A method for manufacturing high-quality panda-type polarization-maintaining optical fiber

By filling the double holes of the preform with glass rods and using positioning rods and tail tubes for vacuum processing, combined with gradual vacuuming, the problems of cladding collapse and boron rod displacement in the manufacturing of panda-type polarization-maintaining optical fibers were solved, and the fiber quality was improved. of finished product quality and performance.

CN118270977BActive Publication Date: 2024-10-29JIANGSU HENGTONG OPTICAL FIBER TECH +2
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410694362.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-31
Publication Date
2024-10-29
Estimated Expiration
2044-05-31

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively solve the problems of cladding collapse, boron rod displacement and interface cavity during the manufacturing process of Panda-type polarization-maintaining optical fiber, resulting in poor performance and quality of the finished optical fiber.

Method used

By filling the double holes of the preform with glass rods and using positioning rods and tail tubes for vacuuming, combined with a gradual or stepped vacuuming method, the position and pressure of the boron rods are controlled to avoid the boron rods from being damaged during the melting and drawing process. Displacements and cavities are generated in the cladding to ensure the roundness of the cladding and the stability of the beat length.

Benefits of technology

Significantly improve the cladding out-of-roundness and beat length stability of the Panda-type polarization-maintaining optical fiber, reduce the manufacturing defect rate, and improve the drawing performance and quality of the optical fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118270977B_ABST
    Figure CN118270977B_ABST
Patent Text Reader

Abstract

The invention discloses a method for manufacturing a high-quality panda-type polarization-maintaining optical fiber, comprising the following steps: taking a preform with double holes, filling a glass rod in each of the double holes at the head of the preform, and then melting and taper the head; welding a tail tube 1 at the tail of the preform; loading two processed boron rods into the double holes from the tail of the preform; welding a tail tube 2 at the end of the tail tube 1; loading two positioning rods into the double holes of the preform from the tail of the tail tube 2, and the two positioning rods support the boron rods; using a vacuum device to continuously vacuum the interior of the preform; inserting the preform into an induction furnace for heating and sinking, and controlling the vacuum pressure of the vacuum device; drawing into fibers to obtain a panda-type polarization-maintaining optical fiber. The method greatly improves the cladding non-circularity and beat length stability of the panda-type polarization-maintaining optical fiber, and can prevent the generation of cavities at the interface of the boron zone, improve the drawing performance and quality of the polarization-maintaining optical fiber, and obtain a high-quality panda-type polarization-maintaining optical fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of optical fibers, and particularly relates to a method for manufacturing a high-quality panda-type polarization-maintaining optical fiber. Background Art

[0002] Fiber optic gyroscopes can accurately determine the orientation of moving objects and are widely used in modern aviation, navigation, aerospace and defense industries. Polarization-maintaining fiber - the more commonly used is the panda-type polarization-maintaining fiber, which is the core sensitive element of the fiber optic gyroscope and has very important strategic significance for the development of the country's industry, defense and other high technologies. However, the manufacturing difficulty of polarization-maintaining fiber is much higher than that of conventional single-mode fiber. Conventional manufacturing methods often have the following problems: (1) The cladding of the optical fiber collapses on the slow axis to form an elliptical structure due to the large gap between the boron rod and the hole wall, resulting in large cladding non-roundness. (2) The boron rod moves up and down during drawing, resulting in large axial fluctuations in the size of the boron zone, resulting in large fluctuations in the beat length. (3) When the boron rod melts in the drawing furnace, it adheres to the hole wall, resulting in bubbles or cavities at the interface between the boron zone and the cladding, making the optical fiber unqualified. These problems seriously affect the performance and quality of the finished product of polarization-maintaining fiber.

