A kind of sodium iron sulfate composite positive electrode material and preparation method thereof

CN118291937BActive Publication Date: 2024-10-08HENAN SOLID LITHIUM BATTERY TECH CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202410411835.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-08
Publication Date
2024-10-08
Estimated Expiration
2044-04-08

AI Technical Summary

Technical Problem

但是文献1使用的是单纯的化学合成的方法,这种方法制备的正极材料的晶粒尺寸分布较大,某些晶粒尺寸为10nm左右,有些晶粒尺寸达到80nm,根据我司的研究,这种晶粒分布较大的情况将影响电池性能的提升

Benefits of technology

[0020] Compared with the prior art, the present invention has the following advantages: the prior art uses a simple chemical synthesis method to prepare cathode materials. The cathode materials prepared by this method have a larger grain size distribution, and some grain sizes are about 10 nm. , some grain sizes reach 80nm. In addition, the methods proposed in the prior art can only produce compounds with simple components, which will also adversely affect the improvement of battery performance. In view of the problems existing in the prior art, the present invention proposes a new process for preparing sodium ferric sulfate cathode material. The process of the present invention ensures that the crystal grain size of the cathode material is smaller and the distribution is more uniform. At the same time, the method of the present invention can prepare A richer cathode material improves battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118291937B_ABST
    Figure CN118291937B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a sodium ferric sulfate composite positive electrode material, comprising: depositing Na2FeMn on a silicon substrate by magnetron sputtering. 0.8 Nd 0.2 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.8 Nd 0.2 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Dy 0.3 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.7 Dy 0.3 Na2FeMn is deposited on (SO4)3 layer 0.9 Dy 0.1 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.9 Dy 0.1 Na2FeMn is deposited on (SO4)3 layer 0.9 Ce 0.1 (SO4)3 layers; peeling the composite film from the silicon substrate to obtain a sodium iron sulfate composite positive electrode material. The method of the present invention ensures that the positive electrode material has a smaller grain size and a more uniform distribution. At the same time, the method of the present invention can prepare a positive electrode material with richer ingredients, thereby improving battery performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sodium ion batteries, and in particular to a sodium iron sulfate composite positive electrode material and a preparation method thereof. Background Art

[0002] Sodium-ion battery is a rechargeable battery that uses sodium ions as charge carriers. Its working principle and structure are similar to those of lithium-ion batteries. The only difference is that sodium, which is in the same group of the periodic table and has similar chemical properties, replaces lithium. Sodium-ion batteries have the following advantages: Rich resources: Sodium is abundant on Earth and has relatively low cost; Good low-temperature performance: It performs relatively well in low-temperature environments; Fast charging performance: It has good fast charging capabilities; High safety: It usually has high safety; Structural stability: The structure is relatively stable and has a long cycle life.

[0003] At present, sodium-ion batteries have broad application prospects in the future due to their high safety, low cost, high energy density, and long cycle life. However, at the same cost, the performance of sodium-ion batteries needs to be further improved, so there are many studies on improving the performance of sodium-ion batteries.

[0004] Prior art CN116706056A (hereinafter referred to as document 1) proposes a method based on ultra-small particles of Na x Fe y M z (SO4)3 lossless fast-charging positive electrode material and its preparation method and application. Document 1 states: "Because the product has small grains and sufficient inter-grain gaps, it is beneficial to relieve the deformation stress caused by the embedding / removal of sodium ions, improve the product cycle stability, and achieve lossless charging and discharging of the product. At the same time, the material has a large specific surface area, which can provide abundant active energy storage sites and promote the specific capacity of the material. In addition, the partial substitution of transition metal ions further improves the reaction activity of the material, thereby improving the rate performance of the material." It can be seen that Document 1 mainly improves battery performance by reducing the grain size. However, Document 1 uses a simple chemical synthesis method. The grain size distribution of the positive electrode material prepared by this method is large, some of the grain sizes are about 10nm, and some of the grain sizes reach 80nm. According to our research, this large grain distribution will affect the improvement of battery performance. In addition, the method proposed in Document 1 can only produce compounds with simple ingredients, which will also adversely affect the improvement of battery performance. Summary of the invention

[0005] To achieve the above object, the present invention provides a method for preparing a sodium iron sulfate composite positive electrode material, characterized in that the method comprises:

