A membrane electrode catalyzing two-electron oxygen reduction reaction and its preparation method and application
By using amorphous titanium dioxide-coated titanium carbonitride and noble metal-doped titanium dioxide nanocomposites as catalysts in the membrane electrode, combined with a gas diffusion layer of hydrophobic carbon paper and titanium fiber felt, the low efficiency of the existing membrane electrode and the amount of precious metals are solved. High-efficiency catalytic two-electron oxygen reduction reaction is achieved, reducing production costs and improving hydrogen peroxide production efficiency.
Patent Information
- Application Number
- CN202410732536.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-07
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-06-07
AI Technical Summary
The existing membrane electrode used to synthesize hydrogen peroxide by electrochemical oxygen reduction method has low efficiency, high energy consumption, high dosage of precious metals, and insufficient catalytic activity, making it difficult to meet the needs of sustainable and green production.
Amorphous titanium dioxide-coated titanium carbonitride nanocomposites are used as cathode catalysts and precious metal-doped titanium dioxide nanocomposites are used as anode catalysts. Through the design of membrane electrodes with a stacked structure, the amount of precious metals is reduced and the catalytic activity is improved, combining hydrophobic carbon paper and titanium The gas diffusion layer of the fiber mat optimizes the proton exchange membrane to achieve efficient catalysis of the two-electron oxygen reduction reaction.
It significantly reduces the usage of precious metals, improves catalytic activity and electrochemical performance, reduces production costs, extends the service life of membrane electrodes, and improves the production efficiency and stability of hydrogen peroxide.
Smart Images

Figure CN118315632B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fuel cells, and in particular to a membrane electrode for catalyzing a two-electron oxygen reduction reaction, and a preparation method and application thereof. Background Art
[0002] Hydrogen peroxide (H2O2) is a strong oxidant that can replace oxygen and is used as an oxidant in some special fuel cells (such as metal semi-fuel cells, direct sodium borohydride-H2O2 fuel cells, direct alcohol-H2O2 fuel cells, etc.). This type of battery has the characteristics of simple structure, high energy density and long storage life. In addition, hydrogen peroxide is also an energy storage material that can undergo electro-oxidation reactions, so it can be used as a fuel (electron donor) for fuel cells. Compared with other fuels used in fuel cell systems, hydrogen peroxide has high energy density, low energy consumption, low price, and does not produce byproducts that are harmful to the ecological environment. Based on the fact that hydrogen peroxide can be used as both a fuel and an oxidant, researchers have proposed a new type of fuel cell - a direct hydrogen peroxide fuel cell. Due to the all-liquid characteristics of the direct hydrogen peroxide fuel cell, it can be used in working environments without oxygen such as the deep sea and space.
[0003] Hydrogen peroxide will maintain a steady market growth trajectory over the next decade, however, economical and large-scale production of hydrogen peroxide can only be achieved through the anthraquinone process, which involves cyclic hydrogenation and oxidation of alkylanthraquinone precursors, palladium catalysts, organic solvents and liquid-liquid extraction, requiring large energy inputs, and also produces waste chemicals that need to be properly treated or recycled. Due to these difficulties and the importance of hydrogen peroxide in the chemical industry and water treatment, research on sustainable and green methods for the production of hydrogen peroxide remains very active. One of these methods is the reduction of O2 to hydrogen peroxide through an electrochemical process. The electroreduction of O2 to produce hydrogen peroxide can be carried out in portable devices, resulting in on-site production at water treatment facilities. Therefore, the high cost and high risk of transporting highly concentrated hydrogen peroxide solutions (e.g., 30 wt.%) to remote areas can be avoided.
