Solid electrolyte material and preparation method thereof, positive electrode active material, positive electrode sheet, solid-state battery and electrical equipment

By employing the NASICON crystal structure and phosphate, pyrophosphate, and heteropolyacid framework design in solid electrolyte materials, the shortcomings of oxide solid electrolyte materials in balancing ionic conductivity and structural stability are solved, thereby improving the rate performance and cycle performance of the battery.

CN118281228BActive Publication Date: 2024-11-05BEIJING EASPRING MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410384654.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2024-11-05
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

Existing oxide solid electrolyte materials struggle to simultaneously improve ionic conductivity and structural stability, impacting battery rate performance and cycle performance.

Method used

Solid electrolyte materials employing the NASICON crystal structure contain phosphate and pyrophosphate as a framework, and their structure is optimized through specific crystal orientation and heteropolyacid doping to improve ionic conductivity and stability.

Benefits of technology

It improves the ionic conductivity and structural stability of solid electrolyte materials, thereby enhancing the rate performance and cycle performance of batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118281228B_ABST
    Figure CN118281228B_ABST
Patent Text Reader

Abstract

The present application proposes a solid electrolyte material and a preparation method thereof, a positive electrode active material, a positive electrode sheet, a solid-state battery and an electrical device, wherein the solid electrolyte material is a NASICON crystal structure, and in the X-ray diffraction spectrum of the solid electrolyte material, there are characteristic diffraction peaks at diffraction angles 2θ of 14.5°-14.8°, 19.5°-19.7° and 22.5°-22.8°, respectively, wherein the ratio of the peak intensity I1 of the characteristic diffraction peak at 2θ value of 14.5°-14.8° to the peak intensity I2 of the characteristic diffraction peak at 2θ value of 22.5°-22.8° satisfies: 1.5≤I2 / I1≤3. Thus, the ionic conductivity and structural stability of the solid electrolyte are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of batteries, and in particular, to solid electrolyte materials and preparation methods thereof, positive electrode active materials, positive electrode plates, solid-state batteries and electrical equipment. Background Art

[0002] Range anxiety and battery safety issues have become the pain points and major bottlenecks that restrict the development of new energy vehicles. The key to the iterative innovation of the next generation of higher energy density and safer power batteries lies in the technological breakthrough of solid-state batteries. As the core material of solid-state batteries, the comprehensive performance and industrialization progress of solid-state electrolytes are the key to the development of solid-state batteries. At present, solid-state electrolytes with industrialization prospects mainly include three major systems: polymers, sulfides and oxides. Among them, although sulfide electrolytes have high conductivity, they have high manufacturing costs and face huge challenges in large-scale production and installation; polymer solid electrolytes are easy to process, but the battery is prone to short circuit; the ionic conductivity of oxide solid electrolytes is between polymers and sulfides, and the preparation difficulty is moderate, and it is easy to achieve iteration from semi-solid, quasi-solid, to all-solid batteries. However, in the related technology, oxide solid electrolytes have the problem of not being able to take into account the improvement of ionic conductivity and powder structure stability, which affects the rate performance and cycle performance of the battery. Summary of the invention

[0003] The present application aims to solve one of the technical problems in the related art at least to some extent.

[0004] In the first aspect of the present application, a solid electrolyte material is provided, wherein the solid electrolyte material is a NASICON crystal structure, and in the X-ray diffraction spectrum of the solid electrolyte material, there are characteristic diffraction peaks at diffraction angles 2θ values ​​of 14.5°-14.8°, 19.5°-19.7°, and 22.5°-22.8°, respectively, wherein the ratio of the peak intensity I1 of the characteristic diffraction peak at 2θ values ​​of 14.5°-14.8° to the peak intensity I2 of the characteristic diffraction peak at 2θ values ​​of 22.5°-22.8° satisfies: 1.5≤I2 / I1≤3. Thus, a composite crystal structure having both hexagonal and monoclinic systems is formed, and at the same time, the solid electrolyte material contains phosphate and pyrophosphate as the skeleton of the solid electrolyte material, which can improve the structural stability of the solid electrolyte material, reduce the binding of carriers, and improve the mobility of carriers, thereby improving the ionic conductivity of the solid electrolyte material and the rate performance of the battery.

[0005] According to some embodiments of the present application, in the X-ray diffraction spectrum of the solid electrolyte material, there is a characteristic diffraction peak I3 at 2θ of 17.8°-18.0° and / or 23.7°-23.9° and / or 26.8°-27.0°. Thus, the solid electrolyte material contains phosphate, pyrophosphate and heteropoly acid as the skeleton of the solid electrolyte material, which can further improve the structural stability of the solid electrolyte material, reduce the binding of carriers, and improve the mobility of carriers, thereby improving the ionic conductivity of the solid electrolyte and improving the rate performance of the battery.

[0006] According to some embodiments of the present application, the X-ray diffraction spectrum of the solid electrolyte material has a crystal plane along the <113> Preferred orientation, the ratio of the peak intensity of the diffraction peak (113) and the diffraction peak (104) satisfies I(113) / I(104)≥2, preferably 2≤I(113) / I(104)≤4; the 2θ value corresponding to the diffraction peak (113) of the X-ray diffraction spectrum is 24.3°-24.6°, the half-peak width range is 0.170-0.172, and the 2θ value corresponding to the diffraction peak (104) is 20.7°-20.9°, and the half-peak width range is 0.180-0.184. Thus, the content of the dominant crystal plane (113) in the solid electrolyte material is increased, the carrier transmission channel is widened, the carrier transmission rate is increased, and the ionic conductivity of the solid electrolyte material is thereby increased.

[0007] According to some embodiments of the present application, the solid electrolyte material has a charge and discharge platform at 2.4V-2.6V.

[0008] According to some embodiments of the present application, the solid electrolyte material includes: Li x M 1 y M 2 z M 3 u (PO4) w1 (P2O7) w2 (RO v ) w3 , where M 1 Including at least one of Mg, Na, K, optionally, M 1 including at least one of Mg or K; M 2 Includes at least one of Al, Ga, In, Y, and Sc, and optionally, M 2 Includes at least one of Al or Y; M 3Including at least one of Ti, Zr, Ge; R includes at least one of Mo, W, Si, Cl, Br, S, Sb, Sn, F, P, optionally, R includes at least one of Si, Mo or W; 0<x≤5, 0≤y≤0.5, 0≤z≤1, 0≤u≤9, 0≤v≤4, 1≤w1≤3, 0<w2≤2.3, 0<w3≤3, w1+w2+w3=3. Thus, the solid electrolyte material has phosphate, pyrophosphate and heteropoly acid as the skeleton at the same time, which can improve the structural stability of the solid electrolyte material, reduce the binding of carriers, improve the mobility of carriers, and thus improve the ionic conductivity of the solid electrolyte and the rate performance of the battery.