[0006] Deposition of Na2FeMn on silicon substrate using magnetron sputtering0.8 Nd 0.2 (SO4) 3 layers;

[0007] Magnetron sputtering was used to deposit Na2FeMn 0.8 Nd 0.2 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 (SO4) 3 layers;

[0008] Magnetron sputtering was used to deposit Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Dy 0.3 (SO4) 3 layers;

[0009] Magnetron sputtering was used to deposit Na2FeMn 0.7 Dy 0.3 Na2FeMn is deposited on (SO4)3 layer 0.9 Dy 0.1 (SO4) 3 layers;

[0010] Magnetron sputtering was used to deposit Na2FeMn 0.9 Dy 0.1 Na2FeMn is deposited on (SO4)3 layer 0.9 Ce 0.1 (SO4) 3 layers;

[0011] The composite film is peeled off from the silicon substrate to obtain the sodium iron sulfate composite positive electrode material.

[0012] In a preferred embodiment, Na2FeMn 0.8 Nd 0.2 The thickness of (SO4)3 layer is 200-300nm, Na2FeMn 0.7 Nd 0.3 The thickness of the (SO4)3 layer is 200-300nm.

[0013] In a preferred embodiment, Na2FeMn 0.7 Dy 0.3 The thickness of (SO4)3 layer is 300-400nm, Na2FeMn 0.9 Dy 0.1 The thickness of (SO4)3 layer is 300-400nm, Na2FeMn 0.9 Ce 0.1 The thickness of the (SO4)3 layer is 200-300nm.

[0014] In a preferred embodiment, Na2FeMn is deposited on a silicon substrate using magnetron sputtering. 0.8 Nd0.2 The specific process of (SO4)3 layer is: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 30-50sccm, the sputtering power is 150-200W, the sputtering voltage is 100-200V, and the sputtering temperature is 100-150℃.

[0015] In a preferred embodiment, magnetron sputtering is used to deposit Na2FeMn 0.8 Nd 0.2 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 30-50sccm, the sputtering power is 250-300W, the sputtering voltage is 150-200V, and the sputtering temperature is 100-150℃.

[0016] In a preferred embodiment, magnetron sputtering is used to deposit Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Dy 0.3 The specific process of (SO4)3 layer is: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 30-50sccm, the sputtering power is 150-200W, the sputtering voltage is 100-200V, and the sputtering temperature is 100-150℃.

[0017] In a preferred embodiment, magnetron sputtering is used to deposit Na2FeMn 0.7 Dy 0.3 Na2FeMn is deposited on (SO4)3 layer 0.9 Dy 0.1 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 30-50sccm, the sputtering power is 250-300W, the sputtering voltage is 150-200V, and the sputtering temperature is 100-150℃.

[0018] In a preferred embodiment, magnetron sputtering is used to deposit Na2FeMn 0.9 Dy 0.1 Na2FeMn is deposited on (SO4)3 layer 0.9 Ce 0.1 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 30-50sccm, the sputtering power is 250-300W, the sputtering voltage is 150-200V, and the sputtering temperature is 100-150℃.

[0019] The present invention also provides a sodium iron sulfate composite positive electrode material, wherein the positive electrode material is prepared using the above-mentioned preparation method.

[0020] Compared with the prior art, the present invention has the following advantages: the prior art uses a simple chemical synthesis method to prepare positive electrode materials. The grain size distribution of the positive electrode materials prepared by this method is relatively large, with some grain sizes of about 10nm and some grain sizes reaching 80nm. In addition, the method proposed in the prior art can only produce compounds with simple ingredients, which will also adversely affect the improvement of battery performance. In view of the problems existing in the prior art, the present invention proposes a new process for preparing sodium ferric sulfate positive electrode materials. The process of the present invention ensures that the grain size of the positive electrode material is smaller and the distribution is more uniform. At the same time, the method of the present invention can prepare positive electrode materials with richer ingredients, thereby improving battery performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the membrane layer structure of an embodiment of the present invention.

[0022] Figure 2 It is a method flow chart of an embodiment of the present invention.

[0023] Figure 3 This is a TEM photograph of one example of the present invention.

[0024] Figure 4 This is a TEM photograph of one example of the present invention. DETAILED DESCRIPTION

[0025] The specific implementation modes of the present invention are described in detail below in conjunction with the accompanying drawings, but it should be understood that the protection scope of the present invention is not limited by the specific implementation modes.

