A leveling die and leveling method for large-size, ultra-thin alloy foil
By designing a leveling mold including an upper platen, a lower plate, a secondary platen and a backing plate, combined with heat treatment and annealing, the problem of leveling large-sized, ultra-thin gadolinium-zirconium alloy foils is solved, and the foil is uniformly stressed and Efficient flatness improvement reduces cost and time costs.
Patent Information
- Application Number
- CN202410718637.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-05
AI Technical Summary
It is difficult to effectively level large-sized, ultra-thin gadolinium-zirconium alloy foils with existing technology, resulting in uneven plate shape, internal stress, and difficulty in processing complex shapes. In addition, the heavy-pressure mold heat treatment and pressure leveling method has manufacturing difficulties and time costs. High question.
A leveling mold including an upper platen, a lower plate, a secondary platen and a backing plate is designed. Through evenly distributed threaded through holes and screw fastening, combined with heat treatment and annealing, uniform stress on large-size, ultra-thin alloy foils is achieved. and improved flatness.
Reduces the weight of the mold and manufacturing costs, improves the flatness of the foil, avoids internal stress and floating phenomena, is suitable for efficient leveling of large-size, ultra-thin foils, and is suitable for thermal leveling, eliminating the need for rolling stress.
Smart Images

Figure CN118287534B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of leveling of metal foils, and in particular to a leveling die and a leveling method for large-size and ultra-thin alloy foils. Background Art
[0002] Neutron collimator is the core component of neutron scattering spectrometer. Gadolinium zirconium alloy foil is the core material of neutron collimator, which is required to have large size (width>600mm, length>1050mm) and ultra-thin thickness (thickness≤0.06mm). Due to the low tensile strength and poor plasticity of gadolinium zirconium alloy, it cannot be prepared by conventional tension rolling method, and can only be prepared by cladding rolling method. The stress state of the foil is complex during rolling, and the foil has plate shape problems such as middle waves and double waves on both sides, which cannot be directly used in neutron collimator. It is urgent to carry out leveling process research on this type of foil.
[0003] At present, the main leveling methods include stretch straightening and heavy pressure die heat treatment pressure leveling. Among them, stretch straightening is a cold leveling method, which mainly removes the wave shape of the cold-rolled plate by applying external force such as two bends and one straightening, two bends and two straightening, etc. This requires the material to have a certain tensile strength and plasticity, and requires the material to have a certain length. The foil leveled by the stretch straightening method has a certain internal stress, and will produce a certain rebound after being placed for a period of time, making it difficult to re-cut more precise and complex shapes; and heavy pressure die heat treatment pressure leveling is currently the main leveling method for sheet non-ferrous metal plates and strips. It mainly uses a high-flatness gravity pressure plate to perform repeated pressure leveling at a suitable temperature. At present, this solution has the following problems:
[0004] (a) The gravity platen is too thick, has high flatness requirements, is difficult to manufacture, and increases the weight of the tooling, making it more difficult to heat and dissipate heat, and is time-consuming.
[0005] (b) When the foil to be leveled is large-sized and ultra-thin, the large middle surface cannot bear force or the force is uneven, and there is floating space in the middle. At the same time, since the foil is double-zero-level thickness, it deforms more seriously when heated. If it is not subjected to uniform heavy pressure and kept at a low temperature, the shape of the foil will be worse.
[0006] Therefore, the heavy-pressure die heat treatment pressure leveling solution has a certain effect on thick materials, but it cannot level large-sized, ultra-thin foils. Summary of the invention
[0007] In view of the above problems existing in the prior art, the present invention provides a leveling die and a leveling method for large-sized and ultra-thin alloy foil materials, so as to achieve the purpose of leveling large-sized and ultra-thin metal foil materials.