[0009] According to some embodiments of the present application, the solid electrolyte material satisfies at least one of the following conditions:

[0010] The ionic conductivity of the solid electrolyte material is greater than or equal to 1×10 -3 S / cm, can be selected to be greater than or equal to 2×10 -3 S / cm;

[0011] The average particle size of the solid electrolyte material is 0.5 μm-20 μm, and can be 0.5 μm-0.9 μm;

[0012] At 25°C, the pH of the solid electrolyte material is 6-10;

[0013] The surface of the solid electrolyte material includes residual lithium, and the residual lithium includes at least one of dilithium hydrogen phosphate, lithium dihydrogen phosphate, lithium carbonate, and lithium pyrophosphate. Based on the total mass of the solid electrolyte material, the mass proportion of the dilithium hydrogen phosphate is a, the mass proportion of the lithium dihydrogen phosphate is b, the mass proportion of the lithium carbonate is c, and the mass proportion of the lithium pyrophosphate is d, and the following conditions are satisfied: 0≤a≤0.5%, 0≤b≤0.1%, 0≤c≤0.3%, and 0≤d≤0.2%.

[0014] The second aspect of the present application provides a method for preparing the solid electrolyte material provided in the first aspect of the present application, comprising: 2 Source, M 3 Source, PO4 3- The first precursor is obtained by mixing the first precursor and the R source, and performing a first sintering in an oxygen-containing atmosphere to obtain a second precursor; the second precursor, the Li source, and the M 1 Source, P2O7 4-The solid electrolyte material is prepared by mixing the solid electrolyte material with the source and performing a second sintering in an oxygen-free atmosphere to obtain the solid electrolyte material. Thus, the solid electrolyte material prepared by the method has all the characteristics and advantages of the aforementioned solid electrolyte material, which will not be described in detail here. In general, it has at least the advantages of high ion conductivity and good structural stability.

[0015] According to some embodiments of the present application, the method further includes: 2 Source, the M 3 Source, the PO4 3- The source, the surfactant, the precipitant and the solvent are mixed, and the first precursor is obtained after co-precipitation and filtration; optionally, based on the PO4 3- The total mass of the source, the mass proportion of the surfactant is ≥ 0.1%, which can be 0.1%-1%, and further can be 0.3%-0.7%; optionally, the surfactant includes at least one of polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate, and sulfonate. Thus, the formation energy of the first precursor produced along the dominant crystal plane is reduced, the proportion of the dominant crystal plane is increased, the diffusion rate of lithium ions is increased, and the ionic conductivity of the solid electrolyte material is increased.

[0016] According to some embodiments of the present application, the method satisfies at least one of the following conditions:

[0017] The oxygen-containing atmosphere includes oxygen or air; the temperature of the first sintering is 700° C.-900° C., and the time of the first sintering is 4 h-10 h;

[0018] The oxygen-free atmosphere includes an inert gas or nitrogen; the temperature of the second sintering is 450° C.-700° C., and the time of the second sintering is 8 h-20 h;

[0019] The M 1 Sources include M 1 At least one of oxides, phosphates, sulfates, chlorides, nitrates and carbonates;

[0020] The M 2 Sources include M 2 At least one of phosphate, acetate, sulfate, chloride, nitrate, and carbonate;

[0021] The M 3 Sources include M 3 At least one of phosphate, acetate, sulfate, chloride, nitrate, and carbonate;

[0022] The PO4 3-The source includes at least one of H3PO4, NH4H2PO4, (NH4)2HPO4, (NH4)3PO4, LiH2PO4, Li2HPO4, Li3PO4, NaH2PO4, Na2HPO4, and Na3PO4;

[0023] The Li source includes at least one of lithium carbonate, lithium hydroxide and lithium nitrate;

[0024] The P2O7 4- The source includes at least one of H4P2O7, (NH4)2H2P2O7, Li2H2P2O7, and Li4P2O7;

[0025] The R source includes at least one of a simple substance, an oxide, and a hydride containing R; the precipitant includes at least one of sodium hydroxide, sodium carbonate, and ammonia water.

[0026] The third aspect of the present application provides a positive electrode active material, including the solid electrolyte material provided in the first aspect of the present application or the solid electrolyte material prepared by the method provided in the second aspect of the present application; optionally, the positive electrode active material includes a substrate, at least part of the surface of the substrate has a coating layer, and the coating layer includes the solid electrolyte material; optionally, based on the total mass of the substrate, the mass proportion of the solid electrolyte material is 0.05%-1%.

[0027] The fourth aspect of the present application provides a positive electrode plate, comprising the positive electrode active material provided in the third aspect of the present application.

[0028] The fifth aspect of the present application provides a solid-state battery, including the positive electrode plate provided by the fourth aspect of the present application.

[0029] The sixth aspect of the present application provides an electrical device, including the solid-state battery provided in the fifth aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0031] Figure 1 A schematic diagram of a process for preparing a solid electrolyte material according to an embodiment of the present application is shown.

[0032] Figure 2 The XRD test spectrum of the solid electrolyte material prepared in Example 3 is shown.

[0033] Figure 3 The XRD test spectrum of the solid electrolyte material prepared in Example 5 is shown.

[0034] Figure 4The XRD test spectrum of the solid electrolyte material prepared in Comparative Example 1 is shown.

[0035] Figure 5 The XRD test spectrum of the solid electrolyte material prepared in Example 2 is shown.

[0036] Figure 6 The discharge curve of the solid electrolyte material prepared in Example 2 is shown. DETAILED DESCRIPTION

[0037] The embodiments of the present application are described in detail below. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific technology or conditions are indicated in the embodiments, the technology or conditions described in the document in this area or the product specification are used. The reagents used or the instruments that do not indicate the manufacturer are all conventional products that can be obtained commercially.

[0038] In a first aspect, the present application provides a solid electrolyte material, the solid electrolyte material is a NASICON crystal structure, and in the X-ray diffraction spectrum of the solid electrolyte material, there are characteristic diffraction peaks at diffraction angles 2θ of 14.5°-14.8°, 19.5°-19.7°, and 22.5°-22.8°, respectively, wherein the ratio of the peak intensity I1 of the characteristic diffraction peak at 2θ of 14.5°-14.8° to the peak intensity I2 of the characteristic diffraction peak at 2θ of 22.5°-22.8° satisfies: 1.5≤I2 / I1≤3. Thus, the structural stability and ionic conductivity of the solid electrolyte material are improved at the same time, and the rate performance of the battery is improved.

[0039] The following is a detailed description of the principle by which the present application can achieve the above beneficial effects:

[0040] The solid electrolyte material proposed in this application has a characteristic diffraction peak of phosphate at 14.5°-14.8° of 2θ value in the X-ray diffraction spectrum, and a characteristic diffraction peak of pyrophosphate at 2θ value of 22.5°-22.8°, indicating that the solid electrolyte material contains both pyrophosphate and phosphate as a skeleton. Specifically, the bond energy between phosphate and metal elements is relatively strong, and the probability of phase change of the crystal structure can be reduced during the transmission of metal ions (taking lithium ions as an example), the structural stability of the solid electrolyte material can be improved, and the precipitation of lithium ions at positions such as the bulk, grain boundaries, and surfaces of the solid electrolyte material can be reduced; and the bond energy between pyrophosphate and metal elements is lower than that between phosphate and metal elements, and the presence of pyrophosphate can weaken the restraint on lithium ions, improve the mobility of lithium ions, and thus improve the migration rate of lithium ions, improve the ionic conductivity of the solid electrolyte material, and improve the rate performance of the battery. At the same time, the present application optimizes the content of phosphate and pyrophosphate in the solid electrolyte material by making the ratio of I2 / I1 within the above range to further improve the structural stability and ionic conductivity of the solid electrolyte material. On this basis, the characteristic diffraction peak at 2θ value of 19.5°-19.7° indicates that the solid electrolyte material has both hexagonal and monoclinic systems. The presence of the monoclinic crystal structure makes the unit cell parameters of the solid electrolyte material relatively large, and the anion binding during lithium ion transmission is weakened, which can further improve the ionic conductivity of the solid electrolyte material.

