A catalyst for bio-oil hydrodeoxygenation and preparation method thereof
By using coal asphalt-based porous activated carbon support and metal ion-supported bimetallic catalysts, the problems of low activity and high cost of bio-oil hydrodeoxygenation catalysts are solved, and efficient bio-oil hydrodeoxygenation is achieved, and the thermal stability of bio-oil is improved. and calorific value, and have good chemical stability and cost advantages.
Patent Information
- Application Number
- CN202410428344.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-10
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-04-10
AI Technical Summary
The existing bio-oil hydrodeoxygenation catalyst has low activity, poor stability and high cost, making it difficult to effectively improve the thermal stability and calorific value of bio-oil.
Using coal asphalt-based porous activated carbon as a support, a bimetallic catalyst with high specific surface area and chemical stability was prepared through high temperature carbonization and metal ion loading, and used for the hydrodeoxygenation reaction of bio-oil.
The high catalytic activity and low cost hydrodeoxygenation of bio-oils has been achieved, which improves the thermal stability and calorific value of bio-oils. The catalyst has strong chemical stability in acidic and alkaline media, supporting the recycling and reuse of catalysts. .
Smart Images

Figure BDA0004784835960000081 
Figure HDA0004784835970000011 
Figure HDA0004784835970000012
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biomass pyrolysis oil quality improvement, and particularly relates to a catalyst used for bio-oil hydrodeoxygenation and a preparation method thereof. Background Art
[0002] Considering the continuous depletion of traditional fossil energy and the increasingly serious environmental pollution, converting eco-friendly and sustainable biomass into high-quality fuels has become an increasingly urgent need for our society. However, the high oxygen content of biomass feedstocks usually leads to poor thermal stability, high corrosiveness and low calorific value of biomass-derived bio-oils. The key to upgrading bio-oil is deoxygenation, and the research on bio-oil deoxygenation technology has become increasingly extensive in recent years. Among the many deoxygenation pathways, hydrodeoxygenation (HDO) technology is considered to be an effective method due to its advantages such as high product calorific value, less coking and mild reaction conditions.
[0003] Based on the active phase, HDO catalysts can be divided into the following categories: (1) metal sulfides; (2) noble metals; (3) metal carbides, nitrides, and phosphides; and (4) non-noble metals. Metal sulfide catalysts such as MoS2, CoMoS2, and NiMoS2 were used relatively early. Although they showed satisfactory activity, they quickly deactivated in the presence of water. In addition, the resulfurization process is not only complicated to operate, but also pollutes the environment. Supported Pt, Pd, and Ru catalysts are excellent hydrogenation catalysts, but due to their weak oxygen affinity, they usually need to be combined with acidic sites to enhance their deoxygenation activity. Metal carbide, nitride, and phosphide catalysts have received increasing attention in recent years due to their catalytic behavior similar to that of noble metal catalysts. However, these materials face the same problems as metal sulfides in terms of deactivation and regeneration. Recently, non-noble metal Ni-based catalysts have shown great promise in replacing noble metals for hydrodeoxygenation reactions due to their low cost and strong H2 activation ability.
[0004] Chinese patent document CN113786851A discloses a hydrodeoxygenation catalyst and its preparation method and application, which includes attaching an active component precursor to a carbon-based mesoporous material in advance, then placing the carbon-based mesoporous material in a reactor, allowing it to be subjected to a reduction reaction treatment under a reducing gas atmosphere and a preset temperature, to obtain an active component attached to the carbon-based mesoporous material, and then maintaining a reducing gas atmosphere, subjecting the carbon-based mesoporous material to a self-heating cooling treatment, and after its temperature drops to room temperature, a hydrodeoxygenation catalyst is obtained. In the above-prepared catalyst, the carbon-based carrier is an organic reagent such as phenol and formaldehyde, which is formed by a thermal polymerization reaction, and mesopores are constructed by a template agent, but the catalyst preparation cost is high, the operation is complicated, and the pores are single.
[0005] Therefore, there is an urgent need to develop a method for preparing a bio-oil hydrodeoxygenation catalyst with high activity, stability and low price. Summary of the invention
[0006] In view of the shortcomings of the prior art, especially the low activity and poor stability of the current bio-oil hydrodeoxygenation catalyst and the high cost of the precious metal catalyst, the present invention provides a catalyst for bio-oil hydrodeoxygenation and a preparation method thereof. The present invention uses coal tar-based porous activated carbon as a carrier to load transition metals to synthesize the bio-oil hydrodeoxygenation catalyst, thereby solving the problems of poor thermal stability, high corrosiveness, low calorific value, etc. of bio-oil.