[0003] Invention patents 201210405095.6 and 200810197257.5 can manufacture conventional panda-type polarization-maintaining optical fiber mother rods or optical fibers, but it is difficult to solve the problems of cladding collapse, boron rod displacement and interface cavity that are prone to occur during the drawing process using their process parameters. Invention patent 202211668682.4 proposes to polish the cladding so that the slow axis of the cladding is pre-elliptical, and then collapses during the drawing process to reach a circular shape, but it is extremely difficult to achieve a regular elliptical shape that does not deviate from the axial direction, and it is not practical; it does not mention how to solve the problem of cavity and displacement of the boron rod during melting and drawing. Invention patent 201811525392.8 uses a two-stage punching method to improve the structural stability of the stress hole, mainly to prevent the stress hole from cracking, but it cannot avoid the problem of excessive cladding collapse caused by the gap between the stress rod and the hole wall. It does not mention how to solve the problem of cavity and displacement of the boron rod during the drawing process. Summary of the invention

[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a method for manufacturing a high-quality Panda-type polarization-maintaining optical fiber, which greatly improves the cladding non-circularity and beat length stability of the Panda-type polarization-maintaining optical fiber, and can prevent the generation of cavities at the interface of the boron region, thereby improving the drawing performance and quality of the polarization-maintaining optical fiber, and can obtain a high-quality Panda-type polarization-maintaining optical fiber.

[0005] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0006] A method for manufacturing a high-quality Panda-type polarization-maintaining optical fiber comprises the following steps:

[0007] Step 1: Take a preform rod with double holes, fill a glass rod in each of the double holes at the head of the preform rod, and then melt and taper the head;

[0008] Step 2, welding a tail pipe 1 at the tail of the preform rod;

[0009] Step 3, inserting two processed boron rods into the double holes from the tail of the preform rod respectively;

[0010] Step 4, welding tail pipe 2 to the end of tail pipe 1;

[0011] Step 5, two positioning rods are respectively installed into the double holes of the preform rod from the tail of the tail tube 2, and the two positioning rods support the boron rod to obtain a finished preform rod;

[0012] Step 6, using a vacuum pumping device to continuously vacuum the interior of the finished preform;

[0013] Step 7, inserting the finished preform into the induction furnace for heating and sinking, and controlling the vacuum pressure of the vacuum device;

[0014] Step eight, drawing into fiber to obtain panda-shaped polarization-maintaining optical fiber.

[0015] Furthermore, the outer diameters of the two glass rods are 0.01 mm to 0.2 mm smaller than the inner diameters of the double holes of the preform rod, and the lengths of the glass rods are 30 mm to 80 mm.

[0016] Furthermore, the lengths of the two boron rods are similar, with a length difference of ≤5mm, and the length of the boron rod is 50mm-200mm smaller than the length of the preform rod; the two boron rods are also ground to have similar outer diameters, with an average outer diameter difference of ≤0.02mm between the two boron rods, and an outer diameter fluctuation range of a single boron rod of ≤0.02mm.

[0017] Furthermore, the length of the tail pipe 1 is 50-100 mm shorter than the length of the boron rod.

[0018] Furthermore, the assembly gap between the boron rod and the inner wall of the hole of the preform rod is 0.01-0.05 mm.

[0019] Furthermore, the outer diameter of the positioning rod is 0.2-1 mm smaller than that of the boron rod.

[0020] Furthermore, in step six, the vacuum device is sealed and connected to the end face of the tail pipe 2, and the vacuum pressure is 1-100 kPa.

[0021] Furthermore, the inner diameter of the induction coil of the induction furnace is 120-180 mm, the number of bundles is 5-6, and the spacing between each bundle is 5-10 mm.

[0022] Furthermore, when the temperature is increased and the head is plummeted, the initial extraction pressure is 20-50 kPa, and the extraction pressure after the head is plummeted is adjusted to 50-100 kPa.

[0023] Furthermore, during the fiber drawing process, a gradual or step-wise vacuuming method is adopted.

[0024] Beneficial effects of the present invention:

[0025] (1) The present invention first fills the head of the double hole of the preform rod with a glass rod before loading the boron rod into the double hole of the preform rod. This is because the boron rod is doped with a high concentration of boron and has great internal stress. It is very easy to burst during the melting and taper drawing, resulting in the leakage of boron water and the loss of the entire boron rod. Even if the taper drawing is successful, it will waste a section of qualified and expensive boron rod. Moreover, if the boron rod is directly loaded, the high temperature during the melting and taper drawing will affect the refractive index of the boron zone. Filling the glass rod first for melting and taper drawing and then loading the boron rod can reduce the waste of the boron rod and avoid the boron rod bursting during operation and the change of refractive index at high temperature, which affects the optical fiber parameters.