[0004] The cathode materials traditionally used in the electrochemical oxygen reduction method for synthesizing hydrogen peroxide are generally graphite gas diffusion electrodes and porous graphite electrodes. Due to the poor mass transfer effect of O2 and low current efficiency, the rate of hydrogen peroxide production is not high. At the same time, due to the large internal resistance of the reactor, the energy consumption is large. Membrane electrodes are mainly used as the core components of fuel cells. This type of electrode generally includes an anode and a cathode on both sides of the membrane. Due to its high efficiency, low energy consumption, low catalyst dosage and flexible operation, it has been favored by many researchers in recent years and has good application potential in the field of electrochemical oxygen reduction method for synthesizing hydrogen peroxide. However, the existing membrane electrodes for synthesizing hydrogen peroxide use a high amount of precious metals and the catalytic activity needs to be improved. Summary of the invention
[0005] The object of the present invention is to provide a membrane electrode for catalyzing a two-electron oxygen reduction reaction, and a preparation method and application thereof. The membrane electrode can reduce the amount of precious metals used and has high catalytic activity.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a membrane electrode for catalyzing a two-electron oxygen reduction reaction, comprising a cathode gas diffusion layer, a cathode catalyst layer, a proton exchange membrane, an anode catalyst layer and an anode gas diffusion layer which are stacked in sequence; the cathode catalyst in the cathode catalyst layer is an amorphous titanium dioxide-coated titanium carbonitride nanocomposite material; the anode catalyst in the anode catalyst layer is a noble metal-doped titanium dioxide nanocomposite material.
[0008] Preferably, the cathode gas diffusion layer is a hydrophobic carbon paper, the contact angle of the hydrophobic carbon paper is 120-150°, and the porosity is 60-80%.
[0009] Preferably, the preparation method of the cathode catalyst comprises the following steps: mixing titanium carbonitride with an acid solution, performing acid treatment, mixing the obtained acid-treated titanium carbonitride, an amorphous titanium dioxide precursor solution and water, and sequentially drying and grinding the obtained colloid, and then performing heat treatment to obtain an amorphous titanium dioxide-coated titanium carbonitride nanocomposite material;
[0010] The components of the amorphous titanium dioxide precursor solution include an alcohol solvent, a titanium source, sodium dodecyl sulfate and glacial acetic acid.
[0011] Preferably, the noble metal includes iridium, ruthenium or platinum;
[0012] The method for preparing the anode catalyst comprises the following steps:
[0013] A noble metal salt aqueous solution, an acid solution and titanium tetrachloride are mixed and heat treated to obtain a noble metal-doped titanium dioxide nanocomposite material;
[0014] The heat treatment temperature is 200-250° C. and the time is 6-10 h.
[0015] Preferably, the proton exchange membrane is a perfluorosulfonic acid proton membrane with a thickness of 50~200μm; the material used for the anode gas diffusion layer is titanium fiber felt, the thickness of the titanium fiber felt is 0.25~0.40mm, the porosity is 50~70%, and the diameter of the titanium fiber in the titanium fiber felt is 30~60μm.
[0016] The present invention provides a method for preparing a membrane electrode for catalyzing a two-electron oxygen reduction reaction according to the above technical solution, comprising the following steps:
[0017] Mixing a cathode catalyst, a first mixed solvent and a first Nafion solution, coating the obtained cathode catalyst slurry on a transfer substrate, and drying to obtain a cathode catalyst layer;
[0018] The anode catalyst, the second mixed solvent and the second Nafion solution are mixed, and the obtained anode catalyst slurry is coated on one side of the proton exchange membrane, and dried to obtain an anode catalyst layer;
[0019] After removing the transfer matrix on the cathode catalyst layer, the cathode catalyst layer is bonded to the other side of the proton exchange membrane with the anode catalyst layer by hot pressing, the cathode gas diffusion layer is bonded to the cathode catalyst layer side, and the anode gas diffusion layer is bonded to the anode catalyst layer side to obtain a membrane electrode that catalyzes a two-electron oxygen reduction reaction.
[0020] Preferably, the mass ratio of the cathode catalyst to the Nafion in the first Nafion solution is 1:(1-2); the loading amount of the cathode catalyst on the transfer substrate is 0.05-1.5 mg / cm 2 ; The mass ratio of the anode catalyst to the Nafion in the second Nafion solution is 1:(3~14); The loading amount of the anode catalyst on the proton exchange membrane is 0.25~0.7 mg / cm 2 .
[0021] Preferably, the hot pressing temperature is 100-170° C., the pressure is 0-10 Mpa, and the pressing time is 60-240 s.