[0007] In order to achieve the above object, the present invention adopts the following technical solutions:
[0008] A method for preparing a catalyst for bio-oil hydrodeoxygenation comprises the following steps:
[0009] (1) mixing coal tar pitch, an activator and a heteroatom dopant and grinding them to obtain a mixture; carbonizing the obtained mixture at high temperature; then grinding, acid washing, water washing and drying to obtain a coal tar pitch-based porous activated carbon;
[0010] (2) placing the coal tar-based porous activated carbon obtained in step (1) in a solution containing metal ions for impregnation, followed by filtering, washing, drying, and calcining to obtain a catalyst precursor loaded with metal;
[0011] (3) reducing the metal-loaded catalyst precursor obtained in step (2) to obtain a catalyst for bio-oil hydrodeoxygenation.
[0012] Preferably according to the present invention, the activator in step (1) is potassium hydroxide; and the mass ratio of the activator to coal tar pitch is 3-8:1.
[0013] Preferably, according to the present invention, the heteroatom dopant in step (1) is melamine; and the mass ratio of the heteroatom dopant to coal tar pitch is 1:3.5-5.
[0014] Preferably, according to the present invention, the temperature of the high temperature carbonization in step (1) is 600-1000°C, the time of the high temperature carbonization is 1-3h, the heating rate of the high temperature carbonization process is 5-10°C / min, and the high temperature carbonization is carried out under a nitrogen atmosphere.
[0015] Preferably, according to the present invention, the pickling step in step (1) is: the ground carbonized material is placed in a 1 mol / L hydrochloric acid aqueous solution and soaked for 10-15 hours, and then filtered; there is no specific requirement for the volume of the hydrochloric acid aqueous solution, which can completely immerse the ground carbonized material, and a slight excess can be used.
[0016] Preferably, according to the present invention, the water washing step in step (1) is: adding the solid obtained by acid washing into deionized water, soaking it at 50-60° C. for 10-12 hours, filtering it, and then washing the filtered solid with deionized water for 3-5 times; there is no specific requirement for the volume of deionized water used to soak the solid obtained by acid washing, and the solid obtained by acid washing can be completely immersed, and a slight excess can be used.
[0017] Preferably, according to the present invention, the drying in step (1) is performed at 70-90° C. for 10-12 hours.
[0018] According to the preferred embodiment of the present invention, the metal ion in step (2) is Ni 2+ and Fe 3+ A combination of Ni 2+ with Fe 3+ The molar ratio of is 0.3-5:1, and more preferably 2-4:1; the solution containing metal ions is obtained by dissolving metal salts of corresponding metals in ethanol aqueous solution, and the concentration of metal ions in the solution containing metal ions is 18-20mmol / L; the metal salts of corresponding metals are nitrates, sulfates, acetates or chlorides of corresponding metals, and the volume fraction of ethanol in the ethanol aqueous solution is 50%.
[0019] Preferably, according to the present invention, the volume ratio of the solution containing metal ions to the mass ratio of the coal tar pitch-based porous activated carbon in step (2) is 80-120 mL:1 g; the impregnation is carried out under stirring conditions, and the impregnation time is 5-7 h.
[0020] Preferably, in step (2), the washing is performed by washing with deionized water for 3-5 times; and the drying is performed at 50-60° C. for 10-15 hours.
[0021] Preferably, according to the present invention, the calcination temperature in step (2) is 300-400°C, and the calcination time is 5-7h; the calcination is carried out in a protective gas, the protective gas is argon or nitrogen, and the heating rate of the calcination process is 2-5°C / min.
[0022] Preferably, according to the present invention, the reduction in step (3) is carried out in a hydrogen atmosphere, the reduction temperature is 300-400°C, the reduction time is 3-5h, and the heating rate of the reduction process is 1-3°C / min.
[0023] The present invention also provides a catalyst for bio-oil hydrodeoxygenation, which is prepared by the above preparation method.
[0024] According to the present invention, the above-mentioned catalyst for bio-oil hydrodeoxygenation is used in catalyzing bio-oil hydrodeoxygenation.