[0026] (2) The present invention inserts a positioning rod into the double-hole tail end of the preform rod through the tail tube, and the positioning rod supports the boron rod. Therefore, during melt drawing, when the entire rod body of the preform rod is completely in the furnace, it can be judged whether the boron rod is displaced according to the positioning rod, so as to facilitate the adjustment of the matching pumping pressure to maintain the balance of the boron rod. In summary, the positioning rod provided in the present invention can judge the position of the boron rod and the actual pumping pressure without affecting the vacuum effect, so as to facilitate timely adjustment of the pumping pressure to keep the boron rod in a balanced state, thereby ensuring the size and roundness of the boron zone and improving the cladding non-roundness and beat length stability.

[0027] (3) The method of the present invention uses a glass rod, a positioning rod, a tail tube 1, a tail tube 2, a boron rod and a double hole of a preform rod to cooperate, which can avoid the influence of taper pulling, welding of the tail tube, etc. on the first-loaded boron rod, thereby providing the feasibility of greatly reducing the gap between the boron rod and the double hole, and ultimately avoiding excessive shrinkage of the cladding on the slow axis. The cladding non-circularity of the prepared polarization-maintaining optical fiber is ≤0.5%;

[0028] (4) During the drawing process, the present invention adopts a gradual or step-wise vacuuming method, which can not only remove the air inside the double holes, but also keep the position of the boron rod in a molten state at the head in a dynamic balance, thereby avoiding the pressure difference between the furnace pressure and the vacuum pressure causing the boron rod to move up or down, thereby avoiding changes in the area of ​​the boron zone, and ensuring that the beat length fluctuation of the prepared polarization-maintaining optical fiber is ≤0.1 mm.

[0029] (5) The present invention adopts a specific coil design and sinker process, which can effectively prevent the boron rod from softening and adhering to the inner wall of the double hole before entering the high-temperature melting zone, avoid the formation of interface bubbles or cavities, avoid the production of a large number of defective products, and greatly reduce the manufacturing defect rate.

[0030] The present invention can solve the problems of large cladding non-circularity, large beat length fluctuation, high defect rate and the like of the Panda-type polarization-maintaining optical fiber, thereby improving the drawing performance and quality of the polarization-maintaining optical fiber, and can be used to prepare various Panda-type polarization-maintaining optical fibers with wavelengths between 1310 nm and 1550 nm, including but not limited to 80 / 165, 60 / 100 and 40 / 80 types. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 FIG. 1 is a schematic diagram of step 1 in the manufacturing method according to an embodiment of the present invention.

[0032] Figure 2 FIG. 1 is a schematic diagram of step 2 in the manufacturing method according to an embodiment of the present invention.

[0033] Figure 3 FIG. 1 is a schematic diagram of step three in the manufacturing method according to an embodiment of the present invention.

[0034] Figure 4 FIG. 4 is a schematic diagram of step 4 in the manufacturing method according to an embodiment of the present invention.

[0035] Figure 5 FIG. 5 is a schematic diagram of step five in the manufacturing method according to an embodiment of the present invention.

[0036] Figure 6 Schematic diagram of steps six to eight in the manufacturing method of an embodiment of the present invention.

[0037] In the figure, 1: preform rod, 11: quartz sleeve, 12: core rod; 2: glass rod; 3: boron rod; 4: tail tube one; 5: tail tube two; 6: positioning rod; 7: induction furnace, 71: induction coil; 8: finished preform rod; 9: vacuum device. DETAILED DESCRIPTION

[0038] The technical solutions in the present invention will be described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0039] The present invention provides a method for manufacturing a high-quality panda-type polarization-maintaining optical fiber. Before performing the following steps, a preform rod 1 with double holes is prepared according to the design requirements, and the preform rod 1 is composed of a quartz sleeve 11 and a core rod 12; two boron rods are melted and cut to a similar length, and then the two boron rods are ground to the same outer diameter, and then ultrasonic cleaning is performed. The length difference between the two boron rods is ≤5mm, and the length of the boron rod is 50mm-200mm smaller than the length of the preform rod; the difference in the average outer diameters of the two boron rods is ≤0.02mm, and the outer diameter fluctuation range of a single boron rod is ≤0.02mm. The manufacturing method includes the following steps:

[0040] Step 1: Take a preform rod 1 with double holes, fill the double holes at the head of the preform rod 1 with a glass rod 2, and then melt and taper the head. Figure 1 As shown;

[0041] The outer diameters of the two glass rods 2 are 0.01 mm to 0.2 mm smaller than the inner diameters of the double holes of the preform rod 1 , and the lengths of the glass rods 2 are 30 mm to 80 mm.