[0041] In the present application, the X-ray diffraction test method is to use an X-ray automatic diffractometer to perform phase and crystal structure analysis, with an operating voltage of 40kV, an operating current of 250mA, continuous scanning, a scanning speed of 4° / min, a step size of 0.02°, and a scanning angle of 10°-80°.

[0042] As an example, I2 / I1 may be 1.5, 2, 2.5 or 3, etc., or may be a range consisting of any of the above values.

[0043] According to some embodiments of the present application, in the X-ray diffraction spectrum of the solid electrolyte material, there is a characteristic diffraction peak I3 at a 2θ value of 17.8°-18.0° and / or 23.7°-23.9° and / or 26.8°-27.0°. For example, when the solid electrolyte material contains molybdate, there is a characteristic diffraction peak at a 2θ value of 17.8°-18.0°, when the solid electrolyte material contains tungstate, there is a characteristic diffraction peak at a 2θ value of 23.7°-23.9°, and when the solid electrolyte material contains silicate, there is a characteristic diffraction peak at a 2θ value of 26.8°-27.0°. That is to say, the heteropolyacid is doped at the phosphate position, and cooperates with the pyrophosphate and phosphate skeleton structures. When phosphate, pyrophosphate and heteropolyacid are contained at the same time, the stability of the skeleton and the widening of the ion channel can be better balanced. Specifically, based on the weak bond energy between pyrophosphate and heteropolyacid and metal elements, compared with phosphate, it can further weaken the binding of lithium ions, improve the mobility of lithium ions, and then increase the migration rate of lithium ions, improve the ionic conductivity of solid electrolyte materials, and improve the rate performance of batteries. Compared with phosphate doped with pyrophosphate, it can have better skeleton stability, reduce the probability of phase change of crystal structure during lithium ion transmission, and improve the cycle performance of batteries.

[0044] According to some embodiments of the present application, the X-ray diffraction spectrum of the solid electrolyte material has a crystal plane along the <113> Preferred orientation, the ratio of the peak intensity of the diffraction peak (113) and the diffraction peak (104) satisfies I(113) / I(104)≥2; the 2θ value corresponding to the diffraction peak (113) of the X-ray diffraction spectrum is 24.3°-24.6°, the half-peak width range is 0.170-0.172, and the 2θ value corresponding to the diffraction peak (104) is 20.7°-20.9°, and the half-peak width range is 0.180-0.184. Therefore, by making I(113) / I(104)≥2, the content of the 113 crystal plane can be increased, thereby increasing the transmission channel of lithium ions, increasing the transmission rate of lithium ions, and thereby improving the ionic conductivity of the solid electrolyte. When the half-peak widths of the diffraction peaks corresponding to the diffraction peaks (113) and the diffraction peaks (104) are within the range, it has better crystallization performance, thereby obtaining better structural stability.

[0045] As an example, I(113) / I(104) may be 2, 2.5, 3, 3.5, 4, 4.5 or 5, or may be a range consisting of any of the above values. According to some embodiments of the present application, 2≤I(113) / I(104)≤4.

[0046] According to some embodiments of the present application, the solid electrolyte material has a charge and discharge platform at 2.4V-2.6V.

[0047] According to some embodiments of the present application, the solid electrolyte material may include Li x M 1 y M 2 z M 3 u (PO4) w1 (P2O7) w2 (RO v ) w3 , where M 1 Includes at least one of Mg, Na, and K; M 2 Includes at least one of Al, Ga, In, Y, and Sc; M 3 Including at least one of Ti, Zr, Ge; R includes at least one of Mo, W, Si, Cl, Br, S, Sb, Sn, F, P; 0<x≤5, 0≤y≤0.5, 0≤z≤1, 0≤u≤9, 0≤v≤4, 1≤w1≤3, 0<w2≤3, 0<w3≤3, w1+w2+w3=3. Therefore, the solid electrolyte material simultaneously uses phosphate, pyrophosphate and heteropoly acid as the skeleton of the solid electrolyte material, the bond energy between phosphate and metal elements is relatively strong, the probability of phase change of crystal structure can be reduced during lithium ion transmission, the structural stability of the solid electrolyte material is improved, and the precipitation of lithium in the bulk phase, grain boundary, surface and other positions of the solid electrolyte material is reduced. At the same time, pyrophosphate and heteropolyacid are used to replace part of the phosphate as the skeleton. Since the bond energy between pyrophosphate and heteropolyacid and metal elements is lower than the bond energy between phosphate and metal elements, the binding of lithium ions can be weakened, the mobility of lithium ions can be improved, and the migration rate of lithium ions can be improved, thereby improving the ionic conductivity of solid electrolyte materials. The solid electrolyte material has both hexagonal and monoclinic crystal systems. The presence of the monoclinic crystal structure makes the unit cell parameters of the solid electrolyte material relatively large, and the anion binding of lithium ions is weakened during the transmission process, thereby improving the ionic conductivity of the solid electrolyte material. In addition, the present application has a transition metal site (M 3 ) doped with M 2 , Li-doped M 1 Afterwards, based on M 2 Compared to M 3 The change in valence of M 1 Compared with the change in the valence of lithium ions, in order to maintain electrical neutrality, the Li content in the unit cell of the solid electrolyte material increases, which can increase the transmission channels of lithium ions, increase the transmission rate of lithium ions, further improve the ionic conductivity of the solid electrolyte material, and improve the rate performance of the battery.

[0048] As an example, 0<x≤5, for example, it can be 0.5, 1, 2, 3, 4 or 5, or it can be a composition range of any of the above values. Thus, the content of lithium in the solid electrolyte material is increased, the number of lithium ions is increased, and then the transmission channel of lithium ions is increased, the transmission rate of lithium ions is increased, and the ionic conductivity of the solid electrolyte material is increased. According to some specific embodiments of the present application, 1≤x≤4.

[0049] As an example, 0≤y≤0.5, for example, can be 0, 0.1, 0.2, 0.3, 0.4 or 0.5, or can be a range of any of the above values. Thus, the ionic conductivity of the solid electrolyte material is improved. According to some specific embodiments of the present application, 0<y≤0.01.

[0050] As an example, 0≤z≤1, for example, can be 0, 0.2, 0.4, 0.6, 0.8 or 1, or can be a range of any of the above values. 3 ) doped with M 2 Afterwards, based on M 2 Compared to M 3 In order to maintain electrical neutrality, the content of Li in the solid electrolyte material unit cell increases, thereby increasing the transmission channel of lithium ions, improving the transmission rate of lithium ions, further improving the ionic conductivity of the solid electrolyte material, and improving the rate performance of the battery. According to some specific embodiments of the present application, 0.1≤z≤0.8.

[0051] As an example, 0≤u≤9, for example, it can be 0, 1, 2, 3, 4, 5, 6, 7, 8 or 9, or can be a range consisting of any of the above values. 3 It can be used as an element constituting the skeleton structure of solid electrolyte materials, through the synergistic effect of the heterovalent element M 1 、M 2 The doping can increase the carrier concentration, increase the carrier transport sites, improve the carrier mobility, and thus improve the intrinsic ionic conductivity of the solid electrolyte material. According to some specific embodiments of the present application, 1≤u≤3.

