A method for efficiently converting zinc and organic sulfur in zinc-containing waste resin into stable compounds using a mixed molten salt and its oxidation treatment of waste cation exchange resin.

By treating waste cation exchange resin with a mixed molten salt system of binary molten carbonate and potassium hydroxide, stable sulfur compounds and oxides are formed, which solves the problem of low retention efficiency of zinc and sulfur in waste resin and achieves efficient and safe waste resin treatment.

CN118255383BActive Publication Date: 2026-11-17烟台哈尔滨工程大学研究院
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410227729.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-29
Publication Date
2026-11-17
Estimated Expiration
2044-02-29

AI Technical Summary

Technical Problem

Existing technologies have limited absorption capacity for sulfur-containing gases and retention efficiency for zinc and sulfur when treating waste cation exchange resins, resulting in environmental pollution risks and low treatment efficiency.

Method used

A mixed molten salt system of binary molten carbonate and potassium hydroxide was used to heat-treat zinc-containing waste resin, forming stable sulfur compounds and oxides, thereby improving the fixation rate of zinc and sulfur.

Benefits of technology

It significantly improves the retention rates of zinc and sulfur, reduces the emissions of hydrogen sulfide and sulfur dioxide, and achieves efficient and safe waste resin treatment, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118255383B_ABST
    Figure CN118255383B_ABST
Patent Text Reader

Abstract

This invention discloses a mixed molten salt capable of efficiently converting zinc and organic sulfur in zinc-containing waste resin into stable compounds, and a method for oxidizing waste cation exchange resin, belonging to the technical field of molten salt treatment of waste resin. This invention solves the problems of limited absorption capacity for sulfur-containing gases and limited retention efficiency of zinc and sulfur in existing methods for treating waste cation exchange resin. By adding potassium hydroxide to a traditional binary carbonate, this invention enhances the absorption of sulfur-containing gases, fixation of sulfur-containing substances, and retention of zinc generated during the molten salt oxidation treatment of zinc-containing waste resin. This significantly reduces the environmental pollution caused by sulfur-containing gases during waste resin treatment while increasing the zinc ion retention rate, achieving efficient and safe treatment of zinc-containing cation exchange resin.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a mixed molten salt capable of efficiently converting zinc and organic sulfur in zinc-containing waste resin into stable compounds, and a method for oxidizing waste cation exchange resin, belonging to the technical field of molten salt treatment of waste resin. Background Technology

[0002] Nuclear energy is recognized as a clean and sustainable energy source. The development of nuclear energy has not only reduced the consumption of fossil fuels but also reduced pollutant emissions. However, nuclear energy production inevitably generates large amounts of radioactive waste, which often contains a certain amount of the radioactive nuclide zinc (…). 65 Zn). 65 Zn is produced by the activation of impurity neutrons in nuclear reactor structural materials and cooling water. 65 Zinc is a gamma and beta radiator with a half-life of approximately 245 days. It is carried into the ocean by treated radioactive wastewater. Zinc is a component of several important enzymes in humans and many other animals. It is readily accumulated by marine organisms and is closely related to human health.

[0003] To avoid 65 Zn accumulates in marine organisms and the human body, containing 65 Zn wastewater is primarily treated using cation exchange resins. Once the ion exchange resin reaches its saturation capacity or exceeds the radiation limit, it cannot be regenerated or eluted and must be treated directly as radioactive solid waste. The continuous accumulation of waste resin will undoubtedly further increase the demand for waste resin treatment technologies.

[0004] In addition, waste cation exchange resin contains 65 Besides zinc (Zn), waste resins also contain significant amounts of sulfur. Current waste resin thermal treatment technologies face numerous challenges in ensuring optimal efficiency and environmental sustainability. The sulfur-containing exhaust gases generated during waste resin treatment typically contain carbonyl sulfide, hydrogen sulfide, and sulfur dioxide. Furthermore, the sulfides produced during waste resin treatment are unstable at high temperatures and are easily oxidized or decomposed into sulfur dioxide or hydrogen sulfide gases released into the air. When the concentrations of hydrogen sulfide and sulfur dioxide exceed 1 ppm and 100 ppm, respectively, they pose a threat to human life. Therefore, secondary treatment of sulfur-containing gases in the exhaust gas is essential during waste resin treatment.