[0025] The technical features and beneficial effects of the present invention are as follows:
[0026] 1. The present invention obtains a coal tar-based porous activated carbon carrier with a high specific surface area and a clear pore size distribution by high-temperature carbonization activation of coal tar, and then loads a specific proportion of metals to obtain a bimetallic catalyst used in bio-oil hydrodeoxygenation. The coal tar-based porous activated carbon carrier of the present invention has a large active surface area, is conducive to providing more active sites, has low cost, clear pore distribution, and has strong chemical stability in acidic and alkaline media. In addition, its preparation requires strict control of the ratio of coal tar, activator, and heteroatom dopant to obtain a catalyst with excellent catalytic performance. If the ratio of activator or heteroatom dopant to coal tar is too high or too low, the catalytic performance of the catalyst will be reduced.
[0027] 2. The entire preparation process of the present invention is simple, the preparation conditions are mild, no precious metals are involved, and the cost is relatively low.
[0028] 3. The catalyst prepared by the present invention has high catalytic activity. A specific proportion of metal combination is loaded on a specific carrier, and a hydrodeoxygenation reaction is carried out at a relatively low temperature to reduce the oxygen content and show a high alkane selectivity. After the reaction is completed, the catalyst is recovered and reused, and the catalyst does not contain precious metal components, which has a good cost advantage. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 The graphs are phenol conversion and cyclohexane selectivity under the catalysis of the catalysts obtained in Example 1 and Comparative Examples 1-2.
[0030] Figure 2 The conversion rates of different reaction substrates and the selectivity of cyclohexane under the catalysis of the catalyst prepared in Example 1 are shown.
[0031] Figure 3 The conversion rate of phenol and the selectivity of cyclohexane catalyzed by the catalyst prepared in Example 1 at different cycle numbers. DETAILED DESCRIPTION
[0032] The present invention proposes a method for preparing a bio-oil hydrodeoxygenation catalyst. In order to make the advantages and technical solutions of the present invention clearer and more specific, the present invention is further described below in conjunction with specific embodiments.
[0033] Example 1
[0034] A method for preparing a catalyst for bio-oil hydrodeoxygenation comprises the following steps:
[0035] (1) Weigh 1.2 g of coal tar, 0.3 g of melamine, and 4.8 g of potassium hydroxide into a mortar and grind thoroughly for 15 min to obtain a powdery mixture;
[0036] (2) placing the powdered mixture obtained in step (1) in a crucible, placing it in a tube furnace, raising the temperature to 800° C. at 5° C. / min in a nitrogen atmosphere, keeping the temperature at 800° C. for 2 h, and naturally cooling it to room temperature to obtain a carbonized material;
[0037] (3) The carbonized material obtained in step (2) was placed in a mortar and ground thoroughly, and the ground carbonized material was placed in a 1 mol / L hydrochloric acid aqueous solution and soaked for 12 h, filtered, and then the filtered solid was placed in deionized water, soaked at 60° C. for 12 h and then filtered, and the filtered solid was washed with deionized water three times, and finally the obtained solid was placed in an oven at 80° C. and dried for 12 h to obtain a coal tar-based porous activated carbon, which was named ACN;
[0038] (4) Dissolve 0.21 g Ni(NO3)2·6H2O and 0.1 g Fe(NO3)3·9H2O in 50 mL of 50% ethanol aqueous solution under magnetic stirring to obtain a solution containing metal ions; immerse 0.5 g coal tar-based porous activated carbon in the above solution containing metal ions and stir continuously for 6 h, then filter, wash the obtained solid with deionized water 3 times, and finally dry the washed solid in an oven at 50°C for 12 h; then place the dried product in a tubular furnace, heat it to 400°C at a heating rate of 3°C / min under argon atmosphere, and calcine it at 400°C for 6 h to obtain a catalyst precursor loaded with metal;
[0039] (5) The metal-loaded catalyst precursor is placed in a tubular furnace, heated to 400°C at a heating rate of 2°C / min in a hydrogen atmosphere, and reduced at 400°C for 4 h to obtain a catalyst loaded with metal nickel and iron, which is a catalyst used for bio-oil hydrodeoxygenation and is named Ni3-Fe1 / ACN.
