A surface corrosion resistant process for titanium alloy oil casing

The corrosion-resistant protective layer is formed through hot rolling process and chemical vapor deposition technology, which solves the problem of titanium alloy pipes being easily corroded in acidic environments and significantly improves their corrosion resistance.

CN118291898BActive Publication Date: 2024-10-25JIANGSU VALIN XIGANG SPECIAL STEEL
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410407946.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-07
Publication Date
2024-10-25
Estimated Expiration
2044-04-07

AI Technical Summary

Technical Problem

Titanium alloy pipes are prone to corrosion in reducing acid environments such as hydrochloric acid and sulfuric acid, which limits their application scope.

Method used

The hot rolling process is used to form a corrosion-resistant protective layer, which includes chemical vapor deposition technology to deposit titanium nitride and silicon carbide doped films on the surface of titanium alloy tubes, and use sealing agents to fill the pores to form a corrosion-resistant protective layer.

Benefits of technology

Significantly improves the corrosion resistance of titanium alloy pipes, reduces the electrochemical corrosion rate, and enhances its stability in acidic environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004778108910000081
    Figure BDA0004778108910000081
Patent Text Reader

Abstract

The present invention relates to the technical field of titanium alloy surface treatment, specifically to a surface corrosion resistant process for titanium alloy oil casing, comprising the following processes: step (1) hot rolling: heating, punching, continuous rolling, and sizing a titanium alloy billet to obtain a titanium alloy tube; step (2) surface treatment: surface treating the titanium alloy tube obtained in the previous step to form a corrosion resistant protective layer to obtain a corrosion resistant titanium alloy tube. The present invention sequentially deposits boron carbon nitrogen and silicon carbide doped titanium nitride on the surface of the titanium alloy through plasma enhanced vapor deposition technology, and sequentially forms a boron carbon nitrogen film and a titanium nitride film, and uses a sealing agent to seal to obtain a corrosion resistant protective layer, which can physically block moisture, chloride ions, oxygen, etc. in the environment, and can hinder metal anode corrosion reactions, reduce electrochemical corrosion rates, and improve the corrosion resistance of titanium alloy oil casing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium alloy pipes, in particular to a surface corrosion resistance process for titanium alloy oil casing. Background Art

[0002] Compared with traditional steel pipes, stainless steel pipes, copper alloy pipes and other pipes, titanium alloy pipes have the advantages of good corrosion resistance, high specific strength, and good processing performance. There are many types of alloys that can meet the use requirements of various fields. It has great development potential and can be widely used in aerospace, weapons, petroleum, marine engineering and other industries. Titanium alloy pipes are mainly divided into welded pipes and seamless pipes. Titanium alloy welded pipes are formed by direct rolling and welding of titanium strips and plates. Their cost is relatively low, but the presence of welds will lead to uneven performance of titanium alloy pipes, limiting their application range. However, the limitation of titanium alloy pipes being easily corroded in reducing acid environments such as hydrochloric acid and sulfuric acid also hinders their further application. Therefore, we propose a surface corrosion resistance process for titanium alloy pipes. Summary of the invention

[0003] The purpose of the present invention is to provide a surface corrosion resistance process for titanium alloy oil casing to solve the problems raised in the above background technology.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: a surface corrosion resistance process of a titanium alloy oil casing, comprising the following processes:

[0005] Step (1) hot rolling: heating, punching, continuous rolling, and sizing the titanium alloy billet to obtain a titanium alloy tube;

[0006] Step (2) surface treatment: The titanium alloy tube obtained in the previous step is subjected to surface treatment to form a corrosion-resistant protective layer to obtain a corrosion-resistant titanium alloy tube.

[0007] Furthermore, in step (1), the heating process conditions are as follows: the titanium alloy billet is kept at 400-480°C for 160-200 min; the temperature is increased to 880-930°C and kept for 200-240 min; the total time in the furnace is 390-400 min.