[0005] Molten salt oxidation technology is a promising method for treating organic solid waste. Using this method, molten salt effectively retains metal elements (such as strontium, cesium, zinc, and cobalt), and acidic gases are effectively absorbed by the molten salt to form corresponding oxides, sulfides, or neutral salts. Many types of salts play a key role in molten salt oxidation technology, among which molten carbonates, as a widely used industrial fluid, have significant advantages in this field. For the oxidation of cation exchange resins by molten salt, domestic and international researchers have focused on oxidation efficiency, while research on how to improve the absorption of sulfur-containing tail gas and the retention of metal ions during the molten salt oxidation process is relatively limited. Therefore, it is essential to provide a mixed molten salt oxidation method that can efficiently convert zinc and organic sulfur in zinc-containing waste resins into stable compounds. Summary of the Invention

[0006] In order to solve the problems of limited absorption capacity of sulfur-containing gases and limited retention efficiency of zinc and sulfur in existing methods for treating waste cation exchange resins, this invention provides a mixed molten salt oxidation method that can efficiently convert zinc and organic sulfur in zinc-containing waste resins into stable compounds.

[0007] The technical solution of this invention:

[0008] One objective of this invention is to provide a mixed molten salt capable of efficiently converting zinc and organic sulfur in zinc-containing waste resin into stable compounds. This mixed molten salt comprises a binary molten carbonate and potassium hydroxide.

[0009] Further specified, the mass ratio of binary molten carbonate to potassium hydroxide is 1:(0.05-0.15).

[0010] To further specify, the binary molten carbonate is composed of sodium carbonate and potassium carbonate in a mass ratio of 1:1.

[0011] Further specified, the mass ratio of binary molten carbonate to potassium hydroxide is 1:(0.05-0.15).

[0012] The second objective of this invention is to provide a method for treating waste cation exchange resin by oxidation with the aforementioned mixed molten salt, the method comprising the following steps:

[0013] (1) The waste cation exchange resin was placed in a zinc chloride solution for ion exchange to obtain zinc-containing waste resin;

[0014] (2) The binary molten carbonate and potassium hydroxide are mixed to obtain a molten salt system. The zinc-containing waste resin is added to the molten salt system and mixed evenly. Then it is placed in a tube furnace for heat treatment to complete the oxidation treatment of the waste cation exchange resin.

[0015] Further, the concentration of zinc chloride solution in (1) is 1-10 g / L.

[0016] Further specified, (1) the zinc ion content in the zinc-containing waste resin is 0.2-1.2 wt.%, the average particle size is less than 1 mm, and the sulfur content is greater than 10%.

[0017] Further specifying, (1) the waste cation exchange resin is nuclear grade ZG CNR 50 strong acid type cation exchange resin.

[0018] Further specifying, (1) the ion exchange treatment conditions are: shaking at room temperature for 48 hours.

[0019] Further specified, the mass ratio of zinc-containing waste resin and mixed molten salt system in (2) is 1:(0.8-1.2).

[0020] Further specified, (2) the heat treatment temperature is 600-800℃, the holding time is 1.5-2.5h, and the air flow rate is 0.4-0.6L / min.

[0021] Furthermore, the zinc-containing waste resin and the binary molten carbonate must be dried at 80-100℃ until the moisture content is no higher than 5% before mixing.

[0022] Beneficial effects:

[0023] This invention adds potassium hydroxide to traditional binary carbonates, enhancing the absorption of sulfur-containing gases, fixation of sulfur-containing substances, and retention of zinc ions generated during the molten salt oxidation treatment of zinc-containing waste resin. This significantly reduces environmental pollution from sulfur-containing gases during waste resin treatment while increasing the zinc ion retention rate. Compared with existing technologies, it has at least the following advantages:

[0024] (1) The potassium hydroxide added in this invention adheres to the surface of the resin to be treated and can efficiently adsorb sulfur-containing gases, significantly reducing the content of hydrogen sulfide and sulfur dioxide, promoting the formation of zinc sulfide at high temperature, and converting zinc sulfide into stable zinc oxide through the reaction of zinc sulfide with oxygen in the air. This can significantly increase the fixation of sulfur elements in waste resin and the retention rate of zinc ions.