[0026] Figure 2 1 is a method flow chart of an embodiment of the present invention. As shown in the figure, the method of the present invention includes the following steps:

[0027] Step 1: Deposition of Na2FeMn on silicon substrate using magnetron sputtering 0.8 Nd 0.2 (SO4)3 layer; It should be understood by those skilled in the art that Na2FeMn 0.8 Nd 0.2 (SO4)3 layer is made of Na2FeMn 0.8 Nd 0.2The (SO4)3 target material is deposited in combination with a magnetron sputtering method. The method for making the target material can refer to document 1, and part of the content of document 1 is quoted here (the remaining necessary parameters can refer to the process of the embodiment of document 1), sodium sulfate is selected as the sodium source, ferrous nitrate is selected as the iron source, manganese sulfate is selected as the soluble salt of Mn, ferrous sulfate is selected as the sulfur source, and NdCl2 is selected as the soluble salt of Nd (the existence of NdCl2 can be proved by U.S. Patent Document US7048809B2, and the substance can be purchased from a chemical store), and the raw materials (that is, sodium sulfate, ferrous nitrate, manganese sulfate, ferrous sulfate, and NdCl2) are configured according to the atomic ratio of the chemical formula, and the suspension is placed in a hydrothermal kettle, and a solvent thermal reaction is carried out at 100°C for 4h; after naturally cooling to room temperature, the product of the solvent thermal reaction is centrifuged, and then washed with ethanol and deionized water to obtain a primary product with a water content of about 20%, and then the primary product is placed in a dryer in a drying chamber, and flash dried for 0.5h at 200°C and a gas flow rate of 2m / s to obtain Na2FeMn 0.8 Nd 0.2 (SO4)3 powder particles; the obtained powder particles were calcined at 350℃ for 8h under argon atmosphere, wherein: the heating rate was 1℃ / min. 0.8 Nd 0.2 The powder particles of (SO4)3 are put into a ball mill for ball milling (this step is mainly to prevent powder agglomeration), and then the powder particles after ball milling are subjected to cold isostatic pressing and low-temperature hot pressing, and then Na2FeMn can be obtained. 0.8 Nd 0.2 (SO4)3 target;

[0028] Step 2: Magnetron sputtering on Na2FeMn 0.8 Nd 0.2 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 (SO4)3 layer; It should be understood by those skilled in the art that Na2FeMn 0.7 Nd 0.3 (SO4)3 layer is made of Na2FeMn 0.7 Nd 0.3 (SO4)3 target material is deposited by combining magnetron sputtering method. Na2FeMn 0.7 Nd 0.3 The preparation method of (SO4)3 target can refer to the method in step 1;

[0029] Step 3: Magnetron sputtering on Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Dy 0.3(SO4)3 layer; It should be understood by those skilled in the art that Na2FeMn 0.7 Dy 0.3 (SO4)3 layer is made of Na2FeMn 0.7 Dy 0.3 (SO4)3 target material is deposited by combining magnetron sputtering method. Na2FeMn 0.7 Dy 0.3 The preparation method of the (SO4)3 target material can refer to the method in step 1. In addition, the soluble salt of Dy is DyCl2 (the existence of DyCl2 can be proved by US Patent Document US11203011B2);

[0030] Step 4: Magnetron sputtering on Na2FeMn 0.7 Dy 0.3 Na2FeMn is deposited on (SO4)3 layer 0.9 Dy 0.1 (SO4)3 layer; It should be understood by those skilled in the art that Na2FeMn 0.9 Dy 0.1 (SO4)3 layer is made of Na2FeMn 0.9 Dy 0.1 (SO4)3 target material is deposited by combining magnetron sputtering method. Na2FeMn 0.9 Dy 0.1 The preparation method of (SO4)3 target can refer to the method in step 1;

[0031] Step 5: Magnetron sputtering on Na2FeMn 0.9 Dy 0.1 Na2FeMn is deposited on (SO4)3 layer 0.9 Ce 0.1 (SO4)3 layer; It should be understood by those skilled in the art that Na2FeMn 0.9 Ce 0.1 (SO4)3 layer is made of Na2FeMn 0.9 Ce 0.1 (SO4)3 target material is deposited by combining magnetron sputtering method. Na2FeMn 0.9 Ce 0.1 The preparation method of the (SO4)3 target material can refer to the method in step 1; in addition, the soluble salt of Ce is selected as CeCl2 (the existence of CeCl2 can be proved by US Patent Document US8052889B2);