[0040] Example 2
[0041] A method for preparing a catalyst for bio-oil hydrodeoxygenation is as described in Example 1, except that in step (4), 0.22 g Ni(NO3)2·6H2O and 0.077 g Fe(NO3)3·9H2O are dissolved in 50 mL of 50% ethanol aqueous solution, and the other conditions are the same as in Example 1. The obtained catalyst is named Ni4-Fe1 / ACN.
[0042] Example 3
[0043] A method for preparing a catalyst for bio-oil hydrodeoxygenation is as described in Example 1, except that in step (4), 0.095 g Ni(NO3)2·6H2O and 0.26 g Fe(NO3)3·9H2O are dissolved in 50 mL of 50% ethanol aqueous solution, and the other conditions are the same as in Example 1. The obtained catalyst is named Ni1-Fe2 / ACN.
[0044] Comparative Example 1
[0045] A method for preparing a catalyst for bio-oil hydrodeoxygenation is as described in Example 1, except that in step (4), 0.28 g of Ni(NO3)2·6H2O is dissolved in 50 mL of 50% ethanol aqueous solution, and the other conditions are the same as in Example 1. The obtained catalyst is named Ni / ACN.
[0046] Comparative Example 2
[0047] A method for preparing a catalyst for bio-oil hydrodeoxygenation is as described in Example 1, except that in step (4), 0.39 g of Fe(NO3)3·9H2O is dissolved in 50 mL of 50% ethanol aqueous solution, and the other conditions are the same as in Example 1. The obtained catalyst is named Fe / ACN.
[0048] Comparative Example 3
[0049] A method for preparing a catalyst for bio-oil hydrodeoxygenation is as described in Example 1, except that in step (1), 1.2 g of coal tar, 1.2 g of melamine, and 4.8 g of potassium hydroxide are weighed into a mortar and ground for 15 minutes to obtain a powdery mixture.
[0050] Comparative Example 4
[0051] A method for preparing a catalyst for bio-oil hydrodeoxygenation is as described in Example 1, except that in step (1), 1.2 g of coal tar, 0.3 g of melamine, and 3.2 g of potassium hydroxide are weighed into a mortar and fully ground for 15 minutes to obtain a powdery mixture.
[0052] Comparative Example 5
[0053] A method for preparing a catalyst for bio-oil hydrodeoxygenation comprises the following steps:
[0054] (1) Dissolve 0.21 g Ni(NO3)2·6H2O and 0.1 g Fe(NO3)3·9H2O in 50 mL of 50% ethanol aqueous solution under magnetic stirring to obtain a solution containing metal ions; immerse 0.5 g activated carbon in the above solution containing metal ions and stir continuously for 6 h, then filter, wash the obtained solid with deionized water 3 times, and finally dry the washed solid in an oven at 50°C for 12 h; then place the dried product in a tubular furnace, heat it to 400°C at a heating rate of 3°C / min under argon atmosphere, and calcine it at 400°C for 6 h to obtain a catalyst precursor loaded with metal;
[0055] (2) The metal-loaded catalyst precursor is placed in a tubular furnace, heated to 400°C at a heating rate of 2°C / min under a hydrogen atmosphere, and reduced at 400°C for 4 hours to obtain a catalyst loaded with metal nickel and iron, which is a catalyst used for bio-oil hydrodeoxygenation and is named Ni-Fe / C.
[0056] Test Example 1
[0057] The catalysts prepared in Examples 1-3 and Comparative Examples 1-5 were used for catalytic hydrodeoxygenation reaction, and the specific steps were as follows:
[0058] 24.5 g of n-dodecane, 0.5 g of phenol and 50 mg of the above-prepared catalyst were added to a 100 mL stainless steel reactor, the device was installed, the reactor was purged with 0.2 MPa of argon for 5 times to remove the air in the reactor, and then the temperature was raised from room temperature to 250 ° C at a rate of 10 ° C / min. When the target temperature was reached, the reactor was pressurized with 5 MPa of hydrogen, the speed was adjusted to 800 r / min, and the reaction was continued for 10 hours. After the reaction was completed, the reactor was cooled to ambient temperature. The product was analyzed by Agilent 8890 / 5977B gas chromatography-mass spectrometry, and the results are shown in Table 1.