[0008] Furthermore, in the perforation process, the reduction is ≥13%, the ovality is 1.16-1.18, and a hair tube is obtained, and the length of the hair tube is controlled to be 6.5-7.7 m;

[0009] In the continuous rolling process: the exit speed of the continuous rolling mill is set at 4.8m / s, the limit speed is 80%, the lubrication speed is 1m / s, and the rough pipe is obtained;

[0010] In the sizing process, the final rolling temperature is ≥750°C to obtain a pipe.

[0011] Furthermore, the tube obtained after sizing is heat treated and straightened to obtain a titanium alloy tube;

[0012] Heat treatment process conditions are: heating temperature 900-950℃, heat preservation 60-90min, water cooling; heating to 510-550℃, heat preservation 230-250min, air cooling after leaving the furnace;

[0013] The straightening process conditions are: utilizing the residual heat after heat treatment for heat straightening, and the straightening temperature is 180-230°C.

[0014] Furthermore, the titanium alloy blank includes the following mass components: vanadium V: 3.5% to 4.5%, aluminum Al: 5.50% to 6.75%, iron Fe: ≤0.3%, carbon C: ≤0.08%, nitrogen N: ≤0.05%, hydrogen H: ≤0.015%, oxygen O: ≤0.20%, and the balance is titanium Ti.

[0015] In the above technical scheme, an intermediate inspection is carried out after sizing. The pipe size is: outer diameter D: ±1mm, wall thickness: ±15%. The actual measurement must be sampled after normal temperature, and flushing is not allowed. The qualified pipes after sizing are subjected to double heat treatment. First, solid solution heat treatment is carried out. In a high temperature environment, the microstructure of the pipe undergoes a phase transformation from the equiaxed α phase to the β phase. The initial β phases are interlaced, and the α phase in the titanium alloy is partially dissolved in the β phase, retaining a relatively coarse α phase. With the increase of the solid solution temperature, the α phase grains are refined, and the secondary α phase is precipitated in the β phase, reducing the α phase of the continuous grain boundary, and producing a network structure of the α phase and the lamellar β phase, which effectively improves the strength and elongation of the titanium alloy pipe. During the cooling process, the secondary lamellar α phase is precipitated in the organization, and is restricted by the equiaxed α phase. The growth of the β phase and the secondary α phase is inhibited, and the grain size is small; the lamellar α phase is embedded in the β phase, which can promote the improvement of the strength and toughness of the titanium alloy. After aging heat treatment, the coarse lamellar α phase disappears, a discontinuous equiaxed phase is formed, the β phase is interlaced, the grains are refined, and an α phase + β phase dual structure is formed, which improves the strength and hardness of the titanium alloy. In an air-cooled environment, the β phase is retained, the reticular structure is retained, and the titanium alloy can exhibit good mechanical properties. After heat treatment, the residual stress and dislocation density in the titanium alloy tube are reduced; the corrosion-resistant β phase is increased; the large-angle grain boundary increases, which can accelerate the formation of the passivation film and the increase of TiO2, and the stability of the passivation film is enhanced, thereby enhancing the corrosion resistance of the titanium alloy tube.

[0016] Furthermore, the surface treatment process is as follows:

[0017] Titanium nitride is deposited on the surface of the titanium alloy tube by chemical vapor deposition technology to form a thin titanium nitride layer; then a sealing agent is applied and the tube is kept at 80 to 100°C for 150 to 180 minutes to form a corrosion-resistant protective layer to obtain a corrosion-resistant titanium alloy tube.

[0018] Furthermore, the chemical vapor deposition technology is plasma enhanced chemical vapor deposition, and the process conditions are:

[0019] S1. In a temperature environment of 950-1000°C, use argon as the working gas and perform plasma cleaning for 15-20 minutes; in a mixed gas atmosphere of hydrogen and methane, inject borane ammonia complex, with a hydrogen flow rate of 38-40 mL / min and a methane flow rate of 4-6 mL / min, react and deposit for 40-60 minutes, a vacuum chamber pressure of 1-2 Pa, and a voltage of 500-800 V to form a boron carbon nitrogen film;

[0020] S2. In an atmosphere of a mixture of argon, hydrogen and nitrogen, titanium tetrachloride and tetramethylsilane are injected with hydrogen as a carrier gas, with a deposition temperature of 510-550°C, an argon flow rate of 20-32 mL / min, a hydrogen flow rate of 80-100 mL / min, a nitrogen flow rate of 10-16 mL / min, a deposition time of 50-120 min, a frequency of 5-8 kHz, a duty cycle of 33%-45%, a voltage of 600-800 V, and a working pressure of 80-100 Pa to form a titanium nitride film.