[0008] The specific content of the invention is as follows:
[0009] In the first aspect, the present invention provides a leveling die for large-size, ultra-thin alloy foil, comprising: an upper pressing plate and a bottom plate; a plurality of first threaded through holes are evenly distributed on the surface of the upper pressing plate; corresponding second threaded through holes are arranged around the upper pressing plate and the bottom plate; angle steels connected to each other are welded around and in the middle of the side of the upper pressing plate away from the bottom plate; angle steels connected to each other are welded around and in the middle of the side of the bottom plate away from the upper pressing plate;
[0010] A secondary pressing plate, the secondary pressing plate being located below the upper pressing plate;
[0011] A plurality of pads, wherein the pads are located between the secondary pressing plate and the bottom plate, and alloy foil is placed between two adjacent pads;
[0012] A plurality of first screws and second screws;
[0013] The first screw is adapted to the first threaded through hole, and the length of the first screw rod is greater than the depth of the first threaded through hole;
[0014] The second screw is matched with the second threaded through hole, and the length of the second screw is greater than the total theoretical thickness of the upper pressing plate, the secondary pressing plate, the backing plate, the alloy foil and the bottom plate.
[0015] Optionally, the number of the pads is between 2 and 500;
[0016] The number of alloy foils placed between two adjacent pads is no more than 5.
[0017] Optionally, the upper pressing plate and the bottom plate have the same size, the upper pressing plate and the bottom plate have the same size, and the pad and the secondary pressing plate have sizes smaller than those of the upper pressing plate and the bottom plate.
[0018] Optionally, the upper pressing plate, the secondary pressing plate and the bottom plate are all made of polished carbon steel plates;
[0019] The material of the backing plate is cold-rolled carbon steel plate.
[0020] Optionally, the thickness of the upper pressing plate is between 10-15 mm;
[0021] The thickness of the secondary pressing plate is between 3-5 mm;
[0022] The thickness of the pad is between 0.5-1 mm;
[0023] The thickness of the bottom plate is between 10-15 mm.
[0024] Optionally, the number of the first threaded through holes is between 40 and 70;
[0025] The number of the second threaded through holes is between 30 and 50.
[0026] In a second aspect, the present invention provides a leveling method for a large-sized, ultra-thin alloy foil, the leveling method being applicable to the leveling mold described in the first aspect, comprising:
[0027] S1: Place a pad on the bottom plate plane;
[0028] S2: placing 1 to 5 alloy foils on the pad, and then covering the alloy foils with a pad;
[0029] S3: Repeat step S2 0 to 500 times;
[0030] S4: placing a secondary pressing plate on the top pad, and placing an upper pressing plate on the secondary pressing plate;
[0031] S5: aligning the second threaded through holes around the bottom plate and the upper pressing plate, and screwing a second screw into each of the second threaded through holes, so that the distance between the upper pressing plate and the bottom plate is consistent with the total theoretical thickness of the secondary pressing plate, the backing plate and the alloy foil;
[0032] S6: sequentially screwing a first screw into each of the first threaded through holes, so that the screw head of the first screw is screwed until it contacts the secondary pressure plate;
[0033] S7: The tooling after S6 is transferred to a vacuum annealing furnace, and annealed at 300-500°C. After cooling, the tooling is opened to obtain a large-size, ultra-thin alloy foil after leveling.
[0034] Optionally, the annealing treatment at 300-550° C. includes:
[0035] Heating rate: 5°C / min, heating to 300-400°C, keeping warm for 2-3 hours;
[0036] Then continue to heat up to 450-550 ℃ at a heating rate of 3-5 ℃ / min and keep warm for 1-3 hours.
[0037] Optionally, the cooling along with the furnace and then taking out the furnace, and opening the tooling includes: cooling along with the furnace to below 80° C. and then taking out the furnace, cooling to room temperature in the atmosphere, and opening the tooling.
[0038] Optionally, the unevenness of the large-sized, ultra-thin alloy foil after leveling is ≤100 μm / m.