[0032] Step 6: Peel off the composite film from the silicon substrate to obtain the sodium iron sulfate composite positive electrode material. The structure of the composite film can be referred to Figure 1 ,like Figure 1As shown, the composite film of the present invention comprises Na2FeMn on a silicon substrate in sequence. 0.8 Nd 0.2 (SO4)3 layers, Na2FeMn 0.7 Nd 0.3 (SO4)3 layers, Na2FeMn 0.7 Dy 0.3 (SO4)3 layers, Na2FeMn 0.9 Dy 0.1 (SO4)3 layers, and Na2FeMn 0.9 Ce 0.1 (SO4)3 layer. The method of film stripping is well known in the art, for example, the film can be stripped from the silicon substrate by mechanical method.

[0033] Example 1

[0034] The cathode material was prepared by the following method: Na2FeMn was deposited on a silicon substrate using magnetron sputtering. 0.8 Nd 0.2 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.8 Nd 0.2 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Dy 0.3 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.7 Dy 0.3 Na2FeMn is deposited on (SO4)3 layer 0.9 Dy 0.1 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.9 Dy 0.1 Na2FeMn is deposited on (SO4)3 layer 0.9 Ce 0.1 (SO4)3 layers; peeling the composite film from the silicon substrate to obtain the sodium ferric sulfate composite positive electrode material.

[0035] Na2FeMn 0.8 Nd 0.2 The thickness of (SO4)3 layer is 200nm, Na2FeMn 0.7 Nd 0.3 The thickness of the (SO4)3 layer is 200nm. Na2FeMn 0.7 Dy 0.3 The thickness of (SO4)3 layer is 300nm, Na2FeMn0.9 Dy 0.1 The thickness of (SO4)3 layer is 300nm, Na2FeMn 0.9 Ce 0.1 The thickness of the (SO4)3 layer is 200 nm.

[0036] Deposition of Na2FeMn on silicon substrate using magnetron sputtering 0.8 Nd 0.2 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 150W, the sputtering voltage is 100V, and the sputtering temperature is 100°C.

[0037] Magnetron sputtering was used to deposit Na2FeMn 0.8 Nd 0.2 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 The specific process of (SO4)3 layer is: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 250W, the sputtering voltage is 150V, and the sputtering temperature is 100℃.

[0038] Magnetron sputtering was used to deposit Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Dy 0.3 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 150W, the sputtering voltage is 100V, and the sputtering temperature is 100°C.

[0039] Magnetron sputtering was used to deposit Na2FeMn 0.7 Dy 0.3 Na2FeMn is deposited on (SO4)3 layer 0.9 Dy 0.1 The specific process of (SO4)3 layer is: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 250W, the sputtering voltage is 150V, and the sputtering temperature is 100℃.