[0021] Furthermore, after the corrosion-resistant protective layer is formed, the surface corrosion-resistant process tube of the obtained corrosion-resistant titanium alloy tube is heat treated and straightened.

[0022] In the above technical scheme, the surface treatment is carried out at high temperature, and the process temperatures of step S1 and step S2 are respectively in the treatment temperature range of solution heat treatment and annealing heat treatment of the titanium alloy tube, and the corresponding deposition time is also close to the heat treatment time. Therefore, the surface treatment process of the titanium alloy tube can approximately replace the heat treatment process and promote the formation of (α+β) phase structure in the titanium alloy tube.

[0023] In the surface treatment step S1, the borane ammonia complex (BH3NH3) is decomposed at high temperature as a precursor, dehydrogenated and volatilized to form aminoborane (NH2BH2), cycloborazine (B3N3H6) and hydrogen, wherein aminoborane (NH2BH2) is a cyclic structure substance, which is very easy to undergo polymerization reaction at room temperature to produce a solid polymer of polyaminoborane and remain in the container, and the decomposed cycloborazine gas will enter the deposition chamber under the transportation of the carrier gas, and adsorb on the surface of the titanium alloy under high temperature and low pressure environment to undergo dehydrogenation reaction until all hydrogen atoms are removed to generate hBN, and diffuse to obtain a thin layer of boron nitride. The vapor deposition atmosphere also contains methane, which can carbonize the thin layer of boron nitride to form boron carbon nitrogen chemicals, so that its structure tends to grow towards a sheet graphene structure. For methane and hydrogen gas systems, under high-energy, high-density plasma and suitable process conditions, the gas dissociates to produce a large number of carbon-containing groups and atomic hydrogen. H radicals can chemically etch BN. By preferentially etching the crystal surface, the nucleation and growth of layered boron carbon nitrogen chemicals are promoted, so that they are deposited on the surface of the titanium alloy tube and stacked layer by layer, which helps to form a maze barrier effect and extend the diffusion path of the corrosive medium. At the same time, it can improve the hydrophobicity and conductivity of the boron carbon nitrogen film, physically block moisture, chloride ions, oxygen, etc. in the environment, and hinder the metal anode corrosion reaction, reduce the electrochemical corrosion rate, and play an anti-corrosion role.

[0024] In the surface treatment step S2, titanium tetrachloride is used as the source material, and titanium nitride is generated and deposited on the surface of the boron carbon nitride film and its pores and defects through the reaction between titanium tetrachloride, hydrogen and nitrogen in the atmosphere of nitrogen, hydrogen and argon, and its surface is sealed; titanium nitride has good electrical conductivity and corrosion resistance, which can further improve the corrosion resistance of the titanium alloy tube. The vapor deposition atmosphere also contains tetramethylsilane, hydrogen is dissociated into hydrogen atoms by the plasma, and tetramethylsilane is dissociated into carbon-containing and silicon-containing active groups, which are deposited to form silicon carbide, and silicon carbide doping can be formed in titanium nitride to obtain a titanium nitride thin layer containing silicon carbide, which can improve the toughness of the protective layer, alleviate thermal shrinkage, and reduce defects such as microcracks in the protective layer, which helps to further improve the corrosion resistance of the titanium alloy tube.

[0025] Furthermore, the sealing agent is one of silica sol and aluminum sol, or a mixture of the two.