[0022] The present invention provides the membrane electrode for catalyzing the two-electron oxygen reduction reaction described in the above technical solution or the use of the membrane electrode for catalyzing the two-electron oxygen reduction reaction prepared by the preparation method described in the above technical solution in the two-electron oxygen reduction reaction.
[0023] Preferably, the application method comprises: constructing an electrochemical reaction system by combining a membrane electrode with a neutral electrolyte or an alkaline electrolyte, connecting the membrane electrode with a direct current power supply, and catalyzing oxygen reduction to obtain hydrogen peroxide.
[0024] The cathode and anode catalysts used in the membrane electrode provided by the present invention are both nanocomposite materials with large specific surface area and high catalytic activity. Compared with the traditional membrane electrode, the amount of precious metals used can be reduced and the cost is low; the cathode and anode catalyst layers have oxidation resistance and corrosion resistance, and are not easy to agglomerate and fall off. The cathode in the membrane electrode of the present invention is amorphous titanium dioxide coated titanium carbonitride, which does not contain precious metal materials, and the anode is precious metal doped titanium dioxide. The total amount of precious metals used in the cathode and anode catalyst layers is 0.001~0.02mg / cm 2Compared with the traditional membrane electrode (the traditional fuel cell membrane electrode uses platinum-carbon catalysts for both the anode and cathode, the anode of the traditional water electrolysis hydrogen production membrane electrode is iridium, the cathode is platinum-carbon, and the total amount of precious metals used in the anode and cathode catalyst layers is 0.3~4.0 mg / cm 2 (relative to membrane electrode)), therefore, the present invention can significantly reduce the usage of precious metals.
[0025] The present invention provides a method for preparing the membrane electrode. Compared with the ultrasonic spraying method, the present invention adopts a semi-CCM method to prepare the membrane electrode, the anode adopts a coating method, and the cathode adopts a transfer method. The process is simple, the preparation time is short, the production efficiency is high, and it is suitable for laboratory level as well as large-scale batch production.
[0026] The cathode catalyst used in the membrane electrode provided by the present invention is amorphous titanium dioxide-coated titanium carbonitride, which is suitable for producing hydrogen peroxide by two-electron oxygen reduction in neutral and alkaline environments, has the ability to efficiently produce hydrogen peroxide, and has excellent electrochemical performance and stability; further, due to the appropriate ratio of the catalyst slurry, the membrane electrode catalytic layer will not fall off during use of the membrane electrode assembly, has a long service life, and has excellent hydrogen peroxide production performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The structure diagram of the membrane electrode of the present invention comprises a cathode catalyst layer 2, a cathode gas diffusion layer 3, an anode catalyst layer 4, an anode gas diffusion layer 5 and a proton exchange membrane 1; the cathode catalyst layer 2 is adhered to the other side of the proton exchange membrane 1 with the anode catalyst layer 4, the cathode gas diffusion layer 3 is attached to the cathode catalyst layer side, and the anode diffusion layer 5 is attached to the anode catalyst layer side;
[0028] Figure 2 It is a schematic diagram of the principle of producing hydrogen peroxide by a membrane electrode catalyzing a two-electron oxygen reduction reaction according to the present invention;
[0029] Figure 3 30% PTFE hydrophobic carbon paper obtained by hydrophobic treatment in Example 1;
[0030] Figure 4 This is a data graph of the membrane electrode prepared in Example 1 producing hydrogen peroxide in a 0.1M sodium sulfate electrolyte;
[0031] Figure 5 This is a data graph showing the concentration of hydrogen peroxide generated by the membrane electrode prepared in Example 2 in a 0.1 M sodium sulfate electrolyte at different times. DETAILED DESCRIPTION
[0032] like Figure 1As shown, the present invention provides a membrane electrode for catalyzing a two-electron oxygen reduction reaction, comprising a cathode gas diffusion layer, a cathode catalyst layer, a proton exchange membrane, an anode catalyst layer and an anode gas diffusion layer stacked in sequence; the cathode catalyst in the cathode catalyst layer is an amorphous titanium dioxide-coated titanium carbonitride nanocomposite material; the anode catalyst in the anode catalyst layer is a precious metal-doped titanium dioxide nanocomposite material.