[0040] Magnetron sputtering was used to deposit Na2FeMn 0.9 Dy 0.1 Na2FeMn is deposited on (SO4)3 layer 0.9 Ce 0.1The specific process of (SO4)3 layer is as follows: the magnetron sputtering power source is a radio frequency power source, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 250W, the sputtering voltage is 150V, and the sputtering temperature is 100°C. The preparation of the test battery can refer to the method of reference 1. In order to ensure the integrity of the specification, the battery preparation method proposed in reference 1 is quoted in this part. First, the composite film of Example 1 peeled off from the silicon substrate is crushed to the degree required for making the battery by ball milling. Then, the powder, carbon black, and polyvinylidene fluoride formed by crushing the composite film are added to an appropriate amount of N-methylpyrrolidone in a mass ratio of 8:1:1, and fully ground to obtain a uniform slurry; then the slurry is evenly coated on the surface of the aluminum foil and vacuum dried; then the dried electrode sheet is cut into a disc with a diameter of 10mm, and after compaction, it is used as a positive electrode sheet of the battery for standby; the battery negative electrode and battery assembly method refer to paragraphs 0164 and 0165 of the specification of reference 1; in order to increase the comparability of the results, the test method refers to paragraph 0180 of the specification of reference 1. The battery manufacturing method and testing method of the subsequent embodiments and comparative examples are the same as those of Example 1, and the battery manufacturing method and testing method will not be repeated in the subsequent embodiments and comparative examples. The battery manufactured using the positive electrode material obtained in Example 1 has a 1C first-cycle discharge specific capacity (mAh / g) of 130.5, a 1C first-cycle coulombic efficiency of 90.5%, and a 1C, 500-cycle capacity retention rate of 97.3%. The battery manufactured using the positive electrode material obtained by the preparation method of the present invention has a significant improvement in the 1C first-cycle discharge specific capacity compared to Document 1. According to the analysis of our researchers, the main sources of this improvement are two points: First, the magnetron sputtering method is particularly suitable for preparing materials with small grain sizes. In fact, due to the fast deposition rate of magnetron sputtering and the slow atomic diffusion rate, many materials prepared by the magnetron sputtering method can even form amorphous. After slightly reducing the deposition rate, film materials with smaller grain sizes can be easily obtained. In order to verify this point of view, it is provided Figure 3 and Figure 4 TEM photos of Figure 3 The sample was prepared by depositing Na2FeMn on a silicon substrate using the process described in Example 1. 0.8 Nd 0.2 (SO4)3 layers, followed by direct addition of Na2FeMn 0.8 Nd 0.2The (SO4)3 layer is peeled off from the silicon substrate, and then the peeled film is subjected to TEM testing (due to the poor TEM imaging effect of the composite film layer, the present invention chooses to deposit only one layer of film when taking TEM photos, and then directly peels off to take TEM photos, which helps to improve the quality of the photos; it is well known that subsequent sputtering will not affect the grain size of the previously sputtered film layer, and the grain size can only be increased through heat treatment. Therefore, even if the present invention adopts the testing method of depositing only one layer of film and then directly peeling off to take TEM photos, the test results can also prove the views of our researchers). Figure 3 The white line in the figure is an auxiliary line used to identify a grain. Figure 3 It can be seen from the graph that the grain size of the positive electrode material of the present invention is approximately 4-5 nm. Figure 4 This is a TEM image of another field of view of the same sample. Figure 4 It can be seen that the size of another grain is also about 4-5nm. It can be seen that the process provided by the present invention can prepare positive electrode materials with nano-scale grain sizes, and combined with Figure 3 and Figure 4 It can be seen (of course, it needs to be combined with battery performance test to assist in proof) that the grain size distribution of the present invention is relatively small, and the grain size distribution in Document 1 will not be from 10nm to 80nm. Therefore, the battery performance obtained by the present invention is improved compared with Document 1. Second, because the present invention dopes rare earths in the components, and because the present invention uses a magnetron sputtering process, the single-component positive electrode material of Document 1 can be transformed into a composite positive electrode material with multiple components, which enables various rare earth elements to exert the characteristics of their respective f-layer electrons. The f-layer electrons of these rare earth elements can change the energy band structure of the material, thereby improving the diffusion capacity of ions and electrons, thereby improving the performance of the battery.

[0041] Example 2

[0042] The cathode material was prepared by the following method: Na2FeMn was deposited on a silicon substrate using magnetron sputtering. 0.8 Nd 0.2 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.8 Nd 0.2 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Dy 0.3 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.7 Dy 0.3Na2FeMn is deposited on (SO4)3 layer 0.9 Dy 0.1 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.9 Dy 0.1 Na2FeMn is deposited on (SO4)3 layer 0.9 Ce 0.1 (SO4)3 layers; peeling the composite film from the silicon substrate to obtain the sodium ferric sulfate composite positive electrode material.

[0043] Na2FeMn 0.8 Nd 0.2 The thickness of (SO4)3 layer is 300nm, Na2FeMn 0.7 Nd 0.3 The thickness of the (SO4)3 layer is 300nm. Na2FeMn 0.7 Dy 0.3 The thickness of (SO4)3 layer is 400nm, Na2FeMn 0.9 Dy 0.1 The thickness of (SO4)3 layer is 400nm, Na2FeMn 0.9 Ce 0.1 The thickness of the (SO4)3 layer is 300 nm.

[0044] Deposition of Na2FeMn on silicon substrate using magnetron sputtering 0.8 Nd 0.2 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 200W, the sputtering voltage is 200V, and the sputtering temperature is 150°C.