[0042] Step 2: welding a tail pipe 4 to the tail of the preform rod 1, and then performing pickling treatment, such as Figure 2 As shown; the length of the tail pipe 4 is 50-100mm smaller than the length of the boron rod 3.

[0043] Step 3: Load the two processed boron rods 3 into the double holes from the tail of the preform rod 1, as shown in FIG. Figure 3 As shown; the assembly gaps between the two boron rods 3 and the inner wall of the hole of the preform rod 1 are 0.01-0.05mm respectively.

[0044] Step 4: weld the tail pipe 2 5 to the end of the tail pipe 1 4, and then perform ultrasonic cleaning. Figure 4 As shown; the length of the tail pipe 2 5 can be matched with the tail pipe 1 4 so that the boron rod can be completely drawn on the wire drawing platform; when welding the tail pipe 2 5, a narrow flame torch such as a hand lamp is preferably used for welding so that the internal boron rod is not affected.

[0045] Step 5: insert two positioning rods 6 from the tail of the tail tube 2 5 into the double holes of the preform 1 respectively, and the two positioning rods 6 support the boron rod 3 to obtain a finished preform 8, as shown in FIG. Figure 5 The outer diameter of the positioning rod 6 is 0.2-1mm smaller than that of the boron rod 3, and the length of the positioning rod 6 is such that the portion of the positioning rod 6 which is left in the tail pipe 4 and the tail pipe 5 is visible to the naked eye from the end of the hanging rod to the end of the drawing.

[0046] Steps 6 to 7 Figure 6 As shown:

[0047] Step six, install the finished preform rod 8 with its head facing downward on the rod hanging platform, and use a vacuum pumping device to continuously evacuate the interior of the finished preform rod 8; the vacuum pumping device 9 is sealed with the end face of the tail pipe 2 5, and the vacuum pressure can be adjusted between 1-100 kPa, with an adjustment accuracy of ≤0.01 kPa.

[0048] Step 7: insert the finished preform rod 8 into the induction furnace 7 for heating and sinking, and control the vacuum pressure of the vacuum device 9; the temperature zone of the induction furnace 7 needs to be reasonably set, wherein the inner diameter of the induction coil 71 is 120-180mm, the number of bundles is 5-6 bundles, and the spacing between each bundle is 5-10mm. When heating and sinking, the initial pressure is 20-50kPa, and after sinking, the pressure is adjusted to 50-100kPa.

[0049] Step 8: Fiber drawing, control the vacuum pressure, bare fiber tension and drawing speed to obtain a panda-shaped polarization-maintaining optical fiber. During the fiber drawing process, a gradual or step-wise vacuuming method is used, and the position of the positioning rod in the tail tube must be kept unchanged. The bare fiber tension control range is 0-30g, and the drawing speed control range is 200-300m / min.

[0050] In the above method, the tail pipe is divided into tail pipe 1 4 and tail pipe 2 5 for welding, and the boron rod 3 is placed after welding the tail pipe 1 4. This is because: (1) if the boron rod is directly placed and then welded as a whole tail pipe, the welding point is at the tail end of the boron rod, and the hydrogen-oxygen flame of welding will affect the boron rod, which is easy to cause the boron rod to explode; (2) if the boron rod is placed first and then the tail pipe is welded, the hydrogen-oxygen flame during welding will produce moisture, so that the tail end of the boron rod is in a high temperature zone and reacts chemically with the moisture to cause hydroxyl contamination. Therefore, the boron rod is placed after welding the tail pipe 1. This not only makes it easier to insert the boron rod, but also allows the welding point to remain close to the boron rod after the boron rod is inserted. (3) If the entire tail tube is welded first and then the boron rod is inserted, the boron rod will get stuck when being inserted into the double holes of the preformed rod, and the boron rod cannot be inserted into the tail tube to operate the boron rod. The tail tube must be destroyed and the boron rod must be pulled out and re-grinded. However, welding only the tail tube first can facilitate the operation of the boron rod, making it feasible to further reduce the gap between the boron rod and the double holes, thereby minimizing the gap and minimizing the collapse of the cladding during the drawing process.