[0052] As an example, 0≤v≤4, for example, can be 0, 1, 2, 3 or 4, or can be a range consisting of any of the above values. According to some specific embodiments of the present application, 0<v<4.

[0053] As an example, 1≤w1≤3, for example, can be 1, 1.5, 2, 2.5 or 3, or can be a range of any of the above values. Thus, phosphate, as the skeleton of the solid electrolyte material, can enhance the binding of the metal element due to the strong bond energy between the phosphate and the metal element, reduce the probability of phase change of the crystal structure during lithium ion transmission, improve the structural stability of the solid electrolyte material, and keep the solid electrolyte material at a low lithium precipitation in the bulk phase, grain boundary, surface and other locations.

[0054] As an example, 0<w2≤2.3, for example, it can be 0.5, 1, 1.5, 2 or 2.3, or it can be a range of any of the above values. Therefore, pyrophosphate is used to replace part of the phosphate as the skeleton of the solid electrolyte material. Since the bond energy between the pyrophosphate and the metal element is weaker than the bond energy between the phosphate and the metal element, it can reduce the binding of the carriers, reduce the transmission barrier of the carriers, and increase the transmission rate of the carriers, thereby improving the ionic conductivity of the solid electrolyte material. At the same time, by doping M in the solid electrolyte material 2 and M 3 , which can improve the structural stability of the solid electrolyte material and reduce the probability of phase change of the solid electrolyte material. According to some specific embodiments of the present application, 0.1<w2≤1.

[0055] As an example, 0<w3≤3, for example, it can be 0.5, 1, 1.5, 2, 2.5 or 3, or it can be a range of any of the above values. Therefore, by using heteropoly acid to replace part of the phosphate as the skeleton of the solid electrolyte material, since the bond energy between the heteropoly acid and the metal element is weaker than the bond energy between the phosphate and the metal element, it can reduce the binding of the carriers, reduce the transmission barrier of the carriers, and increase the transmission rate of the carriers, thereby improving the ionic conductivity of the solid electrolyte material. At the same time, by doping M in the solid electrolyte material 2 and M 3 , which can improve the structural stability of the solid electrolyte material and reduce the probability of phase change of the solid electrolyte material. According to some specific embodiments of the present application, 0<w3≤1.5.

[0056] As an example, M 1 At least one of Mg or K may be included.

[0057] As an example, M 2 At least one of Al or Y may be included.

[0058] As an example, R may include at least one of Si, Mo, or W.

[0059] According to some embodiments of the present application, the ionic conductivity of the solid electrolyte material is greater than or equal to 1×10- 3 S / cm, for example, can be 1×10 -3 S / cm, 2×10 -3 S / cm, 2.5×10 -3 S / cm or 3×10 -3 S / cm, etc., or can be a range of any of the above values. Thus, the transfer rate of lithium ions by the solid electrolyte material is improved, and the rate performance of the battery is improved. According to some specific embodiments of the present application, the ionic conductivity of the solid electrolyte material is greater than or equal to 2×10 -3 S / cm.

[0060] In the present application, the test method for ionic conductivity is to mold 5 mg of solid electrolyte material into a sheet sample at 200 MPa pressure in a steel mold with a diameter of 12 mm, and then place the molded sheet sample in a fixture to perform an AC impedance test on an electrochemical workstation to obtain the ionic conductivity.

[0061] According to some embodiments of the present application, the average particle size of the solid electrolyte material can be 0.5 μm-20 μm, for example, 0.5 μm, 1 μm, 5 μm, 10 μm, 15 μm or 20 μm, etc., or can be a range composed of any of the above numerical values. Thus, the solid electrolyte material can take into account both good dispersibility and high ionic conductivity. According to some specific embodiments of the present application, the average particle size of the solid electrolyte material can be 0.5 μm-0.9 μm.

[0062] In the present application, the method for testing the average particle size of the solid electrolyte material is to disperse and test its particle size distribution in a water solvent using a laser particle size analyzer.

[0063] According to some embodiments of the present application, at 25°C, the pH of the solid electrolyte material is 6-10. For example, it can be 6, 7, 8, 9 or 10, or it can be a range composed of any of the above values. Thus, by making the pH in the above range, the structural stability of the solid electrolyte material is improved, and the influence of structural instability on ionic conductivity is reduced. At the same time, the solid electrolyte material has a sufficient amount of lithium to improve the purity and ionic conductivity of the solid electrolyte material.

[0064] According to some embodiments of the present application, the surface of the solid electrolyte material includes residual lithium, and the residual lithium includes at least one of lithium dihydrogen phosphate, lithium dihydrogen phosphate, lithium carbonate, and lithium pyrophosphate. Based on the total mass of the solid electrolyte material, the mass proportion of the lithium dihydrogen phosphate is a, the mass proportion of the lithium dihydrogen phosphate is b, the mass proportion of the lithium carbonate is c, and the mass proportion of the lithium pyrophosphate is d, and the following conditions are satisfied: 0≤a≤0.5%, 0≤b≤0.1%, 0≤c≤0.3%, and 0≤d≤0.2%. Thus, by testing the type of residual lithium, it can be inferred that the composition of the product must contain pyrophosphate, and the content of residual lithium is within the above range, thereby reducing the probability of lithium inside the solid electrolyte material continuously precipitating to the surface and improving the structural stability of the solid electrolyte material.

[0065] As an example, 0≤a≤0.5%, for example, it can be 0, 0.1%, 0.2%, 0.3%, 0.4% or 0.5%, etc., or can be a range consisting of any of the above values.

[0066] As an example, 0≤b≤0.1%, for example, it can be 0, 0.02%, 0.04%, 0.06%, 0.08% or 0.1%, etc., or can be a range consisting of any of the above values.

[0067] As an example, 0≤c≤0.3%, for example, it can be 0, 0.05%, 0.1%, 0.15%, 0.2%, 0.25% or 0.3%, etc., or it can be a range consisting of any of the above values.

[0068] As an example, 0≤d≤0.2%, for example, it can be 0, 0.05%, 0.1%, 0.15% or 0.2%, etc., or it can be a range consisting of any of the above values.

[0069] The test method for the type and content of residual lithium in this application is: accurately weigh 5.0000g of the sample to be tested in a 150.0mL beaker, and the sample mass is recorded as m 样品 . Add 100.0g pure water and a stirring magnet to the beaker of the sample to be tested, seal it with plastic wrap, and place it on a magnetic stirrer for stirring. Use a dry suction filter to filter the sample solution in the above step to obtain a filtrate. In a 100.0mL beaker, add a stirring magnet, accurately weigh 60.0000g of the filtrate for titration, record it as m 滤液 . Titrate the filtrate to the endpoint with 0.1000mol / L hydrochloric acid standard solution. When the test is over and the number of jump points is 2, record the volume V corresponding to the jump points EP1 and EP2 正1 、V 正2 ; When the test is over and the number of jump points is 3, record the volume V corresponding to the jump points EP1, EP2, and EP3 正1 、V 正2 、V正3 The above titrated solution is titrated to the endpoint with 0.1000 mol / L sodium hydroxide standard solution, and the volume V corresponding to the jump points EP1 and EP2 is recorded. 反1 、V 反2 、V 反3 According to the results of forward and reverse droplet, the corresponding types and contents of residual lithium are calculated in combination with Table 1.