[0039] Compared with the prior art, the present invention has the following advantages:
[0040] The present invention provides a leveling die for large-size, ultra-thin alloy foil, comprising: an upper pressing plate and a bottom plate; a plurality of first threaded through holes evenly distributed on the surface of the upper pressing plate; corresponding second threaded through holes are arranged around the upper pressing plate and the bottom plate; angle steels connected to each other are welded around and in the middle of the upper pressing plate on one side away from the bottom plate; angle steels connected to each other are welded around and in the middle of the bottom plate on one side away from the upper pressing plate; a secondary pressing plate, which is located at the lower part of the upper pressing plate; a plurality of pads, which are located between the secondary pressing plate and the bottom plate, and are used to place alloy foil between two adjacent pads; and a plurality of first screws and second screws. The present invention adopts a low-cost, thin, polished carbon steel plate as the bottom plate and the upper pressing plate, and welds angle steels around and in the middle, which not only ensures the strength of the pressing plate, but also reduces the weight of the overall mold, is beneficial to heat conduction, and will not deform during repeated use, effectively reducing time and economic costs; evenly distributed second threaded through holes are arranged around the upper pressing plate and the bottom plate, so that the mold can be fastened in a bolted manner, increasing the pressure applied to the foil and the pad, so that the upper pressing plate does not need to use a thick plate (the traditional upper pressing plate uses a thick plate to be more evenly stressed), and there is no need to additionally set up a device for applying pressure to the mold; by screwing the first screw into the evenly distributed first threaded through holes in the middle of the upper pressing plate, the screw head is screwed until it contacts the secondary pressing plate, and the secondary pressing plate is acted on by the top screw, effectively solving the problem of uneven stress on a large surface of the ultra-thin foil and floating and unsolid pressure in the middle, and greatly improving the flatness of the large-size ultra-thin foil.
[0041] The method for leveling large-size and ultra-thin alloy foils provided by the present invention can place a plurality of foils between every two adjacent pads, thereby improving production efficiency; the method adopts surrounding bolts for fastening combined with the action of the middle top screw, so that the alloy foil is subjected to greater pressure, the middle of the foil does not float, and the force is evenly applied; and the present invention places a secondary pressure plate between the upper pressure plate and the pad as a transition correction plate, which can not only make the large surface of the alloy foil subjected to uniform force, but also avoid the screws directly acting on the pad to cause damage to the pad and the foil; compared with cold drawing and bending straightening, the leveling method is suitable for hot leveling, which effectively removes the rolling stress of the alloy foil. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0043] Figure 1 A schematic diagram of the structure of a leveling mold provided by an embodiment of the present invention is shown;
[0044] Figure 2A schematic diagram of the structure of an upper pressing plate provided in an embodiment of the present invention is shown;
[0045] Figure 3 A schematic diagram of the structure of a base plate provided by an embodiment of the present invention is shown;
[0046] Figure 4 A flow chart of a method for leveling a large-sized, ultra-thin alloy foil provided by an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0047] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means a limitation on the present invention and its application or use. Based on the embodiments of the present invention, any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts falls within the scope of protection of the present invention. In addition, all other embodiments obtained by ordinary technicians in this field without carrying out creative work belong to the scope of protection of the present invention.
[0048] In the embodiment, no specific experimental steps or conditions are indicated, and the operation or conditions of the conventional experimental steps described in the prior art in this field can be carried out. The reagents used and other instruments that do not indicate the manufacturer are conventional reagent products that can be obtained commercially. In addition, the accompanying drawings are only schematic diagrams of the embodiments of the present invention and are not necessarily drawn to scale. The same reference numerals in the figures represent the same or similar parts, and thus their repeated description will be omitted. Some block diagrams shown in the accompanying drawings are functional entities and do not necessarily correspond to physically or logically independent entities.
[0049] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0050] In the description of the present invention, it should be understood that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. Unless otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.