[0025] (2) The addition of potassium hydroxide in this invention also greatly promotes the formation of sulfate. This is mainly because potassium hydroxide is converted into potassium oxide and water vapor at high temperatures. Then, the water vapor and potassium oxide react with residual sulfur, and can also react with carbon to generate potassium vapor and potassium carbonate, which then continue to react with sulfur-containing compounds. This further enhances the adsorption of hydrogen sulfide and sulfur dioxide by the binary carbonate system. In addition, at temperatures above 500℃, Zn 2+ and K + With SO4 2- The combination forms K2Zn2(SO4)3, which effectively improves the zinc retention rate.

[0026] (3) The waste cation exchange resin treatment method provided by the present invention can further improve the generation rate of stable compounds sulfate and oxide and the oxidation efficiency of zinc-containing waste resin, realize the efficient and safe treatment of zinc-containing waste resin, and is more suitable for industrial application. Attached Figure Description

[0027] Figure 1 This is a comparison chart showing the zinc retention rates of oxidation treatments in Examples 1-4 and Comparative Examples 1-4.

[0028] Figure 2 This is a comparison chart of the desulfurization rates of the oxidation treatments in Examples 1-4 and Comparative Examples 1-4;

[0029] Figure 3 The XRD patterns of the waste salt products after oxidation treatment in Examples 1-4 and Comparative Examples 1-4 are shown.

[0030] Figure 4 The graph shows a comparison of sulfate content in the waste salt products after oxidation treatment in Examples 1-4 and Comparative Examples 1-4. Detailed Implementation

[0031] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0032] Unless otherwise specified, the experimental methods used in the following examples are conventional methods. Unless otherwise specified, the materials, reagents, methods, and instruments used are all conventional materials, reagents, methods, and instruments in the art, and can be obtained commercially by those skilled in the art.

[0033] The terms “comprising,” “including,” “having,” “containing,” or any other variations thereof, as used in the following embodiments, are intended to cover a non-exclusive inclusion. For example, a composition, step, method, article, or apparatus that includes the listed elements is not necessarily limited to those elements, but may include other elements not expressly listed or elements inherent to such a composition, step, method, article, or apparatus.

[0034] When a quantity, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pair of any upper or preferred value with any lower or preferred value, regardless of whether the range is disclosed individually. For example, when the range “1 to 5” is disclosed, the described range should be interpreted as including ranges “1 to 4”, “1 to 3”, “1 to 2”, “1 to 2 and 4 to 5”, “1 to 3 and 5”, etc. When numerical ranges are described herein, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within that range. In this specification and claims, range definitions may be combined and / or interchanged, unless otherwise stated, these ranges include all subranges contained therein.

[0035] The indefinite articles “a” and “an” preceding an element or component of this invention do not impose any limitation on the quantity (i.e., number of times) of the element or component. Therefore, “an” or “a” should be interpreted as including one or at least one, and the singular form of an element or component also includes the plural form, unless the quantity clearly refers only to the singular form.

[0036] In this invention, "an embodiment" or "embodiment" refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that excludes other embodiments.

[0037] The endpoints and any values ​​of the ranges disclosed in this invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0038] Unless otherwise specified, the experimental methods used in the following examples are conventional methods. Unless otherwise specified, the materials, reagents, methods, and instruments used are all conventional materials, reagents, methods, and instruments in the art, and can be obtained commercially by those skilled in the art.

[0039] Example 1:

[0040] The mixed molten salt oxidation method for efficiently converting zinc and organic sulfur in zinc-containing waste resin into stable compounds in this embodiment is carried out according to the following steps:

[0041] Step 1: Preparation of the mixed molten salt system:

[0042] First, potassium hydroxide, sodium carbonate, and potassium carbonate were dried separately in an oven at 80°C until the moisture content of each material was ≤5%.

[0043] Then, take 1.0g of dried sodium carbonate, 1.0g of potassium carbonate and 0.1g of potassium hydroxide, mix them evenly to obtain a mixed molten salt system.