[0033] In the present invention, unless otherwise specified, the required reagents are commercially available products well known in the art.
[0034] The membrane electrode for catalyzing the two-electron oxygen reduction reaction provided by the present invention comprises a cathode gas diffusion layer; the cathode gas diffusion layer is preferably hydrophobic carbon paper, the contact angle of the hydrophobic carbon paper is preferably 120-150°, more preferably 148.1°, and the porosity is preferably 60-80%.
[0035] In the present invention, the preparation method of the hydrophobic carbon paper is preferably: placing the conductive raw carbon paper in acetone and boiling it for 10 to 20 minutes to remove the residual oil and impurities on the surface of the carbon paper, and drying to remove the acetone solution adsorbed on the surface of the carbon paper; immersing the treated carbon paper in a 20 to 60 wt.% PTFE solution for 10 seconds and then taking it out, repeating the immersion process twice, taking it out and drying it at room temperature, placing it in a muffle furnace and first drying it at 50 to 70°C (more preferably 60°C) for 3 hours, and then sintering it at 370 to 430°C (more preferably 380°C) for 10 to 30 minutes, and then placing it in anhydrous ethanol for ultrasonic treatment for 0.3 to 1 hour (more preferably 0.5 hours), washing the obtained carbon paper with deionized water 3 times, and drying it to obtain a hydrophobic carbon paper with a hydrophobicity of 10 to 30%.
[0036] The membrane electrode for catalyzing two-electron oxygen reduction reaction provided by the present invention comprises a cathode catalyst layer; the cathode catalyst in the cathode catalyst layer is an amorphous titanium dioxide-coated titanium carbonitride nanocomposite material.
[0037] In the present invention, the preparation method of the cathode catalyst preferably includes the following steps: mixing titanium carbonitride with an acid solution, performing acid treatment, mixing the obtained acid-treated titanium carbonitride, an amorphous titanium dioxide precursor solution and water, and successively drying and grinding the obtained colloid, and then performing heat treatment to obtain an amorphous titanium dioxide-coated titanium carbonitride nanocomposite material.
[0038] In the present invention, the titanium carbonitride is preferably of industrial grade, with a purity of preferably ≥ 99.9%; the specific surface area of the titanium carbonitride is preferably 50-85 m 2 / g, and the particle size is preferably 30~60nm.
[0039] In the present invention, the loading amount of amorphous titanium dioxide on the surface of titanium carbonitride is preferably 0.2-5 wt.%, more preferably 0.5-1.4 wt.%.
[0040] In the present invention, the titanium carbonitride is preferably first ultrasonically treated with acetone or anhydrous ethanol for 10 to 30 minutes, and then washed with deionized water for 3 to 6 times; the acid solution preferably includes hydrochloric acid; the concentration of the hydrochloric acid is preferably 37wt%; the dosage ratio of the titanium carbonitride to the acid solution is preferably (0.5 to 1.0) g:40 mL, more preferably (0.6 to 0.9) g:40 mL, and further preferably (0.7 to 0.8) g:40 mL; in the present invention, the titanium carbonitride is preferably mixed with the acid solution and then ultrasonicated for 5 to 30 minutes, more preferably 10 to 20 minutes.
[0041] In the present invention, the acid treatment is preferably carried out under Ar or mixed atmosphere conditions; the mixed atmosphere is preferably 10% (volume percentage) H2 / Ar, the temperature of the acid treatment is preferably 30~55°C, more preferably 35~50°C, further preferably 40~45°C; the time is preferably 0.5~2h, more preferably 1~1.5h.
[0042] After the acid treatment, the present invention preferably filters and washes the obtained product mixture with deionized water until it is neutral, then vacuum dries it at 50° C. for 2 to 4 hours, and grinds the obtained product in a ball mill to obtain acid-treated titanium carbonitride. The present invention has no special restrictions on the process of filtering, washing and grinding, and can be carried out according to the process well known in the art.