[0026] The sealing agent is loaded on the surface of the titanium nitride film by brushing, so that it penetrates into the interior of the protective layer to achieve the effect of filling the pores. After drying, a sealing layer is formed, thereby obtaining a corrosion-resistant protective layer.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The present invention describes a surface corrosion resistance process for a titanium alloy oil casing. Through plasma enhanced vapor deposition technology, boron carbon nitrogen and silicon carbide doped titanium nitride are deposited on the surface of the titanium alloy in sequence, and a boron carbon nitrogen film and a titanium nitride film are formed in sequence, which are then sealed with a sealing agent to obtain a corrosion-resistant protective layer. The corrosion-resistant protective layer can physically block moisture, chloride ions, oxygen, etc. in the environment, and can hinder metal anode corrosion reactions, reduce the electrochemical corrosion rate, and improve the corrosion resistance of the titanium alloy tube. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] In the following specific implementations,

[0031] Titanium alloy billet: ingot batch number: HS1905038;

[0032] The dimensions of the titanium alloy tube are Φ130×Φ109×576mm;

[0033] The mass ratio of titanium tetrachloride to tetramethylsilane is 11:1;

[0034] The sealing agent is a water-based nano-alumina sealing agent, which comes from Tianjin Micronapt Technology Co., Ltd.

[0035] The surface treatment was a small laboratory test, and the size of the titanium alloy tube to be treated was 20×20×2mm.

[0036] Embodiment 1: A surface corrosion resistance process for titanium alloy oil casing, comprising the following processes:

[0037] Step (1) hot rolling:

[0038] The titanium alloy billet is heated, and the heating process conditions are as follows: the titanium alloy billet is kept at 400°C for 200 minutes; the temperature is raised to 880°C and kept for 200 minutes; the total furnace time is 400 minutes; the perforation is performed, the reduction is ≥13%, the ovality is 1.16-1.18, and a rough tube is obtained, and the length of the rough tube is controlled at 6.5-7.7m; continuous rolling, the outlet speed of the continuous rolling mill is set to 4.8m / s, the limit speed is 80%, and the lubrication speed is 1m / s to obtain a rough tube; sizing, the final rolling temperature is 780°C, and a titanium alloy tube is obtained;

[0039] Step (2) Surface treatment:

[0040] The titanium alloy tube obtained in the previous step was surface treated, and the process was as follows: in a temperature environment of 950°C, argon was used as the working gas, and plasma cleaning was performed for 15 minutes; in a mixed gas atmosphere of hydrogen and methane, borane ammonia complex was injected, the hydrogen flow rate was 38 mL / min, the methane flow rate was 4 mL / min, the reaction deposition was 40 minutes, the vacuum chamber pressure was 1 Pa, and the voltage was 500 V; in a mixed gas atmosphere of argon, hydrogen and nitrogen, titanium tetrachloride and tetramethylsilane were injected with hydrogen as the carrier gas, the deposition temperature was 510°C, the argon flow rate was 20 mL / min, the hydrogen flow rate was 80 mL / min, the nitrogen flow rate was 10 mL / min, the deposition time was 50 minutes, the frequency was 5 kHz, the duty cycle was 33%, the voltage was 600 V, and the working pressure was 80 Pa;

[0041] Then, the sealing agent is applied 5 times, and the tube is kept at 80° C. for 180 minutes to form a corrosion-resistant protective layer, thereby obtaining a corrosion-resistant titanium alloy tube.

[0042] Embodiment 2: A surface corrosion resistance process for titanium alloy oil casing, comprising the following processes:

[0043] Step (1) hot rolling:

[0044] The titanium alloy billet is heated, and the heating process conditions are as follows: the titanium alloy billet is kept at 440°C for 180 minutes; the temperature is raised to 900°C and kept for 220 minutes; the total furnace time is 400 minutes; the perforation is performed, the reduction is ≥13%, the ovality is 1.16-1.18, and a rough tube is obtained, and the length of the rough tube is controlled at 6.5-7.7m; continuous rolling, the outlet speed of the continuous rolling mill is set to 4.8m / s, the limit speed is 80%, and the lubrication speed is 1m / s to obtain a rough tube; sizing, the final rolling temperature is 830°C, and a titanium alloy tube is obtained;