[0044] Step 2: Resin treatment:

[0045] First, 20g of waste cation exchange resin was placed in a 10g / L zinc chloride solution and shaken at room temperature for 48h to complete the ion exchange, resulting in zinc-containing waste resin; the zinc ion content in the zinc-containing waste resin was 9.3%, and the sulfur content was 10.3%.

[0046] Then, the zinc-containing waste resin (average particle size = 0.5 mm, sulfur content = 8.5%) was dried in an oven at 80°C until the moisture content of the above materials was ≤5%.

[0047] Finally, take 2.0g of the dried zinc-containing waste resin and mix it evenly with the above molten salt system. Then place it in a tube furnace and keep it at 500℃ for 2 hours with an air flow rate of 0.5L / min to complete the treatment of the zinc-containing waste resin.

[0048] During heat treatment, the sulfur content was analyzed using an online gas chromatography-mass spectrometry (GC-MS). After heat treatment, the waste salt product was cooled and subjected to component analysis to obtain the zinc, sulfur, and sulfate content. The test results are as follows: Figure 1 , 2 As shown in Figure 4, the results of the salt composition of the waste salt products are as follows: Figure 3 As shown in (a).

[0049] Example 2:

[0050] The difference between this embodiment and Embodiment 1 is that the dried zinc-containing waste resin and the mixed molten salt system are placed in a tube furnace for heat treatment at a temperature of 600°C, while the remaining process steps and parameter settings are the same as in Embodiment 1.

[0051] During heat treatment, the sulfur content was analyzed using an online gas chromatography-mass spectrometry (GC-MS). After heat treatment, the waste salt product was cooled and subjected to component analysis to obtain the zinc, sulfur, and sulfate content. The test results are as follows: Figure 1 , 2 As shown in Figure 4, the results of the salt composition of the waste salt products are as follows: Figure 3 As shown in (b).

[0052] Example 3:

[0053] The difference between this embodiment and Embodiment 1 is that the dried zinc-containing waste resin and the mixed molten salt system are placed in a tube furnace for heat treatment at 700°C, while the remaining process steps and parameter settings are the same as in Embodiment 1.

[0054] During heat treatment, the sulfur content was analyzed using an online gas chromatography-mass spectrometry (GC-MS). After heat treatment, the waste salt product was cooled and subjected to component analysis to obtain the zinc, sulfur, and sulfate content. The test results are as follows: Figure 1 , 2 As shown in Figure 4, the results of the salt composition of the waste salt products are as follows: Figure 3 As shown in (c).

[0055] Example 4:

[0056] The difference between this embodiment and Embodiment 1 is that the dried zinc-containing waste resin and the mixed molten salt system are placed in a tube furnace for heat treatment at 800°C, while the remaining process steps and parameter settings are the same as in Embodiment 1.

[0057] During heat treatment, the sulfur content was analyzed using an online gas chromatography-mass spectrometry (GC-MS). After heat treatment, the waste salt product was cooled and subjected to component analysis to obtain the zinc, sulfur, and sulfate content. The test results are as follows: Figure 1 , 2 As shown in Figure 4, the results of the salt composition of the waste salt products are as follows: Figure 3 As shown in (d).

[0058] Example 5:

[0059] The difference between this embodiment and Embodiment 1 is that the amounts of sodium carbonate, potassium carbonate, potassium hydroxide, and zinc-containing waste resin are 2.0g, 2.0g, 0.4g, and 4.0g, respectively. The remaining process steps and parameter settings are the same as in Embodiment 1.

[0060] Example 6:

[0061] The difference between this embodiment and Embodiment 1 is that the amounts of sodium carbonate, potassium carbonate, potassium hydroxide, and zinc-containing waste resin are 4.0g, 4.0g, 0.8g, and 8.0g, respectively. The remaining process steps and parameter settings are the same as in Embodiment 1.

[0062] Comparative Example 1:

[0063] The difference between this comparative example and Example 1 is that the mixed molten salt does not contain potassium hydroxide, while the remaining process steps and parameter settings are the same as in Example 1.

[0064] During heat treatment, the sulfur content was analyzed using an online gas chromatography-mass spectrometry (GC-MS). After heat treatment, the waste salt product was cooled and subjected to component analysis to obtain the zinc, sulfur, and sulfate content. The test results are as follows: Figure 1 , 2 As shown in Figure 4, the results of the salt composition of the waste salt products are as follows: Figure 3 As shown in (a).