[0051] In addition, the technical features involved in the different embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0052] The specific implementation contents of the present invention are as follows:
[0053] In a first aspect, the present invention provides a leveling die for large-sized, ultra-thin alloy foil. Figure 1 The schematic diagram of the leveling mold structure provided by the embodiment of the present invention is shown as follows: Figure 1 As shown, the leveling mold includes, from top to bottom, an upper pressing plate 1, a secondary pressing plate 2, a plurality of pads 3, a bottom plate 4, and a plurality of first screws and second screws, wherein the structural schematic diagram of the upper pressing plate 1 is shown in FIG. Figure 2 ,like Figure 2 As shown, the upper pressing plate 1 is provided with second threaded through holes 1-1 around its periphery; the structural schematic diagram of the bottom plate 4 is shown in Figure 3 ,like Figure 3 As shown, the bottom plate 4 is also provided with second threaded through holes 1-1 around it, and the positions of the second threaded through holes 1-1 on the bottom plate 4 correspond to the second threaded through holes 1-1 provided around the upper pressing plate 1 one by one, and the number of the second threaded through holes 1-1 on the upper pressing plate 1 and the bottom plate 4 is between 30 and 50. This ensures that the upper pressing plate 1 and the bottom plate 4 can be connected by the second screws to achieve bolt fastening, thereby increasing the pressure applied to the alloy foil, so that the upper pressing plate does not need to use a thick plate (the traditional upper pressing plate adopts a thick plate to bear the force more evenly), and there is no need to set up an additional device to apply pressure to the mold.
[0054] See also Figure 1 , below the upper pressure plate 1 is the secondary pressure plate 2, which serves as a transition correction plate. The setting of the secondary pressure plate 2 can not only make the large surface of the alloy foil evenly stressed, but also avoid the first screw directly acting on the pad to cause damage to the pad and the foil; the pad 3 is located between the secondary pressure plate 2 and the bottom plate 4, and the number of pads 3 is at least two, that is, alloy foils 5 to be leveled are placed between every two pads 3, and the number of alloy foils 5 to be leveled placed between every two pads 3 is not more than 5. The setting of the pads 3 effectively ensures the uniformity of the force on the alloy foil 5. At the same time, in the process of mass leveling of alloy foils 5, the more pads 3 are set, the more alloy foils 5 can be leveled at the same time; the number of pads 3 can be set within 500, and the stacked pads 3 can effectively avoid adhesion caused by pressure on the alloy foil 5.
[0055] See also Figure 2 , the middle part of the upper pressing plate 1 is also evenly distributed with first threaded through holes 1-2, and the number of the first threaded through holes is between 40 and 70; the first threaded through holes 1-2 are adapted to the first screws, and the first screws are screwed into the first threaded through holes 1-2 evenly distributed in the middle part of the upper pressing plate, and the screw heads are screwed until they contact the secondary pressing plate 2, and the secondary pressing plate 2 is acted on by the top screw, which effectively solves the problem of uneven force on a large surface of the ultra-thin foil and the problem of floating and unsolid pressure in the middle, and greatly improves the flatness of the large-size ultra-thin foil; the middle part of the bottom plate 4 is a complete flat surface without through holes.
[0056] Continue to see Figure 2 and Figure 3 The present invention adopts low-cost, thin-thickness polished carbon steel plate to prepare the upper pressing plate 1 and the bottom plate 4. The upper pressing plate 1 and the bottom plate 4 have the same size, with a width of not less than 800 mm and a length of not less than 1250 mm. A cross-connected angle steel 14-1 is welded around and in the middle of the side of the upper pressing plate 1 that does not contact the secondary pressing plate 2 and the side of the bottom plate 4 that does not contact the pad 3. The enclosed area formed by the intersection of the angle steels 14-1 is a square with a side length of not more than 80 mm. The setting of the angle steel 14-1 not only ensures the strength of the upper pressing plate 1 and the bottom plate 4, but also reduces the weight of the overall mold. Among them, the thickness of the upper pressing plate 1 is between 10-15 mm, and the thickness of the bottom plate 4 is between 10-15 mm, which is conducive to heat conduction and will not deform during repeated use, effectively reducing time and economic costs.