[0070] Table 1

[0071]

[0072] Table 2

[0073]

[0074] The second aspect of the present application provides a method for preparing the solid electrolyte material of the first aspect of the present application, comprising: 2 Source, M 3 Source, PO4 3- A source, a precipitant, and a solvent are mixed, and a first precursor is obtained after coprecipitation and filtration; the first precursor, M 1 The second precursor, Li source, P2O7 4- The solid electrolyte material is prepared by mixing the solid electrolyte material with the source and performing a second sintering in an oxygen-free atmosphere to obtain the solid electrolyte material. Thus, the solid electrolyte material prepared by the method has all the characteristics and advantages of the aforementioned solid electrolyte material, which will not be described in detail here. In general, it has at least the advantages of high ion conductivity and good structural stability.

[0075] The following is a detailed description of this method, see Figure 1 , the method comprising:

[0076] S100: M 2 Source, M 3 Source, PO4 3- Source mixing to prepare the first precursor

[0077] According to some embodiments of the present application, M 2 Source, M 3 Source, PO4 3- The source, precipitant and solvent are mixed, and the first precursor is obtained after co-precipitation and filtration.

[0078] According to some embodiments of the present application, the M 2 Source, the M 3 Source, the PO4 3-The first precursor is obtained by mixing the source, the surfactant, the precipitant and the solvent, co-precipitating and filtering. Thus, by adding the surfactant, the formation energy of the dominant crystal plane can be reduced, the proportion of the dominant crystal plane corresponding to the lithium ion transmission channel can be increased, and the transmission rate of lithium ions can be increased, and finally the ion conductivity of the solid electrolyte material can be improved.

[0079] According to some embodiments of the present application, based on the PO4 3- The total mass of the source, the mass proportion of the surfactant can be greater than or equal to 0.1%, for example, it can be 0.1%, 0.3%, 0.5%, 0.7%, 0.9%, 1%, 1.5% or 2%, or it can be a range composed of any of the above values. Therefore, by making the type of surfactant within the above range, the proportion of the dominant crystal plane can be increased, the transmission rate of lithium ions can be increased, and the ionic conductivity of the solid electrolyte material can be increased. According to some specific embodiments of the present application, based on the PO4 3- The total mass of the source, the mass proportion of the surfactant can be 0.1%-1%. According to other specific embodiments of the present application, based on the PO4 3- The mass of the surfactant may account for 0.3%-0.7% of the total mass of the source.

[0080] According to some embodiments of the present application, the surfactant includes at least one of polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate, and sulfonates. Thus, by selecting the above types of surfactants, the formation energy of the dominant crystal plane corresponding to the lithium ion transmission channel can be reduced, the proportion of the dominant crystal plane can be increased, and the transmission rate of lithium ions can be increased, and finally the ionic conductivity of the solid electrolyte material can be improved.

[0081] According to some embodiments of the present application, the M 2 Sources include M 2 At least one of phosphate, acetate, sulfate, chloride, nitrate and carbonate.

[0082] According to some embodiments of the present application, the M 3 Sources include M 3 At least one of phosphate, acetate, sulfate, chloride, nitrate and carbonate.

[0083] According to some embodiments of the present application, the PO4 3- The source includes at least one of H3PO4, NH4H2PO4, (NH4)2HPO4, (NH4)3PO4, LiH2PO4, Li2HPO4, Li3PO4, NaH2PO4, Na2HPO4, and Na3PO4.

[0084] According to some embodiments of the present application, the precipitant includes at least one of sodium hydroxide, sodium carbonate, and ammonia water.

[0085] According to some embodiments of the present application, the solvent includes at least one of pure water, alcohols, and ethers.

[0086] S200: Mix the first precursor and the R source and perform a first sintering to obtain a second precursor.

[0087] According to some embodiments of the present application, the first precursor and the R source are mixed and sintered for the first time in an oxygen-containing atmosphere to obtain a second precursor.

[0088] According to some embodiments of the present application, the oxygen-containing atmosphere includes oxygen or air.

[0089] According to some embodiments of the present application, the temperature of the first sintering may be 700° C.-900° C., and the time of the first sintering may be 4 h-10 h.

[0090] As an example, the temperature of the first sintering may be 700° C., 750° C., 800° C., 850° C. or 900° C., or may be a range consisting of any of the above values.

[0091] As an example, the first sintering time may be 4 h-10 h, for example, 4 h, 6 h, 8 h or 10 h, or may be within a range consisting of any of the above values.

[0092] Therefore, by making the temperature and time of the first sintering within the above range, a phosphate-heteropolyacid composite precursor with high purity and stable structure can be formed, and the particles are kept within a limited range, thereby maintaining a high ionic conductivity.

[0093] According to some embodiments of the present application, the M 1 Sources include M 1 At least one of oxides, phosphates, sulfates, chlorides, nitrates, and carbonates.

[0094] According to some embodiments of the present application, the R source includes at least one of a simple substance, an oxide, and a hydride containing R.

[0095] S300: The second precursor, Li source, M 1 Source, P2O7 4- The source mixture is sintered for the second time in an oxygen-free atmosphere

[0096] According to some embodiments of the present application, the second precursor, Li source, M 1 Source, P2O7 4- The source mixture is sintered a second time in an oxygen-free atmosphere.

[0097] According to some embodiments of the present application, the temperature of the second sintering may be 450° C.-700° C., and the time of the second sintering may be 8 h-20 h.

[0098] As an example, the temperature of the second sintering may be 450° C., 500° C., 550° C., 600° C., 650° C. or 700° C., or may be a range consisting of any of the above values.

[0099] As an example, the second sintering time is 8h-20h, for example, it can be 8h, 10h, 12h, 14h, 16h, 18h or 20h, etc., or can be a range consisting of any of the above values.

[0100] Therefore, by making the temperature and time of the second sintering within the above range, it is possible to ensure that a phosphate-heteropolyacid-pyrophosphate composite phase with high purity and stable structure is formed, and the particles are kept within a limited range, thereby maintaining a high ionic conductivity.

[0101] According to some embodiments of the present application, the oxygen-free atmosphere includes an inert gas or nitrogen. Thus, by performing the second sintering in an oxygen-free atmosphere, the probability of pyrophosphate being converted into phosphate can be reduced, and the content of pyrophosphate in the solid electrolyte material can be increased.

[0102] According to some embodiments of the present application, the P2O7 4- The source includes at least one of H4P2O7, (NH4)2H2P2O7, Li2H2P2O7, and Li4P2O7.

[0103] According to some embodiments of the present application, the Li source includes at least one of lithium carbonate, lithium hydroxide, and lithium nitrate.

[0104] According to some embodiments of the present application, the method may further include performing nano-processing on the solid electrolyte material.

[0105] As an example, the solid electrolyte material may be nano-processed by ball milling.

[0106] According to some embodiments of the present application, the nano-processing may include: mixing the solid electrolyte material with a solvent to form a slurry, performing sand milling, drying, and dissociation to obtain a nano-scale solid electrolyte material.

[0107] As an example, the mass proportion of the solid electrolyte material in the slurry can be 10%-70%, for example, 10%, 20%, 30%, 40%, 50%, 60% or 70%, etc., or can be a range composed of any of the above values. According to some specific embodiments of the present application, the mass proportion of the solid electrolyte material in the slurry can be 30%-60%.