[0043] In the present invention, the components of the amorphous titanium dioxide precursor solution preferably include an alcohol solvent, a titanium source, sodium dodecyl sulfate and glacial acetic acid; the alcohol solvent is preferably anhydrous ethanol; the titanium source is preferably tetrabutyl titanate; the dosage ratio of the sodium dodecyl sulfate, the alcohol solvent, the titanium source and the glacial acetic acid is preferably (10~20) mg:(2~4) mL:(1~2) mL:(0.6~1.3) mL, and more preferably (15~20) mg:(2~4) mL:(1.2~1.5) mL:(0.6~1.0) mL.
[0044] In the present invention, the method for preparing the amorphous titanium dioxide precursor solution is preferably to add a titanium source and sodium dodecyl sulfate to an alcohol solvent under ultrasonic stirring at 25-30° C., and then add glacial acetic acid to obtain the amorphous titanium dioxide precursor solution.
[0045] In the present invention, the usage ratio of the amorphous titanium dioxide precursor solution to the acid-treated titanium carbonitride is preferably (0.02-0.55) mL:0.8 g, and more preferably (0.1-0.3) mL:0.8 g.
[0046] The present invention preferably mixes the acid-treated titanium carbonitride with the amorphous titanium dioxide precursor solution, adds water to the obtained mixed system, stirs for 2 to 4 hours to form a colloid, and then dries in a 50° C. vacuum oven for 12 to 24 hours. After grinding, the obtained mixture is transferred to a crucible for heat treatment to obtain an amorphous titanium dioxide-coated titanium carbonitride nanocomposite material. The present invention has no special restrictions on the stirring and grinding, and can be carried out according to the process well known in the art.
[0047] In the present invention, the heat treatment is preferably carried out in an oxygen atmosphere or an air atmosphere; the temperature of the heat treatment is preferably 80-160°C, more preferably 85-120°C, and further preferably 90°C; the time is preferably 1-2h, and more preferably 1.5h.
[0048] The membrane electrode for catalyzing a two-electron oxygen reduction reaction provided by the present invention comprises a proton exchange membrane; the proton exchange membrane is preferably a perfluorosulfonic acid proton membrane, and the thickness is preferably 50-200 μm.
[0049] The membrane electrode for catalyzing two-electron oxygen reduction reaction provided by the present invention comprises an anode catalyst layer, wherein the anode catalyst in the anode catalyst layer is a precious metal-doped titanium dioxide nanocomposite material; the precious metal preferably comprises iridium, ruthenium or platinum.
[0050] In the present invention, the method for preparing the anode catalyst preferably comprises the following steps:
[0051] A noble metal salt aqueous solution, an acid solution and titanium tetrachloride are mixed and heat treated to obtain a noble metal-doped titanium dioxide nanocomposite material.
[0052] The present invention preferably adds HCl solution to the precious metal salt aqueous solution to adjust the pH value, and then adds titanium tetrachloride to the resulting solution; the precious metal salt in the precious metal salt aqueous solution is preferably iridium chloride, hydrated ruthenium trichloride or hexahydrate chloroplatinic acid; the molar percentage of the precious metal salt aqueous solution is preferably 0.5~2.5 mol%, more preferably 1.0~2.0 mol%, and further preferably 1.5 mol%; the acid solution is preferably HCl solution. The present invention uses an acid solution to adjust the solution pH value to 1~2, more preferably 1.5; the present invention has no special limitation on the concentration of the HCl solution, as long as it can meet the above pH requirements.
[0053] In the present invention, the heat treatment is preferably carried out in a high pressure reactor; the temperature of the heat treatment is preferably 200-250° C., more preferably 220-240° C.; the time is preferably 6-10 h, more preferably 7-8 h.
[0054] After the heat treatment is completed, the mixture is cooled to room temperature, the obtained suspension is washed with deionized water through a centrifuge, and the obtained product is dried at 60-80° C. to obtain a precious metal-doped titanium dioxide nanocomposite material. The present invention has no particular limitation on the time for the cooling, washing and drying, and the steps can be performed according to the process known in the art.