[0057] During specific implementation, the screw length of the first screw needs to be greater than the depth of the first threaded through hole, so that the top of the screw of the first screw can contact and tighten the secondary pressure plate 2; the screw length of the second screw needs to be greater than the total theoretical thickness of the upper pressure plate, secondary pressure plate, pad, alloy foil and bottom plate, so as to ensure that the upper pressure plate 1 and the bottom plate 4 are bolted together by the second screw; so that the alloy foil located between the pads is evenly stressed.
[0058] During specific implementation, the secondary pressing plate 2 is made of a polished carbon steel plate, and the pad 3 is made of a cold-rolled carbon steel plate. The secondary pressing plate 2 and the pad 3 have the same size. The sizes of the secondary pressing plate 2 and the pad 3 are smaller than those of the upper pressing plate 1 and the bottom plate 4. The thickness of the secondary pressing plate 2 is between 3-5mm; the thickness of the pad 3 is between 0.5-1mm.
[0059] In a second aspect, the present invention provides a method for leveling a large-sized, ultra-thin alloy foil. The method is applicable to the leveling mold of the first aspect. Figure 4 The flow chart of the leveling method of large-size, ultra-thin alloy foil provided by the embodiment of the present invention is shown as follows: Figure 4 As shown, the leveling method specifically includes the following processing steps:
[0060] S1: Place a pad on the bottom plate plane;
[0061] S2: Place 1 to 5 alloy foils on the pad, and then cover the alloy foils with a pad;
[0062] S3: Repeat step S2 0 to 500 times;
[0063] S4: Place a secondary pressing plate on the top pad, and place an upper pressing plate on the secondary pressing plate;
[0064] S5: Align the second threaded through holes around the bottom plate and the upper pressing plate, and screw the second screw into each second threaded through hole so that the spacing between the upper pressing plate and the bottom plate is consistent with the total theoretical thickness of the secondary pressing plate, the backing plate and the alloy foil;
[0065] S6: Screw the first screw into each first threaded through hole in sequence, so that the screw head of the first screw is screwed until it contacts the secondary pressure plate;
[0066] S7: The tooling after S6 is transferred to a vacuum annealing furnace, and annealed at 300-500°C. After cooling, the tooling is opened to obtain a large-size, ultra-thin alloy foil after leveling.
[0067] In some embodiments, the annealing treatment is carried out in a gradient heating manner, specifically including: heating to 300-400°C at a heating rate of 5°C / min, keeping warm for 2-3 hours; then heating to 450-550°C at a heating rate of 3-5°C / min, keeping warm for 1-3 hours, cooling with the furnace and then taking out of the furnace. To prevent the alloy foil from deforming, the alloy foil is taken out of the furnace after cooling to below 80°C with the furnace, and then continues to cool to room temperature in the atmosphere, unscrewing the screws to open the tooling, and taking out the alloy foil. The unevenness of the large-size, ultra-thin alloy foil obtained after leveling is ≤100 μm / m.
[0068] The method for leveling large-size and ultra-thin alloy foils provided by the present invention can place a plurality of foils between every two adjacent pads, thereby improving production efficiency; the method adopts surrounding bolts for fastening combined with the action of the middle top screw, so that the alloy foil is subjected to greater pressure, the middle of the foil does not float, and the force is evenly applied; and the present invention places a secondary pressure plate between the upper pressure plate and the pad as a transition correction plate, which can not only make the large surface of the alloy foil subjected to uniform force, but also avoid the screws directly acting on the pad to cause damage to the pad and the foil; compared with cold drawing and bending straightening, the leveling method is suitable for hot leveling, which effectively removes the rolling stress of the alloy foil.