[0051] Therefore, the tail tube is divided into tail tube one and tail tube two for welding, and the boron rod is inserted after welding tail tube one. This method not only reduces the loss of the boron rod and the potential quality risk, but also greatly improves the cladding non-circularity parameters of the optical fiber.

[0052] In the above method, the reason why the glass rod 2 is first filled into the double holes of the preform rod 1 for melt taper drawing is that: (1) the boron rod is doped with a high concentration of boron, which has great internal stress and is very easy to burst during melt taper drawing, resulting in leakage of boron water and inability to continue to use, resulting in the loss of the entire boron rod. (2) Even if the taper drawing is successful by directly filling the boron rod, a section of qualified and expensive boron rod is wasted. (3) When the boron rod is directly filled, the high temperature during melt taper drawing will affect the refractive index of the boron region. Filling the glass rod for melt taper drawing can reduce the waste of boron rods and avoid the explosion of boron rods during operation and the change of refractive index at high temperature, which affects the optical fiber parameters.

[0053] In the above method, the reason for designing the positioning rod 6 at the tail end of the boron rod 3 is that: during melt drawing, the rod hanging platform clamps the tail tube at the tail end of the light rod (finished preform rod), and the light rod is sent into the induction furnace for melt drawing. When the rod body is gradually pulled off and completely enters the furnace, it is impossible to know whether the boron rod has been displaced, and thus it is impossible to adjust the matching pumping pressure to maintain the balance of the boron rod. Insert the positioning rod above the boron rod, and the positioning rod is in the tail tube one and the tail tube two. Its length can ensure that the end position of the positioning rod can still be seen after the rod body is completely pulled, so that it can be judged whether the boron rod has been displaced according to the positioning rod to set the correct progressive pumping pressure value. The diameter of the positioning rod can ensure that there is a certain gap between the double holes of the preform rod, so as not to hinder vacuuming. The way of designing the positioning rod can determine the position of the boron rod and the size of the actual pumping pressure without affecting the vacuuming effect, so that the boron rod is in a balanced state, thereby ensuring the size and roundness of the boron zone, and improving the cladding non-roundness and the stability of the beat length.

[0054] In the above method, the present invention adopts progressive or stepped vacuuming and pressing during the drawing process. The reasons are as follows: (1) The rod head of the preform rod is in a molten state in the drawing induction furnace. At this time, the boron rod will sink due to gravity, and the internal boron water will accumulate under the double holes and form a larger elliptical shape under the pressure of the surface tension of the preform rod cladding, resulting in unqualified fiber beat length; (2) There is a lot of air remaining in the boron rod and the double holes, which can still react with quartz at high temperature, causing the quartz to be oxidized and affecting the fiber attenuation parameters; (3) The induction furnace itself is filled with inert gas and maintains a low-oxygen positive pressure state. If the vacuum is too large, the boron rod will be in a state of pressure at the head and suction at the tail. When the rod head is in a molten state, it will move upward, which will cause the boron rod to fail to fill the double holes, the size of the boron area will become smaller, and the fiber beat length will be unqualified. The progressive or stepped vacuuming method can not only remove the air inside the double holes, but also keep the furnace pressure and the weight of the boron rod balanced during wire drawing. The boron rod neither sinks nor moves up, making the size of the boron area stable, ensuring the stability of the roundness and beat length parameters.