[0055] The membrane electrode for catalyzing the two-electron oxygen reduction reaction provided by the present invention includes an anode gas diffusion layer; the material used for the anode gas diffusion layer is preferably titanium fiber felt, the thickness of the titanium fiber felt is preferably 0.25~0.40mm, the porosity is preferably 50~70%, and the diameter of the titanium fiber in the titanium fiber felt is preferably 30~60μm.
[0056] The titanium fiber felt of the present invention is preferably pretreated before use. The pretreatment is preferably to immerse the titanium fiber felt in anhydrous ethanol and perform ultrasonic treatment for 0.3 to 1 h (more preferably 0.5 h), clean the anhydrous ethanol with deionized water, and dry it.
[0057] The present invention has no special limitation on the thickness of each layer of the membrane electrode, which can be adjusted according to actual preparation requirements.
[0058] The present invention provides a method for preparing a membrane electrode for catalyzing a two-electron oxygen reduction reaction according to the above technical solution, comprising the following steps:
[0059] Mixing a cathode catalyst, a first mixed solvent and a first Nafion solution, coating the obtained cathode catalyst slurry on a transfer substrate, and drying to obtain a cathode catalyst layer;
[0060] The anode catalyst, the second mixed solvent and the second Nafion solution are mixed, and the obtained anode catalyst slurry is coated on one side of the proton exchange membrane, and dried to obtain an anode catalyst layer;
[0061] After removing the transfer matrix on the cathode catalyst layer, the cathode catalyst layer is bonded to the other side of the proton exchange membrane with the anode catalyst layer by hot pressing, the cathode gas diffusion layer is bonded to the cathode catalyst layer side, and the anode gas diffusion layer is bonded to the anode catalyst layer side to obtain a membrane electrode.
[0062] The present invention mixes a cathode catalyst, a first mixed solvent and a first Nafion solution, and coats the obtained cathode catalyst slurry on a transfer substrate, and dries the mixture to obtain a cathode catalyst layer.
[0063] In the present invention, the cathode catalyst, the first mixed solvent and the first Nafion solution are preferably mixed by ultrasonic mixing; the temperature of the ultrasonic mixing is preferably 20°C; the first mixed solvent is preferably water and isopropanol; the mass ratio of water to isopropanol is preferably (3~3.5):1; the mass ratio of the first mixed solvent to the cathode catalyst is preferably 4:3~2.5:1, more preferably 2.25:1; the concentration of the first Nafion solution is preferably 10 wt.%; the mass ratio of the cathode catalyst to Nafion in the first Nafion solution is preferably 1:(1~2), more preferably 1:(1~1.75).
[0064] In the present invention, the loading amount of the cathode catalyst on the transfer substrate is preferably 0.05-1.5 mg / cm 2 , more preferably 0.1~1.2 mg / cm 2 , more preferably 0.35~0.83 mg / cm 2 .
[0065] In the present invention, the transfer substrate is preferably a polyimide film or a Teflon film; the present invention has no special limitation on the source of the transfer substrate, and any commercially available product with a source well known in the art may be used.
[0066] In the present invention, the drying temperature is preferably 30-70° C., more preferably 50-60° C. The present invention has no special limitation on the coating, and the above-mentioned loading requirement can be achieved according to the process well known in the art.
[0067] The present invention mixes an anode catalyst, a second mixed solvent and a second Nafion solution, and applies the obtained anode catalyst slurry on one side of a proton exchange membrane, and dries the mixture to obtain an anode catalyst layer.
[0068] In the present invention, the anode catalyst, the second mixed solvent and the second Nafion solution are preferably mixed by ultrasonic mixing; the temperature of the ultrasonic mixing is preferably 20°C; the present invention has no special limitation on the mixing time, which can be adjusted according to actual needs; the second mixed solvent is preferably water and isopropanol, and the mass ratio of water to isopropanol is preferably (8~11):1, more preferably 10.66:1; the mass ratio of the second mixed solvent to the anode catalyst is preferably (3~12):1, more preferably 11.66:1, and the concentration of the second Nafion solution is preferably 8~15 wt.%, more preferably 10~12wt.%; the mass ratio of the anode catalyst to Nafion in the second Nafion solution is preferably 1:(3~14), more preferably 1:(2.66~13.33).
