0.03mL / min, and the speed of the receiving tube is 500rpm, and then vacuum dried at 80°C in a vacuum oven for 12 hours, and hot pressed at 120°C and 0.3MPa to obtain a nanofiber diaphragm with a thickness of 30μm;

[0110] The positive electrode sheet, the nanofiber separator, and the negative electrode sheet are sequentially stacked to obtain a battery electrode group, which is assembled in an aluminum-plastic film and dried in a vacuum oven to obtain a battery cell.

[0111] S2. In a glove box, 2.81 g of lithium salt (lithium difluorobisoxalate phosphate), 4 mL of ionic liquid (N-butyl-N-methylpyrrolidino tetrafluoroborate, CAS No. 345974-11-4) and 6 mL of plasticizer (triethylene glycol dimethyl ether) were stirred evenly to form a composite electrolyte; then 4 mL of monomer (triethylene glycol diacrylate, CAS No. 1680-21-3) was added and stirred evenly to obtain a polymer precursor solution;

[0112] The polymer precursor solution was injected into the battery cell, vacuum sealed and allowed to stand at 25°C for 12 hours, and then placed in an oven at 100°C for reaction for 15 minutes to obtain an in-situ self-polymerized all-solid-state polymer lithium metal battery.

[0113] Comparative Example 1

[0114] The preparation method of the lithium metal battery provided in this comparative example refers to Example 1, except that the nanofiber separator is replaced by a PE film with a thickness of 12 μm.

[0115] Comparative Example 2

[0116] The preparation method of the lithium metal battery provided in this comparative example refers to Example 1, except that in step S1, SiO 2 , that is, PVDF-HFP is dispersed in a mixed solvent of N,N-dimethylformamide and acetone with a volume ratio of 7:3.

[0117] Comparative Example 3

[0118] The preparation method of the lithium metal battery provided in this comparative example refers to Example 1, except that, in step S2, 2.81 g of lithium salt (lithium bis(trifluoromethylsulfonyl)imide) and 10 mL of ionic liquid (N-ethyl-N-methylpyrrolidine tetrafluoroborate, CAS No. 117947-85-0) are stirred evenly to form a composite electrolyte.

[0119] Comparative Example 4

[0120] The preparation method of the lithium metal battery provided in this comparative example refers to Example 1, except that in step S2, the ionic liquid is an imidazole ionic liquid (Im + BF 4 - ), replacing N-ethyl-N-methylpyrrolidine tetrafluoroborate with 1-methylimidazole tetrafluoroborate (CAS No. 151200-14-5).

[0121] Comparative Example 5

[0122] The preparation method of the lithium metal battery provided in this comparative example comprises the following steps:

[0123] S1. In a glove box, 2.81 g of lithium salt (lithium bis(trifluoromethylsulfonyl)imide), 5 mL of ionic liquid (N-ethyl-N-methylpyrrolidine tetrafluoroborate, CAS No. 117947-85-0) and 5 mL of plasticizer (succinonitrile) were stirred evenly to form a composite electrolyte; then 5 mL of monomer (ethylene glycol diacrylate, CAS No. 2274-11-5) was added and stirred evenly to obtain a polymer precursor solution;

[0124] The polymer precursor solution was poured into a polytetrafluoroethylene plate, and then placed in an oven at 80° C. to react for 20 min to obtain a polymer electrolyte membrane.

[0125] S2. Assemble a battery electrode group by stacking the positive electrode sheet, the polymer electrolyte membrane, and the negative electrode sheet in sequence, assemble the battery electrode group in an aluminum-plastic film, and dry it in a vacuum oven. After drying, vacuum seal it to obtain a lithium metal battery.

[0126] Test Example 1

[0127] The performance of lithium metal batteries prepared by the preparation methods of lithium metal batteries of Examples 1 to 8 and Comparative Examples 1 to 5 were tested, and the results are shown in Table 1.

[0128] The preparation method of the positive electrode sheet in the lithium metal battery includes: a ternary positive electrode material LiNi 0.83 Co 0.12 Mn 0.05 O 2 , conductive agent Super P, binder PVDF and carbon nanotubes CNT were mixed evenly in a mass ratio of 97.8:0.75:1.2:0.25 to form a slurry, which was then coated on the aluminum foil current collector to control the surface density to 23.5 mg / cm 2 After drying, the product is rolled, slit and cut into pieces to obtain the positive electrode sheet of a lithium metal battery.