[0069] In order to enable those skilled in the art to more clearly understand the present invention, a leveling mold and a leveling method for a large-size, ultra-thin alloy foil according to the present invention are now described in detail through the following embodiments.
[0070] See the leveling die used. Figure 1 Schematic diagram of the leveling mold is shown. Embodiment 1:
[0071] Place the bottom plate 4 on a flat surface, and place a pad 3 (0.5 mm thick) on the bottom plate 4;
[0072] Place a gadolinium-zirconium alloy foil 5 (0.06 mm thick) on the backing plate 3, and then cover the alloy foil 5 with another backing plate 3;
[0073] One alloy foil 5 and one backing plate 3 are placed as one layer, and 100 layers are placed in sequence. A secondary pressing plate 3 (3 mm thick) is placed on the top backing plate 3, and an upper pressing plate is placed on the secondary pressing plate 2. The theoretical spacing between the upper pressing plate 1 and the bottom plate 4 is 59.5 mm.
[0074] Align the threaded through holes of the bottom plate 4 and the upper pressure plate 1, first tighten the screws around with screws, measure the height difference between the upper pressure plate 1 and the bottom plate 4, measure 5 points in the length direction and 3 points in the width direction, the height difference is 59.5mm, which is consistent with the theoretical spacing between the upper pressure plate and the bottom plate.
[0075] Use M12×40mm screws to tighten all (53) threaded through holes in the middle in turn. Tighten the screw heads until they touch the secondary pressure plate 2. The height to which the screws are screwed down is the thickness of the upper pressure plate 1. Measure the length of the unscrewed screws. The unscrewed heights of the 53 screws are all 28mm.
[0076] The above-mentioned tooling is hoisted into a vacuum annealing furnace, heated to 300°C and kept for 1 hour at a heating rate of 5°C / min; then the temperature is continued to be raised to 480°C and kept for 2 hours at a heating rate of 3°C / min. After cooling to below 80°C with the furnace, the vacuum is turned off and the furnace is taken out.
[0077] To prevent the foil from deforming, after cooling to room temperature in the atmosphere, the screws are unscrewed to open the tooling, and a large-sized, ultra-thin gadolinium-zirconium alloy foil with good flatness is obtained, and the foil unevenness is ≤100μm / m.
[0078] 10% of the foils were randomly selected for unevenness testing, and the results were as follows: 80μm / m, 75μm / m, 85μm / m, 95μm / m, 90μm / m, 95μm / m, 90μm / m, 80μm / m, 85μm / m, 90μm / m. Embodiment 2:
[0079] Place the base plate 4 on a flat surface, and place a pad 3 (0.5 mm thick) on the base plate 4 .
[0080] Three gadolinium-zirconium alloy foils 5 (thickness 0.06 mm) are placed on the backing plate 3 , and one backing plate 3 is then placed on the alloy foils 5 .
[0081] Three alloy foils 5 and one backing plate 3 are placed as one layer, and 250 layers are placed in sequence. A secondary pressing plate 3 (3 mm thick) is placed on the top backing plate 3, and an upper pressing plate is placed on the secondary pressing plate 2. The theoretical spacing between the upper pressing plate 1 and the bottom plate 4 is 173.5 mm.
[0082] Align the through holes of the bottom plate 4 and the upper pressure plate 1, first tighten the screws around with screws, measure the height difference between the upper pressure plate 1 and the bottom plate 4, measure 5 points in the length direction and 3 points in the width direction, the height difference is 173.5mm, which is consistent with the theoretical spacing between the upper pressure plate 1 and the bottom plate 4.
[0083] Use M12×40mm screws to tighten the middle threaded holes in sequence. Tighten the screw heads until they contact the secondary pressure plate 2. The height to which the screws are screwed down is the thickness of the upper pressure plate 1. Measure the length of the unscrewed screws. The unscrewed heights of the 53 screws are all 28mm.