[0055] The above method reasonably designs the inner diameter, number of ties and spacing of ties of the induction coil. When an alternating current is passed through the induction coil, the electromagnetic field generated on the induction coil acts on the graphite conductor within the inner diameter range of the coil to generate eddy current heating. Through the practical comparison of the electromagnetic field strength under different gaps between the induction coil and the conductor, a reasonable inner diameter of the coil is obtained; the number of ties and spacing of the coils will affect the length of the temperature zone in the furnace and the electromagnetic field coupling efficiency. Reasonable design can make the temperature zone concentrated and sensitive to adjustment, avoiding the excessively long temperature zone causing the boron rod to soften prematurely before entering the melting zone, and causing the silicon skin of the boron rod to adhere to the inner wall of the double hole to form a closed cavity, which cannot be healed even if vacuumized, resulting in unqualified optical fiber after drawing and forming, and avoiding the excessively short temperature zone causing the heating to be too concentrated, so that the boron rod above the high temperature zone is not fully preheated, requiring the furnace temperature to be too high, affecting the control of parameters such as bare fiber tension, and the temperature adjustment is not sensitive. Reasonable design of the inner diameter, number of ties and spacing of the induction coil can ensure a reasonable temperature zone distribution, avoid the boron rod from melting prematurely to form a boron zone cavity, and cause unqualified optical fiber.

[0056] The sinking process in the above method adopts the method of first fusing the boron rod and the cladding together in the initial state, and then increasing the vacuum to exhaust the air in the hole. This method fixes the position of the boron rod when sinking the head, and does not sink or move up; by setting a reasonable initial suction pressure, the fusion at this stage is guaranteed and the air at the head is excluded, making it difficult for the boron rod to move up, and then after the head falls off (indicating that it has been fused), the suction pressure is increased to a reasonable value to exhaust the air. The sinking process can exclude the air in the conical cavity of the boron rod head through a certain suction pressure adjustment to fully fuse it with the inner wall of the double hole. After fusion, it prevents the boron rod from moving up, causing dissatisfaction of the boron water filling, and then leads to a reduction in the size of the boron area.

[0057] Example

[0058] The length of the preform rod 1 with double holes is 556.68 mm, the inner diameter of the double holes after punching is 14.22 mm, and the inner diameter of the double holes after pickling is 14.23 mm. Two boron rods 3 with suitable parameters are selected, and their lengths are 431.26 mm and 458.57 mm respectively. The boron rod with a length of 458.57 mm is melted and cut off using an oxyhydrogen flame, and the length of the boron rod after cutting is measured to be 435.12 mm. The two boron rods are then ground on a grinder, and their diameters after grinding are 14.21±0.01 mm and 14.22±0.01 mm respectively, and then ultrasonically cleaned.

[0059] Two glass rods 2 with a length of about 60 mm and an outer diameter of about 14.1 mm are inserted into the double holes from one end (head) of the preform rod 1 and aligned with the end faces. Then, the head of the preform rod 1 is tapered by a taper machine to form a cone head. Figure 1 As shown. Select the length of tail pipe 14 to be 375.45 mm, and weld tail pipe 14 at the other end (tail) of preform rod 1 by hand. Figure 2 As shown, then pickling is performed for a certain period of time. Two boron rods 3 are inserted into the double holes of the preform rod 1 from the tail of the tail tube 4, just to support the glass rod 2 of the cone head, as shown in FIG. Figure 3 Use a hand lamp to weld a section of tail pipe 2 5 to the tail of tail pipe 1 4, as shown in FIG. Figure 4 As shown, ultrasonic cleaning is then performed. Select two positioning rods 6 with a length of about 500 mm and an outer diameter of about 14 mm, and insert them into the double holes of the preform rod 1 from the tail of the tail tube 2 5, just supporting the tail ends of the two boron rods 3, as shown in FIG. Figure 5 As shown, a finished preform rod 8 is obtained.

[0060] The finished preform rod 8 is hung on the rod hanging platform, and a vacuum device 9 is installed at the tail. The device contains a sealing ring to prevent air leakage, and the suction pressure of the vacuum pump can be displayed and adjusted. Use an induction furnace 7 for heating and wire drawing. The inner diameter of the induction coil 71 is 180mm, the number of bundles is 5, and the spacing between each bundle is 5mm. Insert the optical rod into the induction furnace 7, set the initial suction pressure to 20kPa, and heat it to the head sinking power to perform the head sinking operation. After the head comes down, adjust the suction pressure to 50kPa. After cutting the head, clamp the optical rod with an auxiliary traction wheel for wire drawing until the optical fiber is observed with the naked eye without intermittent shining bright spots. Adjust the suction pressure to 10kPa, pass the mold and increase the speed. Increase the speed to a stable speed of about 220m / min, and control the furnace temperature so that the optical fiber drawing tension is about 10g. Figure 6 As shown. During the wire drawing process, the pressure is adjusted in stages until the wire drawing is completed. The gradient setting parameters of the pressure are shown in Table 1:

[0061] Table 1

[0062]

[0063] A PM1310-80 / 135 polarization-maintaining optical fiber prepared by the above method was screened and divided into reels. The typical parameters of the test optical fiber of 1 km sampled from each reel are shown in Table 2:

[0064] Table 2

[0065]

[0066] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.