[0108] According to some embodiments of the present application, the drying temperature may be 80°C-400°C, for example, 80°C, 100°C, 150°C, 200°C, 250°C, 300°C, 350°C or 400°C, or a range of any of the above values. According to some specific embodiments of the present application, the first drying

[0109] According to some embodiments of the present application, the drying time may be 0.1h-10h, for example, 0.1h, 1h, 3h, 5h, 7h, 9h or 10h, etc., or may be a range of any of the above values. According to some embodiments of the present application, the drying time may be 0.5h-3h.

[0110] According to some embodiments of the present application, the drying equipment may include at least one of a spray dryer, a fluidized bed dryer, a belt dryer, and a flash dryer.

[0111] According to some embodiments of the present application, the average particle size of the nano-sized solid electrolyte material may be less than or equal to 200 nm, specifically, may be 5 nm-100 nm.

[0112] According to some embodiments of the present application, the dissociation equipment may include at least one of a jet mill, a mechanical mill and a colloid mill.

[0113] The third aspect of the present application provides a positive electrode active material, including the solid electrolyte material provided in the first aspect of the present application or the solid electrolyte material prepared by the method provided in the second aspect of the present application.

[0114] According to some embodiments of the present application, the positive electrode active material includes a substrate, at least part of the surface of the substrate has a coating layer, and the coating layer includes the solid electrolyte material. Thus, by forming the solid electrolyte material on at least part of the surface of the substrate, the ionic conductivity of the positive electrode active material can be improved due to the high ionic conductivity of the solid electrolyte material, thereby improving the rate performance of the battery.

[0115] According to some embodiments of the present application, based on the total mass of the matrix, the mass proportion of the solid electrolyte material can be 0.05%-1%. For example, it can be 0.05%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1%, etc., or it can be a range composed of any of the above values. Thus, by making the content of the solid electrolyte material within the above range, the ionic conductivity of the positive electrode active material can be improved, thereby improving the rate performance of the battery.

[0116] The fourth aspect of the present application provides a positive electrode plate, comprising the positive electrode active material provided in the third aspect of the present application.

[0117] The fifth aspect of the present application provides a solid-state battery, including the positive electrode plate provided by the fourth aspect of the present application.

[0118] The sixth aspect of the present application provides an electrical device, including the solid-state battery provided in the fifth aspect of the present application.

[0119] Example 1

[0120] Aluminum nitrate, titanyl sulfate, and disodium hydrogen phosphate were mixed according to the molar ratio of Al 3+ :Ti 4+ :PO4 3- =0.3:1.7:1.5 in pure water, add PVP (polyvinyl pyrrolidone) surfactant, based on the total mass of disodium hydrogen phosphate, the mass proportion of PVP is 0.5%, heat to 60°C and stir for 30 minutes to form a uniform precipitate, and obtain the powder of the first precursor after filtering and drying.

[0121] The first precursor and silicon dioxide are mixed according to Si 4+ :PO4 3- =1:1.5 ratio and mixed evenly in a high-speed mixer, and sintered at 800° C. for 6 hours in an air atmosphere to obtain a powder of the second precursor.

[0122] The second precursor, lithium carbonate, potassium carbonate and titanium pyrophosphate are mixed according to Li + :K + :P2O7 4- :PO4 3- =0.6:0.2:0.5:1.5 in a ratio of weighed and mixed evenly in a high-speed mixer, and sintered at 550° C. for 12 hours in a nitrogen atmosphere to obtain a micron-sized composite oxide solid electrolyte material.

[0123] The obtained micron-sized composite oxide solid electrolyte material was added into pure water to prepare a slurry with a solid content of 50%, and the slurry was milled with zirconium oxide balls in a ball mill for 6 hours to obtain a nano-slurry with an average particle size of less than 200 nm. The powder was treated by a spray dryer, and the powder was dissociated and sieved to finally obtain a relatively uniform particle size distribution with a composition of Li 0.6 K 0.2 Al 0.3 Ti 1.7 (SiO3)(P2O7) 0.5 (PO4) 1.5 Solid electrolyte nanopowder.

[0124] The preparation methods of Example 2-Example 11, Comparative Example 2, Comparative Example 3 and Comparative Example 4 are the same as those of Example 1, and the differences are detailed in Table 1.

[0125] Example 12

[0126] The preparation method is the same as that of Example 1, except that K element is not doped.

[0127] Embodiment 13

[0128] The preparation method is the same as that of Example 1, except that K element is not doped, and the first precursor, silicon dioxide, and molybdenum trioxide are mixed according to Si 4+ :PO4 3- :Mo 6+ =0.5:1:0.5 ratio weighed and mixed evenly in a high speed mixer.

[0129] Embodiment 14

[0130] The preparation method is the same as that of Example 1, except that the doped M 1 Elements: Na, M 1 The source is sodium carbonate, and M 1 Source, M 2 Source, M 3 Source, PO4 3- Source, P2O7 4- The R source, R source and lithium source are weighed according to the ratio of each element in the chemical formula.

[0131] Embodiment 15

[0132] The preparation method is the same as that of Example 1, except that the doped M 2 The elements are Y, M 2 The source is yttrium oxide, and M 1 Source, M 2 Source, M 3 Source, PO4 3- Source, P2O7 4- The R source, R source and lithium source are weighed according to the ratio of each element in the chemical formula.

[0133] Example 16

[0134] The preparation method is the same as that of Example 1, except that the doped M 3 Elements are Zr, M 2 The source is zirconium oxide, and M 1 Source, M 2 Source, M 3 Source, PO4 3- Source, P2O7 4- The R source, R source and lithium source are weighed according to the ratio of each element in the chemical formula.

[0135] Embodiment 17

[0136] The preparation method is the same as that of Example 1, except that the R source is molybdenum oxide, and during the preparation process, M 1 Source, M 2 Source, M 3 Source, PO4 3- Source, P2O7 4- The R source, R source and lithium source are weighed according to the ratio of each element in the chemical formula.

[0137] Comparative Example 1

[0138] (1) weighing Li2CO3, MgCO3, Al2O3, TiO2, ZrO2, and NH4H2PO4 compounds according to a stoichiometric ratio, adding a certain amount of pure water to mix, and then mixing and crushing them in a ball mill to obtain a mixed slurry A with a solid content of 50%; adding 55% by weight of acrylamide (monomer), (NH4)2S2O8 (initiator), and TEMED (catalyst) to the mixed slurry A, and evenly dispersing them in a stirring device to obtain a mixed slurry B;

[0139] (2) pouring the mixed slurry B into a sagger container and drying it in a 100° C. forced air oven to initiate a polymerization reaction of the substances in the mixed slurry B, and obtaining a bulk solid electrolyte precursor A after 12 hours;

[0140] (3) The solid electrolyte precursor A obtained in step (2) is pre-sintered at 550° C. in a muffle furnace for 2 hours, and the sintered product is crushed in a wall breaker at the highest level for 5 minutes to obtain a powdered solid electrolyte precursor B.

[0141] (4) Sintering the solid electrolyte precursor B obtained in step (3) at 800° C. for 6 hours in a muffle furnace, crushing the sintered product in a jet mill to obtain a powdery, micron-sized solid electrolyte Li 1.2 Mg 0.05 Al 0.3 Zr 0.05 Ti1.65 (PO4)3.