[0045] Magnetron sputtering was used to deposit Na2FeMn 0.8 Nd 0.2 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 300W, the sputtering voltage is 200V, and the sputtering temperature is 150°C.

[0046] Magnetron sputtering was used to deposit Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Dy 0.3 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 200W, the sputtering voltage is 200V, and the sputtering temperature is 150°C.

[0047] Magnetron sputtering was used to deposit Na2FeMn 0.7 Dy 0.3 Na2FeMn is deposited on (SO4)3 layer 0.9 Dy 0.1 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 300W, the sputtering voltage is 200V, and the sputtering temperature is 150°C.

[0048] Magnetron sputtering was used to deposit Na2FeMn 0.9 Dy 0.1 Na2FeMn is deposited on (SO4)3 layer 0.9 Ce 0.1 The specific process of the (SO4)3 layer is as follows: the magnetron sputtering power source is a radio frequency power source, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40 sccm, the sputtering power is 300 W, the sputtering voltage is 200 V, and the sputtering temperature is 150° C. The battery manufactured using the positive electrode material obtained in Example 2 has a 1C first cycle discharge specific capacity (mAh / g) of 132.1, a 1C first cycle coulomb efficiency of 89.5%, and a 1C, 500 cycle capacity retention rate of 97.4%.

[0049] Example 3

[0050] The cathode material was prepared by the following method: Na2FeMn was deposited on a silicon substrate using magnetron sputtering. 0.8 Nd 0.2 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.8 Nd 0.2 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Dy 0.3 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.7 Dy 0.3 Na2FeMn is deposited on (SO4)3 layer 0.9 Dy 0.1 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.9 Dy 0.1 Na2FeMn is deposited on (SO4)3 layer 0.9 Ce 0.1 (SO4)3 layers; peeling the composite film from the silicon substrate to obtain the sodium ferric sulfate composite positive electrode material.

[0051] Na2FeMn 0.8 Nd 0.2 The thickness of (SO4)3 layer is 250nm, Na2FeMn 0.7 Nd 0.3 The thickness of the (SO4)3 layer is 250nm. Na2FeMn 0.7 Dy 0.3 The thickness of (SO4)3 layer is 350nm, Na2FeMn 0.9 Dy 0.1 The thickness of (SO4)3 layer is 350nm, Na2FeMn 0.9 Ce 0.1 The thickness of the (SO4)3 layer is 250 nm.

[0052] Deposition of Na2FeMn on silicon substrate using magnetron sputtering 0.8 Nd 0.2 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 170W, the sputtering voltage is 150V, and the sputtering temperature is 120°C.

[0053] Magnetron sputtering was used to deposit Na2FeMn 0.8 Nd 0.2 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 270W, the sputtering voltage is 170V, and the sputtering temperature is 120℃.

[0054] Magnetron sputtering was used to deposit Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Dy 0.3 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 170W, the sputtering voltage is 150V, and the sputtering temperature is 120°C.

[0055] Magnetron sputtering was used to deposit Na2FeMn 0.7 Dy 0.3 Na2FeMn is deposited on (SO4)3 layer 0.9 Dy 0.1 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 270W, the sputtering voltage is 180V, and the sputtering temperature is 120℃.

[0056] Magnetron sputtering was used to deposit Na2FeMn 0.9 Dy 0.1 Na2FeMn is deposited on (SO4)3 layer 0.9 Ce 0.1 The specific process of the (SO4)3 layer is as follows: the magnetron sputtering power source is a radio frequency power source, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40 sccm, the sputtering power is 270 W, the sputtering voltage is 170 V, and the sputtering temperature is 120° C. The battery manufactured using the positive electrode material obtained in Example 3 has a 1C first cycle discharge specific capacity (mAh / g) of 131.4, a 1C first cycle coulomb efficiency of 91.5%, and a 1C, 500 cycle capacity retention rate of 97.7%.