[0065] Comparative Example 2:

[0066] The difference between this comparative example and Comparative Example 1 is that the dried zinc-containing waste resin and the mixed molten salt system are placed in a tube furnace for heat treatment at 600℃, while the remaining process steps and parameter settings are the same as those in Comparative Example 1.

[0067] During heat treatment, the sulfur content was analyzed using an online gas chromatography-mass spectrometry (GC-MS). After heat treatment, the waste salt product was cooled and subjected to component analysis to obtain the zinc, sulfur, and sulfate content. The test results are as follows: Figure 1 , 2 As shown in Figure 4, the results of the salt composition of the waste salt products are as follows: Figure 3 As shown in (b).

[0068] Comparative Example 3:

[0069] The difference between this comparative example and Comparative Example 1 is that the dried zinc-containing waste resin and the mixed molten salt system are placed in a tube furnace for heat treatment at 700℃, while the remaining process steps and parameter settings are the same as those in Comparative Example 1.

[0070] During heat treatment, the sulfur content was analyzed using an online gas chromatography-mass spectrometry (GC-MS). After heat treatment, the waste salt product was cooled and subjected to component analysis to obtain the zinc, sulfur, and sulfate content. The test results are as follows: Figure 1 , 2 As shown in Figure 4, the results of the salt composition of the waste salt products are as follows: Figure 3 As shown in (c).

[0071] Comparative Example 4:

[0072] The difference between this comparative example and Comparative Example 1 is that the dried zinc-containing waste resin and the mixed molten salt system are placed in a tube furnace for heat treatment at 800℃, while the remaining process steps and parameter settings are the same as those in Comparative Example 1.

[0073] During heat treatment, the sulfur content was analyzed using an online gas chromatography-mass spectrometry (GC-MS). After heat treatment, the waste salt product was cooled and subjected to component analysis to obtain the zinc, sulfur, and sulfate content. The test results are as follows: Figure 1 , 2 As shown in Figure 4, the results of the salt composition of the waste salt products are as follows: Figure 3 As shown in (d).

[0074] Comparative Example 5:

[0075] The difference between this comparative example and Example 5 is that the mixed molten salt does not contain potassium hydroxide, while the remaining process steps and parameter settings are the same as in Example 5.

[0076] Comparative Example 6:

[0077] The difference between this comparative example and Example 6 is that the mixed molten salt does not contain potassium hydroxide, while the remaining process steps and parameter settings are the same as in Example 6.

[0078] Example of results:

[0079] (1) The zinc retention rates of the oxidation treatments in Examples 1-4 and Comparative Examples 1-4 were compared and analyzed. The results are as follows: Figure 1 As shown. By Figure 1 It can be seen that when potassium hydroxide is added, the zinc ion rejection rate increases with increasing temperature. After treatment with molten carbonate without potassium hydroxide, the zinc rejection rate decreases significantly. After treatment with molten carbonate system containing potassium hydroxide, the zinc rejection rate further increases, reaching a maximum of 98.34%. This indicates that adding potassium hydroxide has an excellent rejection capacity for zinc in the molten salt oxidation of zinc-containing waste resin, and its rejection effect is significantly better than the traditional molten carbonate oxidation technology for waste resin. At the same time, this method has lower cost and less environmental pollution.

[0080] (2) A comparative analysis was conducted on the sulfur content in the waste salt products after treatment in Examples 1-4 and Comparative Examples 1-4. The results are as follows: Figure 2 As shown. By Figure 2 It can be seen that after treatment with molten carbonate without potassium hydroxide, the desulfurization rate of zinc-containing waste resin increases with increasing temperature. After treatment with molten carbonate system containing potassium hydroxide, the desulfurization rate further increases, reaching a maximum of 98.05%. This indicates that the addition of potassium hydroxide has an excellent ability to remove sulfur-containing structures during the molten salt oxidation process of zinc-containing waste resin.