[0084] The above-mentioned tooling is hoisted into a vacuum annealing furnace, heated to 300°C and kept for 2 hours at a heating rate of 5°C / min; then the temperature is continued to be raised to 480°C and kept for 3 hours at a heating rate of 3°C / min. After cooling to below 80°C with the furnace, the vacuum is turned off and the furnace is taken out.
[0085] To prevent the foil from deforming, after cooling to room temperature in the atmosphere, the screws are unscrewed to open the tooling, and a large-sized, ultra-thin gadolinium-zirconium alloy foil with good flatness is obtained, and the foil unevenness is ≤100μm / m.
[0086] 10% of the foils were randomly selected for unevenness testing, and the results were as follows: 85μm / m, 85μm / m, 90μm / m, 92μm / m, 96μm / m, 98μm / m, 87μm / m, 80μm / m, 82μm / m, and 90μm / m. Embodiment 3:
[0087] Place the base plate 4 on a flat surface, and place a pad 3 (0.5 mm thick) on the base plate 4 .
[0088] Five sheets of gadolinium-zirconium alloy foils 5 (thickness 0.06 mm) were placed on the backing plate 3 , and one sheet of the backing plate 3 was then placed on the alloy foils 5 .
[0089] Five alloy foils 5 and one backing plate 3 are placed as one layer, and 400 layers are placed in sequence. A secondary pressing plate 3 (3 mm thick) is placed on the top backing plate 3, and an upper pressing plate is placed on the secondary pressing plate 2. The theoretical spacing between the upper pressing plate 1 and the bottom plate 4 is 323.5.5 mm.
[0090] Align the through holes of the bottom plate 4 and the upper pressure plate 1, first tighten the screws around with screws, measure the height difference between the upper pressure plate 1 and the bottom plate 4, measure 5 points in the length direction and 3 points in the width direction, the height difference is 323.5mm, which is consistent with the theoretical spacing between the upper pressure plate 1 and the bottom plate 4.
[0091] Use M12×40mm screws to tighten the middle threaded holes in sequence. Tighten the screw heads until they contact the secondary pressure plate 2. The height to which the screws are screwed down is the thickness of the upper pressure plate 1. Measure the length of the unscrewed screws. The unscrewed heights of the 53 screws are all 28mm.
[0092] The above-mentioned tooling is hoisted into a vacuum annealing furnace, heated to 300°C and kept for 3 hours at a heating rate of 5°C / min; then the temperature is continued to be raised to 480°C and kept for 4 hours at a heating rate of 3°C / min. After cooling to below 80°C with the furnace, the vacuum is turned off and the furnace is taken out.
[0093] To prevent the foil from deforming, after cooling to room temperature in the atmosphere, the screws are unscrewed to open the tooling, and a large-sized, ultra-thin gadolinium-zirconium alloy foil with good flatness is obtained, and the foil unevenness is ≤100μm / m.
[0094] 10% of the foils were randomly selected for unevenness testing, and the results were as follows: 95μm / m, 80μm / m, 80μm / m, 90μm / m, 98μm / m, 88μm / m, 85μm / m, 75μm / m, 80μm / m, and 92μm / m.
[0095] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification.
[0096] For the method embodiments, for the sake of simplicity, they are all described as a series of action combinations, but those skilled in the art should know that the present invention is not limited by the order of the actions described, because according to the present invention, some steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also know that the embodiments described in the specification are all preferred embodiments, and the actions and components involved are not necessarily required by the present invention.
[0097] The above is a detailed introduction to a leveling mold and a leveling method for a large-size, ultra-thin alloy foil provided by the present invention. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea; at the same time, for a general technician in this field, according to the idea of the present invention, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.