[0045] Step (2) Surface treatment:

[0046] The titanium alloy tube obtained in the previous step was surface treated, and the process was as follows: in a temperature environment of 980°C, argon was used as the working gas, and plasma cleaning was performed for 18 minutes; in a mixed gas atmosphere of hydrogen and methane, borane ammonia complex was injected, the hydrogen flow rate was 39 mL / min, the methane flow rate was 5 mL / min, the reaction deposition was 50 minutes, the vacuum chamber pressure was 1.5 Pa, and the voltage was 750 V; in a mixed gas atmosphere of argon, hydrogen and nitrogen, titanium tetrachloride and tetramethylsilane were injected with hydrogen as the carrier gas, the deposition temperature was 530°C, the argon flow rate was 26 mL / min, the hydrogen flow rate was 90 mL / min, the nitrogen flow rate was 13 mL / min, the deposition time was 90 minutes, the frequency was 6 kHz, the duty cycle was 40%, the voltage was 700 V, and the working pressure was 90 Pa;

[0047] Then the sealing agent is applied 5 times, and the tube is kept at 90°C for 160 minutes to form a corrosion-resistant protective layer, thereby obtaining a corrosion-resistant titanium alloy tube.

[0048] Embodiment 3: A surface corrosion resistance process for titanium alloy oil casing, comprising the following processes:

[0049] Step (1) hot rolling:

[0050] The titanium alloy billet is heated, and the heating process conditions are as follows: the titanium alloy billet is heated at 480°C for 160 minutes; the temperature is raised to 930°C and the temperature is maintained for 240 minutes; the total furnace time is 400 minutes; the perforation is performed, the reduction is ≥13%, the ovality is 1.16-1.18, and a rough tube is obtained, and the length of the rough tube is controlled at 6.5-7.7m; continuous rolling, the outlet speed of the continuous rolling mill is set to 4.8m / s, the limit speed is 80%, and the lubrication speed is 1m / s to obtain a rough tube; sizing, the final rolling temperature is 880°C, and a titanium alloy tube is obtained;

[0051] Step (2) Surface treatment:

[0052] The titanium alloy tube obtained in the previous step was surface treated, and the process was as follows: in a temperature environment of 1000°C, argon was used as the working gas, and plasma cleaning was performed for 20 minutes; in a mixed gas atmosphere of hydrogen and methane, borane ammonia complex was injected, the hydrogen flow rate was 40 mL / min, the methane flow rate was 6 mL / min, the reaction deposition was 60 minutes, the vacuum chamber pressure was 2 Pa, and the voltage was 800 V; in a mixed gas atmosphere of argon, hydrogen and nitrogen, titanium tetrachloride and tetramethylsilane were injected with hydrogen as the carrier gas, the deposition temperature was 550°C, the argon flow rate was 32 mL / min, the hydrogen flow rate was 100 mL / min, the nitrogen flow rate was 16 mL / min, the deposition time was 120 minutes, the frequency was 8 kHz, the duty cycle was 45%, the voltage was 800 V, and the working pressure was 100 Pa;

[0053] Then, the sealing agent is applied 5 times, and the tube is kept at 100° C. for 150 minutes to form a corrosion-resistant protective layer, thereby obtaining a corrosion-resistant titanium alloy tube.

[0054] Comparative Example 1: A surface corrosion resistance process for a titanium alloy oil casing, comprising the following processes:

[0055] Step (1) hot rolling:

[0056] The titanium alloy billet is heated, and the heating process conditions are as follows: the titanium alloy billet is kept at 400°C for 200 minutes; the temperature is raised to 880°C and kept for 200 minutes; the total furnace time is 400 minutes; the perforation is performed, the reduction is ≥13%, the ovality is 1.16-1.18, and a rough tube is obtained, and the length of the rough tube is controlled at 6.5-7.7m; continuous rolling, the outlet speed of the continuous rolling mill is set to 4.8m / s, the limit speed is 80%, and the lubrication speed is 1m / s to obtain a rough tube; sizing, the final rolling temperature is 780°C, and a titanium alloy tube is obtained;