[0059] Table 1 Phenol conversion and cyclohexane selectivity under different catalysts
[0060] catalyst Phenol conversion rate / % Cyclohexane selectivity / % Example 1 100 49.2 Example 2 100 44.9 Example 3 87.4 43.2 Comparative Example 1 100 8.1 Comparative Example 2 6.1 3.2 Comparative Example 3 84.5 39.8 Comparative Example 4 79.3 41.2 Comparative Example 5 78.5 42.3
[0061] It can be seen from Example 1 and Comparative Examples 1-2 that in the hydrodeoxygenation process, the prepared bimetallic catalyst has high catalytic activity, high phenol conversion rate and cyclohexane selectivity, while the cyclohexane selectivity of the catalyst loaded with single metal Ni is greatly reduced, and the phenol conversion rate and cyclohexane selectivity of the catalyst loaded with single metal Fe are greatly reduced.
[0062] Analysis of Example 1 and Comparative Example 3 shows that when the mass ratio of coal tar pitch to melamine is reduced from 4:1 to 1:1, the phenol conversion rate and the selectivity of cyclohexane decrease. This may be due to excessive nitrogen doping leading to blockage of active sites, reducing the effective surface area of the catalyst, and reducing the activity and selectivity of the catalyst.
[0063] Analysis of Example 1 and Comparative Example 4 shows that when the mass ratio of potassium hydroxide to coal tar pitch decreases from 4:1 to 8:3, the phenol conversion rate and the selectivity of cyclohexane decrease. This may be due to the small amount of potassium hydroxide as the activator, the uneven pore structure formed, and the limited active surface area, which are not conducive to the diffusion of substances and the reaction, resulting in a decrease in the reaction activity of the prepared catalyst.
[0064] Comparison of Example 1 and Comparative Example 5 shows that, compared with the supported bimetallic catalyst prepared using common activated carbon as a carrier, the bio-oil hydrodeoxygenation catalyst prepared in the present invention has better hydrodeoxygenation activity.
[0065] Test Example 2
[0066] The catalyst prepared in Example 1 was used to catalyze different reaction substrates for hydrodeoxygenation reaction, and the specific steps were as follows:
[0067] 24.5 g of n-dodecane, reaction substrate and 50 mg of the above-prepared catalyst were added to a 100 mL stainless steel reactor, the device was installed, the reactor was purged with 0.2 MPa of argon for 5 times to remove the air in the reactor, and then the temperature was raised from room temperature to 250 ° C at a rate of 10 ° C / min. When the target temperature was reached, the reactor was pressurized with 5 MPa of hydrogen, the speed was adjusted to 800 r / min, and the reaction was continued for 10 hours. After the reaction was completed, the reactor was cooled to ambient temperature. The product was analyzed by Agilent 8890 / 5977B gas chromatography-mass spectrometry. The reaction substrates used, the feed amount, the conversion rate of different reaction substrates and the selectivity of cyclohexane are shown in Table 2.
[0068] Table 2 Conversion rate of different reaction substrates and selectivity of cyclohexane
[0069] Reaction substrate Feeding amount / g Conversion rate / % Cyclohexane selectivity / % Cyclohexanol 0.53 55.7 96.6 Catechol 0.88 100 30.8 Guaiacol 0.65 100 42.1 p-Cresol 0.57 100 46.3 Eugenol 0.87 100 44.7
[0070] It can be seen from the above that the catalyst of the present invention has a wide range of substrates, the prepared bimetallic catalyst has high catalytic activity, and the conversion rate and selectivity of the reactants are relatively high.
[0071] Test Example 3
[0072] The bimetallic catalyst prepared in Example 1 can be separated from the reaction solution by applying an external magnetic field. After each cycle, it is washed twice with 5 mL of ethanol and then used in the next cycle experiment.
[0073] Table 3 Conversion rate of phenol and selectivity of cyclohexane under different cycle numbers
[0074]
[0075] A slight decrease in cyclohexane selectivity was found during the four-cycle evaluation. The decrease in cyclohexane selectivity may be attributed to the slight deactivation of the catalyst and a small amount of catalyst loss during the cycle.
[0076] The preparation of the bio-oil hydrodeoxygenation catalyst of the present invention has easy-to-obtain raw materials and simple operation. The coal tar pitch-based porous activated carbon carrier with high specific surface area and clear pore size distribution is prepared by high-temperature carbonization activation of coal tar pitch, and then metal loading is performed to prepare the catalyst. In the hydrodeoxygenation process, the prepared bimetallic catalyst has high catalytic activity, and its reactant conversion rate and selectivity are both high. After the reaction is completed, the catalyst is recycled and reused, and the catalyst does not contain precious metal components, which has good cost advantages.