[0067] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for manufacturing a high-quality Panda-type polarization-maintaining optical fiber, characterized in that: The following steps are involved: Step 1: Take a preform rod with double holes, fill a glass rod into each of the double holes at the head of the preform rod, and then melt and taper the head; Step 2, welding a tail pipe 1 at the tail of the preform rod; Step 3, inserting two processed boron rods into the double holes from the tail of the preform rod respectively; Step 4, welding tail pipe 2 to the end of tail pipe 1; Step 5, two positioning rods are respectively installed into the double holes of the preform rod from the tail of the tail tube 2, and the two positioning rods support the boron rod to obtain a finished preform rod; Step 6, using a vacuum pumping device to continuously vacuum the interior of the finished preform; Step 7, inserting the finished preform into the induction furnace for heating and sinking, and controlling the vacuum pressure of the vacuum device; Step eight, drawing the fiber to obtain a Panda-type polarization-maintaining optical fiber; during the fiber drawing process, a gradual or step-wise vacuuming method is adopted.

2. The method for manufacturing a high-quality Panda-type polarization-maintaining optical fiber according to claim 1, characterized in that: The outer diameters of the two glass rods are 0.01 mm to 0.2 mm smaller than the inner diameters of the double holes of the preform rod, and the lengths of the glass rods are 30 mm to 80 mm.

3. The method for manufacturing a high-quality Panda-type polarization-maintaining optical fiber according to claim 1, characterized in that: The length difference between the two boron rods is ≤5mm, and the length of the boron rod is 50mm-200mm shorter than the length of the preformed rod; the two boron rods are also ground to a mean outer diameter difference of ≤0.02mm, and the outer diameter fluctuation range of a single boron rod is ≤0.02mm.

4. The method for manufacturing a high-quality Panda-type polarization-maintaining optical fiber according to claim 1, characterized in that: The length of the tail pipe 1 is 50-100 mm shorter than the length of the boron rod.

5. The method for manufacturing a high-quality Panda-type polarization-maintaining optical fiber according to claim 1, characterized in that: The assembly gap between the boron rod and the inner wall of the hole of the preform rod is 0.01-0.05mm.

6. The method for manufacturing a high-quality Panda-type polarization-maintaining optical fiber according to claim 1, characterized in that: The outer diameter of the positioning rod is 0.2-1 mm smaller than that of the boron rod.

7. The method for manufacturing a high-quality Panda-type polarization-maintaining optical fiber according to claim 1, characterized in that: In step six, the vacuum device is sealed and connected to the end face of the tail pipe 2, and the vacuum pressure is 1-100 kPa.

8. The method for manufacturing a high-quality Panda-type polarization-maintaining optical fiber according to claim 1, characterized in that: The inner diameter of the induction coil of the induction furnace is 120-180 mm, the number of bundles is 5-6, and the spacing between each bundle is 5-10 mm.

9. The method for manufacturing a high-quality Panda-type polarization-maintaining optical fiber according to claim 1, characterized in that: When the temperature rises and the head is plummeted, the initial extraction pressure is 20-50kPa, and the extraction pressure is adjusted to 50-100kPa after the head is plummeted.

Citation Information

Patent Citations

  • Method for manufacturing panda type polarization-preserving fiber

    CN101367608B

  • Method for manufacturing polarization-preserving optical fiber

    CN102910812A

  • Improved panda-type polarization maintaining optical fiber preform and manufacturing process thereof

    CN109553291A

  • Method for correcting out-of-roundness of panda polarization-maintaining optical fiber cladding

    CN116217064A

  • Panda polarization-maintaining optical fiber preform and preparation method thereof

    CN117776515A