[0057] Step (2) Surface treatment:

[0058] The titanium alloy tube obtained in the previous step was surface treated, and the process was as follows: in a temperature environment of 950°C, argon was used as the working gas, and plasma cleaning was performed for 15 minutes; in a mixed gas atmosphere of hydrogen and methane, borane ammonia complex was injected, the hydrogen flow rate was 38 mL / min, the methane flow rate was 4 mL / min, the reaction deposition was 40 minutes, the vacuum chamber pressure was 1 Pa, and the voltage was 500 V; in a mixed gas atmosphere of argon, hydrogen and nitrogen, titanium tetrachloride was injected with hydrogen as the carrier gas, the deposition temperature was 510°C, the argon flow rate was 20 mL / min, the hydrogen flow rate was 80 mL / min, the nitrogen flow rate was 10 mL / min, the deposition time was 50 minutes, the frequency was 5 kHz, the duty cycle was 33%, the voltage was 600 V, and the working pressure was 80 Pa; it was placed at a temperature of 80°C and kept warm for 180 minutes to form a corrosion-resistant protective layer to obtain a corrosion-resistant titanium alloy tube.

[0059] Comparative Example 2: A surface corrosion resistance process for a titanium alloy oil casing, comprising the following processes:

[0060] Step (1) hot rolling:

[0061] The titanium alloy billet is heated, and the heating process conditions are as follows: the titanium alloy billet is kept at 400°C for 200 minutes; the temperature is raised to 880°C and kept for 200 minutes; the total furnace time is 400 minutes; the perforation is performed, the reduction is ≥13%, the ovality is 1.16-1.18, and a rough tube is obtained, and the length of the rough tube is controlled at 6.5-7.7m; continuous rolling, the outlet speed of the continuous rolling mill is set to 4.8m / s, the limit speed is 80%, and the lubrication speed is 1m / s to obtain a rough tube; sizing, the final rolling temperature is 780°C, and a titanium alloy tube is obtained;

[0062] Step (2) Surface treatment:

[0063] The titanium alloy tube obtained in the previous step is surface treated, and the process is as follows: in a temperature environment of 950°C and a nitrogen atmosphere, borane ammonia complex is injected, the nitrogen flow rate is 38 mL / min, the reaction deposition is 40 minutes, the vacuum chamber pressure is 1 Pa, and the voltage is 500 V; in a mixed gas atmosphere of argon, hydrogen and nitrogen, titanium tetrachloride is injected with hydrogen as a carrier gas, the deposition temperature is 510°C, the argon flow rate is 20 mL / min, the hydrogen flow rate is 80 mL / min, the nitrogen flow rate is 10 mL / min, the deposition time is 50 minutes, the frequency is 5 kHz, the duty cycle is 33%, the voltage is 600 V, and the working pressure is 80 Pa; it is placed at 80°C and kept warm for 180 minutes to form a corrosion-resistant protective layer to obtain a corrosion-resistant titanium alloy tube.

[0064] Comparative Example 3: A surface corrosion resistance process for a titanium alloy oil casing, comprising the following processes:

[0065] Step (1) hot rolling:

[0066] The titanium alloy billet is heated, and the heating process conditions are as follows: the titanium alloy billet is kept at 400°C for 200 minutes; the temperature is raised to 880°C and kept for 200 minutes; the total furnace time is 400 minutes; the perforation is performed, the reduction is ≥13%, the ovality is 1.16-1.18, and a rough tube is obtained, and the length of the rough tube is controlled at 6.5-7.7m; continuous rolling, the outlet speed of the continuous rolling mill is set to 4.8m / s, the limit speed is 80%, and the lubrication speed is 1m / s to obtain a rough tube; sizing, the final rolling temperature is 780°C, and a titanium alloy tube is obtained;

[0067] Step (2) Surface treatment:

[0068] The titanium alloy tube obtained in the previous step was surface treated, and the process was as follows: in a mixed gas atmosphere of argon, hydrogen and nitrogen, titanium tetrachloride was injected with hydrogen as a carrier gas, the deposition temperature was 510°C, the argon flow rate was 20 mL / min, the hydrogen flow rate was 80 mL / min, the nitrogen flow rate was 10 mL / min, the deposition time was 50 min, the frequency was 5 kHz, the duty cycle was 33%, the voltage was 600 V, and the working pressure was 80 Pa; it was placed at 80°C and kept warm for 180 min to form a corrosion-resistant protective layer to obtain a corrosion-resistant titanium alloy tube.

[0069] Comparative Example 4: A surface corrosion resistance process for a titanium alloy oil casing, comprising the following processes:

[0070] The titanium alloy billet is heated, and the heating process conditions are as follows: the titanium alloy billet is kept at 400°C for 200 minutes; the temperature is raised to 880°C and kept for 200 minutes; the total furnace time is 400 minutes; the perforation is performed, the reduction is ≥13%, the ovality is 1.16-1.18, and a rough tube is obtained, and the length of the rough tube is controlled at 6.5-7.7m; continuous rolling, the outlet speed of the continuous rolling mill is set to 4.8m / s, the limit speed is 80%, and the lubrication speed is 1m / s to obtain a rough tube; sizing, the final rolling temperature is 780°C, and a titanium alloy tube is obtained;

[0071] The pipe obtained after sizing is subjected to heat treatment and straightening to obtain a corrosion-resistant titanium alloy pipe; the heat treatment process conditions are: heating temperature 920°C, insulation for 75 minutes, water cooling; heating to 530°C, insulation for 240 minutes, air cooling after taking out of the furnace; the straightening process conditions are: hot straightening using the residual temperature after heat treatment, and the straightening temperature is 200°C.

[0072] Experiment: The corrosion-resistant titanium alloy tubes obtained in Examples 1-3 and Comparative Examples 1-4 were taken to prepare samples, and their properties were tested and the test results were recorded:

[0073] Mechanical properties test: GB / T228.1 was used as the reference standard to test the tensile properties of the specimens. The test temperature was 25°C and the tensile rate was 1mm / min.

[0074] Corrosion resistance test: The electrochemical workstation was used to conduct electrochemical corrosion test on the sample. A three-electrode system was used with a volume of 1 cm2, the sample was the working electrode, the AgCl electrode was the reference electrode, and graphite was the auxiliary electrode. The corrosion media were 5wt.% HCl and 5wt.% H2SO4 solution respectively. The test time was 3600s and the test frequency range was 10 -2 ~105Hz, voltage amplitude is 10mV.

[0075]

[0076] According to the data in the above table, we can clearly draw the following conclusions:

[0077] The corrosion-resistant titanium alloy tubes obtained in Examples 1-3 are compared with the corrosion-resistant titanium alloy tubes obtained in Comparative Examples 1-4. The test results show that:

[0078] Compared with Comparative Example 4, the tensile strength of the corrosion-resistant titanium alloy tubes obtained in Examples 1-3 did not change much, and the corrosion current density in hydrochloric acid and sulfuric acid decreased significantly, which fully demonstrated that the present invention achieved the improvement of the corrosion resistance of the titanium alloy tube.

[0079] Compared with Example 1, no sealing treatment was performed in the surface treatment process of Comparative Example 1, and no tetramethylsilane was injected; compared with Comparative Example 2, the atmosphere in the surface treatment of Comparative Example 2 was different and no plasma cleaning was performed; compared with Comparative Example 3, the surface treatment of Comparative Example 3 was the injection of titanium tetrachloride; the corrosion-resistant titanium alloy tubes obtained in Comparative Examples 1-3 had increased tensile strength and corrosion current density in hydrochloric acid and sulfuric acid. It can be seen that the setting of the surface treatment process of the present invention can promote the improvement of the corrosion resistance of the titanium alloy tube while maintaining its strength.