[0142] (5) The solid electrolyte Li obtained in step (4) 1.2 Mg 0.05 Al 0.3 Zr 0.05 Ti 1.65 (PO4)3 was mixed with pure water in a sand mill at 1000 rpm for 2 hours to obtain a nanoscale slurry with a solid content of 50%. The slurry was freeze-dried and the powder obtained after drying was further dissociated by a jet mill to obtain a powdery, nanoscale solid electrolyte material Li 1.2 Mg 0.05 Al 0.3 Zr 0.05 Ti 1.65 (PO4)3.

[0143]

[0144]

[0145] Preparation method of button battery: positive electrode material NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 O2), solid electrolyte, acetylene black and polyvinylidene fluoride (PVDF) were mixed in a mass ratio of 90:2:3:5, coated on aluminum foil and dried, and stamped into a positive electrode sheet with a diameter of 12mm and a thickness of 120μm at a pressure of 100MPa, and then placed in a vacuum drying oven and dried at 120℃ for 12h. The negative electrode used a Li metal sheet with a diameter of 17mm and a thickness of 1mm; the diaphragm used a Celgard 2400 porous membrane with a thickness of 25μm; the electrolyte used an equal mixture of 1mol / L LiPF6, ethylene carbonate (EC) and diethyl carbonate (DEC). The positive electrode sheet, diaphragm, negative electrode sheet and 4μL electrolyte were assembled into a 2025 button battery in an Ar gas glove box with a water content and an oxygen content of less than 5ppm.

[0146] Performance Testing Methods

[0147] 1. Test method for ionic conductivity of solid electrolyte materials

[0148] The test method for ionic conductivity is to mold 5 mg of nanopowder of solid electrolyte material into a sheet sample at 200 MPa pressure in a steel mold with a diameter of 12 mm, and then place the molded sheet sample in a fixture to perform AC impedance test on an electrochemical workstation to obtain ionic conductivity.

[0149] 2. Solid electrolyte structural stability test method

[0150] Take 5g of solid electrolyte material powder, place it in a beaker of 95g of pure water, stir and heat to 100°C for 5 minutes, then cool the beaker naturally to room temperature and filter it. Titrate the filtrate with standard hydrochloric acid solution to obtain the lithium content in the filtrate.

[0151] 3. XRD test method

[0152] The X-ray diffraction test method is to use an X-ray automatic diffractometer to perform phase and crystal structure analysis, with an operating voltage of 40 kV, an operating current of 250 mA, continuous scanning, a scanning speed of 4° / min, a step size of 0.02°, and a scanning angle of 10°-80°.

[0153] 4. Battery rate performance test method

[0154] The assembled battery was tested at 0.1C and 1C rates, and the ratio of the capacity at 1C rate to the capacity at 0.1C rate was calculated.

[0155] 5. Battery interface impedance test method

[0156] The assembled battery was measured in the electrochemical workstation using the AC impedance mode.

[0157] The test results of the batteries in Examples 1 to 17 and Comparative Examples 1 to 4 are shown in Table 2.

[0158]

[0159]

[0160] Conclusion: By comparing Examples 1 to 17 with Comparative Examples 1 to 4, it can be seen that the solid electrolyte material proposed in this application has the characteristics of high ion conductivity and low Li content in the filtrate, and the battery containing the solid electrolyte material proposed in this application has excellent rate performance and low interfacial impedance of the battery. This shows that by using phosphate, pyrophosphate and heteropolyacid as the skeleton of the solid electrolyte material, the mobility of carriers can be increased, and the probability of phase change of the crystal structure can be reduced during the carrier movement process, thereby improving the structural stability of the solid electrolyte material and improving the intrinsic ionic conductivity of the solid electrolyte material.

[0161] It can be seen from Examples 1 to 4 that by adding different contents of pyrophosphate to the solid electrolyte material, the mobility of carriers can be increased and the ionic conductivity of the solid electrolyte material can be improved.

[0162] It can be seen from the comparison between Example 5 and Examples 1 to 4 and Examples 6 to 17 that, in the process of preparing the solid electrolyte material, by adding a surfactant, the content of the dominant crystal face 113 can be increased, thereby increasing the transmission rate of lithium ions and improving the ionic conductivity of the solid electrolyte material.

[0163] It can be seen from Examples 6 to 11 that in the process of preparing solid electrolyte materials, by adding surfactants of different masses, the content of the dominant crystal face 113 in the solid electrolyte material can be adjusted, thereby increasing the lithium ion transmission rate and improving the ionic conductivity of the solid electrolyte material.

[0164] It can be seen from the comparison between Examples 1 to 17 and Comparative Example 3 that by adopting a double sintering process, a solid electrolyte material having both hexagonal and monoclinic crystal systems can be formed, and the binding of anions to lithium ions can be weakened during lithium ion transmission, thereby improving the ionic conductivity of the solid electrolyte material.

[0165] It can be seen from Examples 13 to 17 that different types of M can be doped into the solid electrolyte material. 1 Element, M 2 Element, M 3 element.

[0166] By the attached Figure 2 It can be seen that the characteristic diffraction peaks of phosphate, pyrophosphate and silicate exist in the XRD spectrum, indicating that the solid electrolyte material prepared in Example 3 has phosphate, pyrophosphate and heteropolyacid at the same time. The ratio of I(113) to I(104) is greater than 2, so the content of 113 crystal plane is relatively high, which can increase the transmission channel of lithium ions, improve the transmission rate of lithium ions, and thus improve the ionic conductivity of the solid electrolyte material.

[0167] By the attached Figure 3 It can be seen that the characteristic diffraction peaks of phosphate, pyrophosphate and silicate exist simultaneously in the XRD spectrum, indicating that the solid electrolyte material prepared in Example 5 has phosphate, pyrophosphate and heteropolyacid at the same time. The ratio of I(113) to I(104) is less than 2, so the content of 113 crystal plane in the solid electrolyte material in Example 5 is less than that in Example 3, and the transmission channels of lithium ions are less, so the ionic conductivity of the solid electrolyte material is lower than that in Example 3.

[0168] By the attached Figure 4It can be seen that only the characteristic diffraction peak of phosphate exists in the XRD spectrum, indicating that the solid electrolyte material in Comparative Example 1 has only phosphate. The ratio of I(113) to I(104) is less than 2, so the content of 113 crystal plane in the solid electrolyte material in Comparative Example 1 is small, and the transmission channels of lithium ions are small, so the ionic conductivity of the solid electrolyte is low.

[0169] By the attached Figure 5 It can be seen that the characteristic diffraction peaks of phosphate, pyrophosphate and silicate exist in the XRD spectrum at the same time, indicating that the solid electrolyte material prepared in Example 2 has phosphate, pyrophosphate and heteropolyacid at the same time. The ratio of I(113) to I(104) is greater than 2, so the content of 113 crystal plane is relatively high, which can increase the transmission channel of lithium ions, improve the transmission rate of lithium ions, and thus improve the ionic conductivity of the solid electrolyte. The characteristic diffraction peaks of the hexagonal phase and the monoclinic phase exist in the XRD spectrum at the same time, which can weaken the binding of anions during the transmission of lithium ions and further improve the ionic conductivity of the solid electrolyte material.

[0170] By the attached Figure 6 It can be seen that the solid electrolyte material prepared in Example 2 can be discharged.