[0129] The invention discloses a method for preparing a negative electrode sheet in a lithium metal battery, comprising: cutting a lithium copper composite strip with 50 μm metal lithium on both sides into sheets to obtain a lithium metal negative electrode sheet.

[0130] Performance test: Use the Blue Electric charge and discharge tester to test the cycle performance of each lithium metal battery at 25°C. First, charge the battery at 0.2C constant current to 4.25V, then charge it at 4.25V at constant voltage to 0.05C, let it stand for 30 minutes, and then discharge it at 1C constant current to 2.5V. The capacity is recorded as C. 0 After 200 cycles of this procedure, the capacity is recorded as C 1 , then the capacity retention rate = (C 1 / C 0 )×100%.

[0131] Table 1

[0132]

[0133] It can be seen from Table 1 that the all-solid-state polymer lithium metal battery prepared by the preparation method of the lithium metal battery of the present invention has significantly improved cycle performance and has excellent capacity retention rate.

[0134] The present invention adopts an in-situ polymerization process to make the polymer solid electrolyte and the electrode have better interface compatibility, effectively improving the solid-solid interface contact; the PVDF-HFP fiber membrane prepared by electrospinning has sufficient electrolyte wetting and absorption capacity, and can also provide ionic conductivity and mechanical stability; the pyrrolidine cation Py in the ionic liquid of the polymer precursor solution - It can neutralize the radiation electric field and help to homogenize the lithium deposition path, achieving an "electrostatic shielding effect".

[0135] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a lithium metal battery, characterized in that: The steps include: S1. Assemble a battery cell by stacking a positive electrode sheet, a nanofiber separator and a negative electrode sheet in sequence; the nanofiber separator comprises an inorganic nanomaterial and a polyvinylidene fluoride-hexafluoropropylene copolymer; S2, injecting a polymer precursor solution into the battery cell, and sequentially allowing the solution to stand and react to obtain the lithium metal battery; the polymer precursor solution includes an ionic liquid, a plasticizer, a lithium salt and a monomer; The ionic liquid includes at least one of a pyrrolidinyl ionic liquid containing tetrafluoroborate or hexafluorophosphate; The monomer includes at least one of the compounds having a structure as shown in formula (III) or formula (IV); (III); (IV); wherein c is an integer between 1 and 9, and d is an integer between 0 and 9; The inorganic nanomaterials include SiO2, Al2O3, ZrO2 and Li7La3Zr2O 12 At least one of; The mass ratio of the inorganic nanomaterial to the polyvinylidene fluoride-hexafluoropropylene copolymer is (0.5-3): (7-9.5); The volume ratio of the ionic liquid to the plasticizer is 1:(1-5).

2. The method for preparing a lithium metal battery according to claim 1, characterized in that: The ionic liquid includes at least one of the compounds having a structure as shown in formula (I) or formula (II); (I); (II); wherein a is an integer between 1 and 9, and b is an integer between 1 and 9.

3. The method for preparing a lithium metal battery according to claim 1, characterized in that: The plasticizer includes at least one of succinonitrile, acetonitrile, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, ethylene glycol diethyl ether, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate.

4. The method for preparing a lithium metal battery according to claim 1, characterized in that: The lithium salt comprises at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium bis(pentafluoroethanesulfonyl)imide, lithium hexafluorophosphate, lithium difluorooxalatoborate, lithium bis(oxalatoborate), lithium difluorobis(oxalatophosphate) and lithium difluorophosphate; And / or, in the polymer precursor solution, the concentration of lithium salt is 0.5-2 mol / L.

5. The method for preparing a lithium metal battery according to claim 1, characterized in that: In the polymer precursor solution, the volume percentage of the monomer is 16% to 50%.

6. The method for preparing a lithium metal battery according to claim 1, characterized in that: The standing temperature is 20-30°C, and the standing time is 10-24h; And / or, the reaction temperature is 60-100° C., and the reaction time is 10-30 min.

7. The method for preparing a lithium metal battery according to claim 1, characterized in that: The positive electrode material in the positive electrode plate includes at least one of lithium iron phosphate, lithium iron manganese phosphate, lithium manganese oxide and lithium nickel cobalt manganese oxide; And / or, the negative electrode plate includes a lithium-copper composite strip with metallic lithium or lithium alloy disposed on both sides.

8. A lithium metal battery, characterized in that: The lithium metal battery is prepared by the preparation method of any one of claims 1 to 7.