[0080] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process method article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process method article or device.

[0081] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A surface corrosion resistance process for titanium alloy oil casing, characterized by: Including the following processes: Step (1) hot rolling: heating the titanium alloy billet, punching, continuous rolling, sizing, and heat treating and straightening the obtained tube after sizing. The heat treatment process conditions are: heating temperature 900-950°C, heat preservation 60-90min, water cooling; heating to 510-550°C, heat preservation 230-250min, air cooling after exiting the furnace; straightening process conditions are: hot straightening using the residual temperature after heat treatment, the straightening temperature is 180-230°C, and a titanium alloy tube is obtained; Step (2) surface treatment: performing surface treatment on the titanium alloy tube obtained in the previous step to form a corrosion-resistant protective layer to obtain a corrosion-resistant titanium alloy tube; The surface treatment process is as follows: Using chemical vapor deposition technology, titanium nitride is deposited on the surface of the titanium alloy tube to form a thin titanium nitride layer; then a sealing agent is applied, heat treatment is performed, and a corrosion-resistant protective layer is formed to obtain a corrosion-resistant titanium alloy tube; The chemical vapor deposition technology is plasma enhanced chemical vapor deposition, and the process is as follows: S1, injecting borane ammonia complex in a mixed gas atmosphere of hydrogen and methane at a temperature of 950 to 1000° C., and reacting and depositing for 40 to 60 minutes; before the implementation of S1, plasma cleaning is performed for 15 to 20 minutes in a temperature environment of 950 to 1000° C. with argon as the working gas; S2. In an atmosphere of a mixture of argon, hydrogen and nitrogen, titanium tetrachloride and tetramethylsilane are injected with hydrogen as a carrier gas at a deposition temperature of 510 to 550° C. for a deposition time of 50 to 120 min.

2. The surface corrosion resistance process of a titanium alloy oil casing according to claim 1 is characterized in that: In step (1), the heating process conditions are as follows: the titanium alloy billet is heated to 400-480°C and kept at this temperature for 160-200 min; the temperature is raised to 880-930°C and kept at this temperature for 200-240 min; and the total time in the furnace is 390-400 min.

3. The surface corrosion resistance process of a titanium alloy oil casing according to claim 1 is characterized in that: The titanium alloy blank comprises the following components by mass: vanadium: 3.5% to 4.5%, aluminum: 5.50% to 6.75%, iron: ≤0.3%, carbon: ≤0.08%, nitrogen: ≤0.05%, hydrogen: ≤0.015%, oxygen: ≤0.20%, and the balance is titanium.

4. The surface corrosion resistance process of a titanium alloy oil casing according to claim 1 is characterized in that: In S1, the hydrogen flow rate is 38-40 mL / min, the methane flow rate is 4-6 mL / min, the vacuum chamber pressure is 1-2 Pa, and the voltage is 500-800 V.

5. The surface corrosion resistance process of a titanium alloy oil casing according to claim 1 is characterized in that: In S2, the argon flow rate is 20-32 mL / min, the hydrogen flow rate is 80-100 mL / min, and the nitrogen flow rate is 10-16 mL / min; the frequency is 5-8 kHz, the duty cycle is 33%-45%, the voltage is 600-800 V, and the working pressure is 80-100 Pa.

6. The surface corrosion resistance process of a titanium alloy oil casing according to claim 1 is characterized in that: The sealing agent is one of silica sol and aluminum sol or a mixture of the two.

7. The surface corrosion resistance process of a titanium alloy oil casing according to claim 1 is characterized by: The heat treatment process is: keeping the temperature at 80-100° C. for 150-180 minutes.

Citation Information

Patent Citations

  • Method for producing high-strength titanium alloy seamless tube

    CN104259246A

  • Titanium alloy tube and production method thereof

    CN104308461A

  • Titanium alloy pipe and preparation process

    CN107779666A

  • High-toughness titanium alloy oil well pipe and manufacturing method thereof

    CN110303067A

  • Preparation method of boron-carbon-nitrogen film

    CN113151803A