[0081] (3) The components of the waste salt products after treatment in Examples 1-4 and Comparative Examples 1-4 were subjected to XRD tests and comparative analysis. The results are as follows: Figure 3 As shown. By Figure 3 As can be seen in (a), at 500℃, after treatment with molten carbonate without potassium hydroxide, the waste salt product mainly consists of sodium carbonate and potassium carbonate. After treatment with molten carbonate containing potassium hydroxide, the waste salt product newly contains sodium sulfate. This indicates that the combination of potassium hydroxide and carbonate plays a certain role in fixing sulfur-containing substances. Figure 3 As can be seen in (b), when the temperature is 600℃, after treatment with a molten carbonate system containing potassium hydroxide and a molten carbonate system without potassium hydroxide, the waste salt products mainly consist of sodium carbonate, potassium sulfate, and potassium zinc sulfate. This indicates that the zinc element in the resin is effectively fixed by the molten salt system of this invention. Figure 3 As can be seen in (c), when the temperature is 700℃, after treatment with a molten carbonate system containing potassium hydroxide and a molten carbonate system without potassium hydroxide, the waste salt products mainly consist of potassium sulfate, potassium zinc sulfate, and zinc sulfide. This indicates that the sulfur and zinc elements in the resin are effectively fixed by the molten salt system of this invention, and that the zinc and sulfur elements combine to form sulfides. Figure 3 As can be seen from (d), when the temperature is 800℃, after the zinc-containing waste resin is treated by a molten carbonate system containing potassium hydroxide and a molten carbonate system without potassium hydroxide, the waste salt products are mainly potassium sulfate, potassium zinc sulfate and zinc oxide. This is mainly because zinc sulfide has undergone an oxidation reaction. The sulfur dioxide produced in this process will be further absorbed by the molten carbonate to generate stable sulfate.

[0082] (4) The sulfate content in the waste salt products after treatment in Examples 1-4 and Comparative Examples 1-4 was compared and analyzed. The results are as follows: Figure 4 As shown: by Figure 4 It can be seen that after zinc-containing waste resin is treated with molten carbonate without potassium hydroxide, the sulfate content in the waste salt product increases with the increase of temperature. After treatment with molten carbonate system containing potassium hydroxide, the sulfate content further increases, reaching a maximum of 76.51%. This indicates that the addition of potassium hydroxide indirectly fixes the sulfur element, which exists in the waste salt in a relatively stable compound form.

[0083] Although the present invention has been disclosed above with reference to preferred embodiments, it is not intended to limit the present invention. Anyone skilled in the art can make various modifications and alterations without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be determined by the claims.

Claims

1. A method for treating waste cation exchange resin by oxidizing with mixed molten salt, characterized in that, include: (1) The waste cation exchange resin was placed in a zinc chloride solution for ion exchange to obtain zinc-containing waste resin; (2) Mix binary molten carbonate and potassium hydroxide to obtain mixed molten salt. Add zinc-containing waste resin to the mixed molten salt and mix evenly. Then place it in a tube furnace for heat treatment to complete the oxidation treatment of waste cation exchange resin. The mixed molten salt can efficiently convert zinc and organic sulfur in zinc-containing waste resin into stable compounds. The mixed molten salt includes a binary molten carbonate and potassium hydroxide, with a mass ratio of 1:(0.05-0.15). The binary molten carbonate is composed of sodium carbonate and potassium carbonate in a mass ratio of 1:

1. (2) The heat treatment temperature is 600-800℃, the holding time is 1.5-2.5 h, and the air flow rate is 0.4-0.6 L / min.

2. The method according to claim 1, characterized in that, (1) The concentration of zinc chloride solution is 1-10 g / L.

3. The method according to claim 1, characterized in that, (1) The zinc ion content in the obtained zinc-containing waste resin is 0.2-1.2 wt.%, the average particle size is less than 1 mm, and the sulfur content is greater than 10%.

4. The method according to claim 1, characterized in that, (1) The ion exchange treatment conditions were: shaking at room temperature for 48 h.

5. The method according to claim 1, characterized in that, (2) The mass ratio of zinc-containing waste resin and mixed molten salt is 1:(0.8-1.2).

Citation Information

Patent Citations

  • Method for treating cation exchange resin by molten salt oxidation technology

    CN110665548A