[0057] Comparative Example 1

[0058] The cathode material was prepared by the following method: Na2FeMn was deposited on a silicon substrate using magnetron sputtering. 0.8 Nd 0.2 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.8 Nd 0.2 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.9 Nd 0.1 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.9 Nd 0.1 Na2FeMn is deposited on (SO4)3 layer 0.9 Nd 0.1 (SO4)3 layers; peel off the composite film from the silicon substrate to obtain the sodium iron sulfate composite positive electrode material. The thickness of each layer is 200nm. Na2FeMn 0.8 Nd 0.2 (SO4)3 layer and Na2FeMn 0.7 Nd 0.3 The magnetron sputtering process of the (SO4)3 layer refers to that of Example 1. The magnetron sputtering process of the other layers refers to that of the Na2FeMn 0.8 Nd 0.2(SO4) 3 layers of magnetron sputtering process. The battery manufactured using the positive electrode material obtained in Comparative Example 1 has a 1C first cycle discharge specific capacity (mAh / g) of 123.2, a 1C first cycle coulomb efficiency of 88.9%, and a 1C, 500 cycle capacity retention rate of 96.7%. It can be seen that the composite thin film positive electrode material formed by a rich variety of rare earth elements can maximize the battery performance.

[0059] Comparative Example 2

[0060] The cathode material was prepared by the following method: Na2FeMn was deposited on a silicon substrate using magnetron sputtering. 0.5 Nd 0.5 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.5 Nd 0.5 Na2FeMn is deposited on (SO4)3 layer 0.6 Nd 0.4 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.6 Nd 0.4 Na2FeMn is deposited on (SO4)3 layer 0.5 Dy 0.5 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.5 Dy 0.5 Na2FeMn is deposited on (SO4)3 layer 0.6 Dy 0.4 (SO4)3 layer; magnetron sputtering on Na2FeMn 0.6 Dy 0.4 Na2FeMn is deposited on (SO4)3 layer 0.6 Ce 0.4 (SO4)3 layers; the composite film is peeled off from the silicon substrate to obtain a sodium ferric sulfate composite positive electrode material. The remaining parameters refer to Example 1. The battery manufactured using the positive electrode material obtained in Comparative Example 2 has a 1C first-cycle discharge specific capacity (mAh / g) of 117.3, a 1C first-cycle coulomb efficiency of 88.7%, and a 1C, 500-cycle capacity retention rate of 95.7%. It can be seen that the ratio between rare earth elements and transition metals (Mn) needs to be controlled. If the rare earth elements are doped too much, it may lead to excessive changes in the band structure and affect the role of the transition metal elements, thereby causing the battery performance to decline.

[0061] Comparative Example 3

[0062] Na2FeMn 0.8 Nd 0.2 The thickness of (SO4)3 layer is 500nm, Na2FeMn 0.7 Nd 0.3 The thickness of the (SO4)3 layer is 500nm. Na2FeMn 0.7Dy 0.3 The thickness of (SO4)3 layer is 500nm, Na2FeMn 0.9 Dy 0.1 The thickness of (SO4)3 layer is 500nm, Na2FeMn 0.9 Ce 0.1 The thickness of the (SO4)3 layer is 500nm. The remaining parameters refer to Example 1. The battery manufactured using the positive electrode material obtained in Comparative Example 3 has a 1C first-cycle discharge specific capacity (mAh / g) of 112.4, a 1C first-cycle coulomb efficiency of 89.5%, and a 1C, 500-cycle capacity retention rate of 92.7%. Although increasing the thickness of each layer can increase the output of positive electrode materials (the thicker the film layer, the heavier the weight of the film obtained per unit area, that is, the greater the output), if the film layer thickness is too large, due to the effect of stress during deposition, this will cause micro cracks to appear inside the film layer, and will also cause detachment of the interface between the film layers. These cracks will hinder the diffusion of electrons and ions, thereby causing a decrease in battery performance.

[0063] Comparative Example 4

[0064] Magnetron sputtering was used to deposit Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Dy 0.3 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 40sccm, the sputtering power is 600W, the sputtering voltage is 300V, and the sputtering temperature is 150°C. The remaining parameters refer to Example 1. The 1C first cycle discharge specific capacity (mAh / g) of the battery manufactured using the positive electrode material obtained in Comparative Example 4 is 118.4, the 1C first cycle coulomb efficiency is 89.5%, and the 1C, 500 cycle capacity retention rate is 94.7%. Excessive sputtering power and sputtering voltage lead to too fast deposition speed, which first leads to the appearance of amorphous inside the positive electrode material, and also leads to micro cracks inside the film layer and detachment of the interface between the film layers. This may lead to a decrease in battery performance.

[0065] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.