[0077] Parts not described in the present invention can be implemented by referring to the existing technology.
[0078] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable ordinary technicians in the field to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a catalyst for bio-oil hydrodeoxygenation, characterized in that: The steps include: (1) coal tar pitch, an activator and a heteroatom dopant are mixed and ground to obtain a mixture; the obtained mixture is subjected to high temperature carbonization; and then ground, pickled, washed with water and dried to obtain a coal tar pitch-based porous activated carbon; the activator is potassium hydroxide; the mass ratio of the activator to the coal tar pitch is 3-8:1; the heteroatom dopant is melamine; the mass ratio of the heteroatom dopant to the coal tar pitch is 1:3.5-5; (2) placing the coal tar-based porous activated carbon obtained in step (1) in a solution containing metal ions for impregnation, followed by filtering, washing, drying, and calcining to obtain a catalyst precursor loaded with metal; the metal ions are Ni 2+ and Fe 3+ A combination of Ni 2+ with Fe 3+ The molar ratio is 0.3-5:1; the concentration of metal ions in the solution containing metal ions is 18-20mmol / L, and the volume ratio of the solution containing metal ions to the mass ratio of the coal tar pitch-based porous activated carbon is 80-120mL:1g; (3) Reducing the metal-loaded catalyst precursor obtained in step (2) to obtain a catalyst for bio-oil hydrodeoxygenation.
2. The method for preparing a catalyst for bio-oil hydrodeoxygenation according to claim 1, characterized in that: The temperature of the high-temperature carbonization in step (1) is 600-1000°C, the time of the high-temperature carbonization is 1-3h, the heating rate of the high-temperature carbonization process is 5-10°C / min, and the high-temperature carbonization is carried out under a nitrogen atmosphere.
3. The method for preparing a catalyst for bio-oil hydrodeoxygenation according to claim 1, characterized in that: The pickling step in step (1) is as follows: the ground carbonized material is placed in a 1 mol / L hydrochloric acid aqueous solution and soaked for 10-15 hours, and then filtered; The water washing step comprises: adding the solid obtained by acid washing into deionized water, soaking it at 50-60° C. for 10-12 hours, filtering it, and then washing the filtered solid with deionized water for 3-5 times; The drying is carried out at 70-90° C. for 10-12 hours.
4. The method for preparing a catalyst for bio-oil hydrodeoxygenation according to claim 1, characterized in that: Step (2) Ni 2+ with Fe 3+ The molar ratio is 2-4:1; the solution containing metal ions is obtained by dissolving a metal salt of the corresponding metal in an ethanol aqueous solution, the metal salt of the corresponding metal is a nitrate, sulfate, acetate or chloride of the corresponding metal, and the volume fraction of ethanol in the ethanol aqueous solution is 50%.
5. The method for preparing a catalyst for bio-oil hydrodeoxygenation according to claim 1, characterized in that: The immersion in step (2) is carried out under stirring conditions for 5-7 hours; The washing comprises washing with deionized water for 3-5 times; and the drying comprises drying at 50-60° C. for 10-15 hours.
6. The method for preparing a catalyst for bio-oil hydrodeoxygenation according to claim 1, characterized in that: The calcination temperature in step (2) is 300-400°C, and the calcination time is 5-7h; the calcination is carried out in a protective gas, the protective gas is argon or nitrogen, and the heating rate of the calcination process is 2-5°C / min.
7. The method for preparing a catalyst for bio-oil hydrodeoxygenation according to claim 1, characterized in that: The reduction in step (3) is carried out in a hydrogen atmosphere, the reduction temperature is 300-400°C, the reduction time is 3-5h, and the heating rate of the reduction process is 1-3°C / min.
8. A catalyst for bio-oil hydrodeoxygenation, characterized in that: The preparation method according to claim 1 is used for preparation.
9. Use of the catalyst for bio-oil hydrodeoxygenation according to claim 8 in catalyzing bio-oil hydrodeoxygenation.
Citation Information
Cited By
Hydrophobic hydrodeoxygenation catalyst and preparation method thereof
CN120605760A