Claims
1. A leveling die for large-size, ultra-thin alloy foil, characterized in that: include: An upper pressing plate and a bottom plate; a plurality of first threaded through holes are evenly distributed on the surface of the upper pressing plate; corresponding second threaded through holes are arranged around the upper pressing plate and the bottom plate; angle steels connected to each other are welded around and in the middle of the side of the upper pressing plate away from the bottom plate; angle steels connected to each other are welded around and in the middle of the side of the bottom plate away from the upper pressing plate; A secondary pressing plate, the secondary pressing plate being located below the upper pressing plate; A plurality of pads, wherein the pads are located between the secondary pressing plate and the bottom plate, and alloy foil is placed between two adjacent pads; a plurality of first screws and second screws; The first screw is adapted to the first threaded through hole, the length of the first screw is greater than the depth of the first threaded through hole, and the screw head of the first screw is screwed to contact the secondary pressing plate to avoid floating in the middle of the alloy foil during leveling; The second screw is adapted to the second threaded through hole, the length of the second screw is greater than the total theoretical thickness of the upper pressing plate, the secondary pressing plate, the backing plate, the alloy foil and the bottom plate, and the upper pressing plate and the bottom plate are fastened by the second screw bolt to apply pressure to level the alloy foil; The upper pressing plate, the secondary pressing plate and the bottom plate are all made of polished carbon steel plates; The material of the pad is cold-rolled carbon steel plate; The thickness of the upper pressing plate is between 10-15 mm; The thickness of the secondary pressing plate is between 3-5 mm; The thickness of the pad is between 0.5-1 mm; The thickness of the bottom plate is between 10-15 mm; The process of leveling the alloy foil using the leveling die includes: S1: Place a pad on the bottom plate plane; S2: placing 1 to 5 alloy foils on the pad, and then covering the alloy foils with a pad; S3: Repeat step S2 0 to 500 times; S4: placing a secondary pressing plate on the top pad, and placing an upper pressing plate on the secondary pressing plate; S5: aligning the second threaded through holes around the bottom plate and the upper pressing plate, and screwing a second screw into each of the second threaded through holes, so that the distance between the upper pressing plate and the bottom plate is consistent with the total theoretical thickness of the secondary pressing plate, the backing plate and the alloy foil; S6: sequentially screwing a first screw into each of the first threaded through holes, so that the screw head of the first screw is screwed until it contacts the secondary pressure plate; S7: After S6, the tooling is transferred to a vacuum annealing furnace, and annealed at 300-550°C. After cooling, the tooling is opened to obtain a large-size, ultra-thin alloy foil after leveling.
2. The leveling mold according to claim 1, characterized in that: The number of the pads is between 2 and 500; The number of alloy foils placed between two adjacent pads is no more than 5.
3. The leveling mold according to claim 1, characterized in that: The upper pressing plate and the bottom plate have the same size, the secondary pressing plate and the pad have the same size, and the pad and the secondary pressing plate are smaller in size than the upper pressing plate and the bottom plate.
4. The leveling mold according to claim 1, characterized in that: The number of the first threaded through holes is between 40 and 70; The number of the second threaded through holes is between 30 and 50.
5. The leveling mold according to claim 1, characterized in that: The annealing treatment at 300-550°C includes: Heating rate: 5°C / min, heating to 300-400°C, keeping warm for 2-3 hours; Then continue to heat up to 450-550 ℃ at a heating rate of 3-5 ℃ / min and keep warm for 1-3 hours.
6. The leveling mold according to claim 1, characterized in that: The step of taking out the furnace after cooling along with the furnace and opening the tooling comprises: taking out the furnace after cooling along with the furnace to below 80° C., cooling to room temperature in the atmosphere, and opening the tooling.
7. The leveling mold according to claim 1, characterized in that: The unevenness of the large-size and ultra-thin alloy foil after leveling is ≤100 μm / m.
Citation Information
Patent Citations
Compression moulding device and method of flat product
CN102029724A
Tungsten panel levelling anchor clamps