[0171] In this application, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of this application, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0172] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0173] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A solid electrolyte material, characterized in that: include: Li x M 1 y M 2 z M 3 u (PO4) w1 (P2O7) w2 (RO v ) w3 , Among them, M 1 including at least one of Mg, Na, and K; M 2 Including at least one of Al, Ga, In, Y, and Sc; M 3 Includes at least one of Ti, Zr, and Ge; R includes at least one of Mo, W, Si, Cl, Br, S, Sb, Sn, F, and P; 0<x≤5, 0≤y≤0.5, 0≤z≤1, 0≤u≤9, 0≤v≤4, 1≤w1≤3, 0<w2≤2.3, 0<w3≤3, w1+w2+w3=3; The solid electrolyte material has a NASICON crystal structure. In the X-ray diffraction spectrum of the solid electrolyte material, there are characteristic diffraction peaks at diffraction angles 2θ of 14.5°-14.8°, 19.5°-19.7° and 22.5°-22.8°, respectively, wherein the ratio of the peak intensity I1 of the characteristic diffraction peak at the 2θ value of 14.5°-14.8° to the peak intensity I2 of the characteristic diffraction peak at the 2θ value of 22.5°-22.8° satisfies: 1.5≤I2 / I1≤3.

2. The solid electrolyte material according to claim 1, characterized in that Satisfy at least one of the following conditions: M 1 including at least one of Mg or K; M 2 including at least one of Al or Y; R includes at least one of Si, Mo, or W.

3. The solid electrolyte material according to claim 1 or 2, characterized in that: In the X-ray diffraction spectrum of the solid electrolyte material, there is a characteristic diffraction peak I3 at 2θ values ​​of 17.8°-18.0° and / or 23.7°-23.9° and / or 26.8°-27.0°.

4. The solid electrolyte material according to claim 3, characterized in that The X-ray diffraction spectrum of the solid electrolyte material shows that the crystal plane is along <113> Preferred orientation, the ratio of the peak intensity of the diffraction peak (113) to the diffraction peak (104) satisfies I (113) / I (104) ≥ 2; the 2θ value corresponding to the diffraction peak (113) of the X-ray diffraction spectrum is 24.3°-24.6°, and the half-peak width range is 0.170-0.172, and the 2θ value corresponding to the diffraction peak (104) is 20.7°-20.9°, and the half-peak width range is 0.180-0.

184.

5. The solid electrolyte material according to claim 4, characterized in that 2≤I(113) / I(104)≤4.

6. The solid electrolyte material according to claim 5, characterized in that The solid electrolyte material has a charge and discharge platform at 2.4V-2.6V.

7. The solid electrolyte material according to claim 6, characterized in that Satisfy at least one of the following conditions: The ionic conductivity of the solid electrolyte material is greater than or equal to 1×10 -3 S / cm; The average particle size of the solid electrolyte material is 0.5 μm-20 μm; At 25°C, the pH of the solid electrolyte material is 6-10; The surface of the solid electrolyte material includes residual lithium, and the residual lithium includes at least one of dilithium hydrogen phosphate, lithium dihydrogen phosphate, lithium carbonate, and lithium pyrophosphate. Based on the total mass of the solid electrolyte material, the mass proportion of the dilithium hydrogen phosphate is a, the mass proportion of the lithium dihydrogen phosphate is b, the mass proportion of the lithium carbonate is c, and the mass proportion of the lithium pyrophosphate is d, and the following conditions are satisfied: 0≤a≤0.5%, 0≤b≤0.1%, 0≤c≤0.3%, and 0≤d≤0.2%.

8. The solid electrolyte material according to claim 7, characterized in that Satisfy at least one of the following conditions: The ionic conductivity of the solid electrolyte material is greater than or equal to 2×10 -3 S / cm; The average particle size of the solid electrolyte material is 0.5 μm-0.9 μm.

9. A method for preparing the solid electrolyte material according to any one of claims 1 to 8, characterized in that: include: M 2 Source, M 3 Source, PO4 3- The source, the precipitant and the solvent are mixed, and a first precursor is obtained after co-precipitation and filtration; The first precursor and the R source are mixed, and a first sintering is performed in an oxygen-containing atmosphere to obtain a second precursor; The second precursor, Li source, M 1 Source, P2O7 4- The solid electrolyte material is mixed with the raw materials and subjected to a second sintering in an oxygen-free atmosphere to obtain the solid electrolyte material.

10. The method according to claim 9, characterized in that The M 2 Source, the M 3 Source, the PO4 3- The source, the surfactant, the precipitant and the solvent are mixed, and the first precursor is obtained after co-precipitation and filtration.

11. The method according to claim 10, characterized in that Based on the PO4 3- The mass of the surfactant accounts for ≥0.1% of the total mass of the source.

12. The method according to claim 11, characterized in that Based on the PO4 3- The mass of the surfactant accounts for 0.1%-1% of the total mass of the source.

13. The method according to claim 12, characterized in that Based on the PO4 3- The mass of the surfactant accounts for 0.3%-0.7% of the total mass of the source.

14. The method according to claim 10, characterized in that The surfactant includes at least one of polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate and sulfonates.

15. The method according to claim 9 or 10, characterized in that Satisfy at least one of the following conditions: The oxygen-containing atmosphere includes oxygen or air; The temperature of the first sintering is 700°C-900°C, and the time of the first sintering is 4h-10h; The oxygen-free atmosphere includes an inert gas or nitrogen; The temperature of the second sintering is 450°C-700°C, and the time of the second sintering is 8h-20h; The M 1 Sources include M 1 At least one of oxides, phosphates, sulfates, chlorides, nitrates and carbonates; The M 2 Sources include M 2 At least one of phosphate, acetate, sulfate, chloride, nitrate, and carbonate; The M 3 Sources include M 3 At least one of phosphate, acetate, sulfate, chloride, nitrate, and carbonate; The PO4 3- The source includes at least one of H3PO4, NH4H2PO4, (NH4)2HPO4, (NH4)3PO4, LiH2PO4, Li2HPO4, Li3PO4, NaH2PO4, Na2HPO4, and Na3PO4; The Li source includes at least one of lithium carbonate, lithium hydroxide and lithium nitrate; The P2O7 4- The source includes at least one of H4P2O7, (NH4)2H2P2O7, Li2H2P2O7, and Li4P2O7; The R source includes at least one of a simple substance, an oxide, and a hydride containing R; The precipitant includes at least one of sodium hydroxide, sodium carbonate and ammonia water.

16. A positive electrode active material, characterized in that: The invention comprises the solid electrolyte material according to any one of claims 1 to 8 or the solid electrolyte material prepared by the method according to any one of claims 9 to 15.

17. The positive electrode active material according to claim 16, characterized in that The positive electrode active material includes a substrate, at least a portion of the surface of the substrate has a coating layer, and the coating layer includes the solid electrolyte material.

18. The positive electrode active material according to claim 17, characterized in that Based on the total mass of the substrate, the mass proportion of the solid electrolyte material is 0.05%-1%.

19. A positive electrode plate, characterized in that: The positive electrode active material comprises the positive electrode active material according to any one of claims 16 to 18.

20. A solid-state battery, characterized in that: Including the positive electrode sheet as described in claim 19.

21. An electrical equipment, characterized in that: Including the solid-state battery as described in claim 20.