Claims

1. A method for preparing a sodium iron sulfate composite positive electrode material, characterized in that: The preparation method comprises the following steps: Deposition of Na2FeMn on silicon substrate using magnetron sputtering 0.8 Nd 0.2 (SO4) 3 layers; Using magnetron sputtering on the Na2FeMn 0.8 Nd 0.2 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 (SO4) 3 layers; Using magnetron sputtering on the Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Dy 0.3 (SO4) 3 layers; Using magnetron sputtering on the Na2FeMn 0.7 Dy 0.3 Na2FeMn is deposited on (SO4)3 layer 0.9 Dy 0.1 (SO4) 3 layers; Using magnetron sputtering on the Na2FeMn 0.9 Dy 0.1 Na2FeMn is deposited on (SO4)3 layer 0.9 Ce 0.1 (SO4) 3 layers; The composite film is peeled off from the silicon substrate to obtain the sodium ferric sulfate composite positive electrode material.

2. The preparation method according to claim 1, characterized in that The Na2FeMn 0.8 Nd 0.2 The thickness of the (SO4)3 layer is 200-300nm, and the Na2FeMn 0.7 Nd 0.3 The thickness of the (SO4)3 layer is 200-300nm.

3. The preparation method according to claim 1, characterized in that: The Na2FeMn 0.7 Dy 0.3 The thickness of the (SO4)3 layer is 300-400nm, and the Na2FeMn 0.9 Dy 0.1 The thickness of the (SO4)3 layer is 300-400nm, and the Na2FeMn 0.9 Ce 0.1 The thickness of the (SO4)3 layer is 200-300nm.

4. The preparation method according to claim 1, characterized in that: Deposition of Na2FeMn on silicon substrate using magnetron sputtering 0.8 Nd 0.2 The specific process of (SO4)3 layer is: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 30-50sccm, the sputtering power is 150-200W, the sputtering voltage is 100-200V, and the sputtering temperature is 100-150℃.

5. The method according to claim 1, characterized in that Using magnetron sputtering on the Na2FeMn 0.8 Nd 0.2 Na2FeMn is deposited on (SO4)3 layer 0.7 Nd 0.3 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 30-50sccm, the sputtering power is 250-300W, the sputtering voltage is 150-200V, and the sputtering temperature is 100-150℃.

6. The preparation method according to claim 1, characterized in that: Using magnetron sputtering on the Na2FeMn 0.7 Nd 0.3 Na2FeMn is deposited on (SO4)3 layer 0.7 Dy 0.3 The specific process of (SO4)3 layer is: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 30-50sccm, the sputtering power is 150-200W, the sputtering voltage is 100-200V, and the sputtering temperature is 100-150℃.

7. The preparation method according to claim 1, characterized in that: Using magnetron sputtering on the Na2FeMn 0.7 Dy 0.3 Na2FeMn is deposited on (SO4)3 layer 0.9 Dy 0.1 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 30-50sccm, the sputtering power is 250-300W, the sputtering voltage is 150-200V, and the sputtering temperature is 100-150℃.

8. The preparation method according to claim 1, characterized in that: Using magnetron sputtering on the Na2FeMn 0.9 Dy 0.1 Na2FeMn is deposited on (SO4)3 layer 0.9 Ce 0.1 The specific process of (SO4)3 layer is as follows: the magnetron sputtering power supply is a radio frequency power supply, the sputtering atmosphere is an argon atmosphere, the argon flow rate is 30-50sccm, the sputtering power is 250-300W, the sputtering voltage is 150-200V, and the sputtering temperature is 100-150℃.

9. A sodium iron sulfate composite positive electrode material, characterized in that: The positive electrode material is prepared using the preparation method as described in any one of claims 1 to 8.

Citation Information

Patent Citations

  • Non-destructive fast-charging positive electrode material based on ultra-small particle NaxFeyMz (SO4) 3 and preparation method and application of non-destructive fast-charging positive electrode material

    CN116706056A

  • Nitrogen oxide reduction catalyst regenerable at low temperature

    US11203011B2

  • Magnetic implement having a linear BH loop

    US7048809B2

  • Etchant composition, and methods of patterning conductive layer and manufacturing flat panel display device using the same

    US8052889B2

  • Na2Fe(SO4)2 / C electrode material jointly prepared by graphene and / or acetylene black, preparation method thereof and prepared battery

    CN110336021A