[0069] In the present invention, the loading amount of the anode catalyst on the proton exchange membrane is preferably 0.25-0.7 mg / cm 2 , more preferably 0.3~0.6 mg / cm 2 , more preferably 0.5 mg / cm 2 The present invention preferably uses a coating machine to scrape the anode catalyst slurry onto the proton exchange membrane, and the loading amount of the anode catalyst is determined by weighing the proton exchange membrane before and after coating, so that the loading amount reaches the above requirements. The present invention has no special limitation on the coating, and the above loading amount can be achieved according to the process well known in the art.
[0070] After obtaining the cathode catalyst layer and the anode catalyst layer, the present invention removes the transfer matrix on the cathode catalyst layer, and then uses a hot pressing method to adhere the cathode catalyst layer to the other side of the proton exchange membrane with the anode catalyst layer, adhere the cathode gas diffusion layer to the cathode catalyst layer side, and adhere the anode gas diffusion layer to the anode catalyst layer side to obtain a membrane electrode.
[0071] The present invention has no particular limitation on the process of removing the transfer matrix on the cathode catalyst layer, and the process may be carried out according to methods well known in the art.
[0072] In the present invention, the temperature of the hot pressing is preferably 100-170°C, more preferably 130-160°C, and further preferably 135-150°C; the pressure is preferably 0-10 MPa, more preferably 2-8 MPa, and further preferably 3-5 MPa; the pressing time is preferably 60-240 s, more preferably 90-200 s, and further preferably 120-160 s.
[0073] The present invention provides the membrane electrode for catalyzing the two-electron oxygen reduction reaction described in the above technical solution or the use of the membrane electrode for catalyzing the two-electron oxygen reduction reaction prepared by the preparation method described in the above technical solution in the two-electron oxygen reduction reaction.
[0074] Figure 2 The schematic diagram is a principle diagram of the membrane electrode for catalyzing the two-electron oxygen reduction reaction to produce hydrogen peroxide in the present invention. Water on the anode catalyst layer loses two electrons and is oxidized into protons (hydrogen ions) and oxygen. The oxygen is discharged with the water flow, and the protons diffuse to the cathode catalyst layer through the proton exchange membrane. The oxygen introduced into the cathode catalyst layer reacts with the protons and two electrons to generate hydrogen peroxide liquid.
[0075] In the present invention, the application method preferably includes: constructing an electrochemical reaction system by combining a membrane electrode with a neutral electrolyte or an alkaline electrolyte, connecting the membrane electrode with a direct current power supply, and catalyzing oxygen reduction to obtain hydrogen peroxide.
[0076] The present invention has no special limitation on the neutral electrolyte or alkaline electrolyte, and any corresponding electrolyte in a fuel cell known in the art can be used.
[0077] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0078] Example 1
[0079] In this embodiment, the cathode catalyst layer 2 is prepared by amorphous titanium dioxide coated titanium carbonitride nanocomposite material, the cathode gas diffusion layer 3 is 30% PTFE hydrophobic carbon paper after hydrophobic treatment, the anode catalyst layer 4 is prepared by iridium doped titanium dioxide nanocomposite material, the anode gas diffusion layer 5 is a titanium fiber felt with a thickness of 0.25 mm, a porosity of 50-70%, and a titanium fiber diameter of 30-60 μm; the proton exchange membrane 1 is a commercially available Nafion non-reinforced membrane with a thickness of 183 μm;
[0080] Preparation of cathode gas diffusion layer: The conductive raw carbon paper was boiled in acetone for 20 min, dried, immersed in 60wt.% PTFE solution for 10 s and taken out, repeated twice, and blown dry at room temperature after being taken out; then placed in a muffle furnace and dried at 60℃ for 3h, and then sintered at 380℃ for 10 min. The treated carbon paper was ultrasonically treated in anhydrous ethanol for 0.5 h, washed with deionized water 3 times, and dried to obtain PTFE hydrophobic carbon paper with a hydrophobicity of 30%, a contact angle of 148.1°, and a porosity of 60~80%.
[0081] Preparation of anode gas diffusion layer: The titanium fiber felt was immersed in anhydrous ethanol and ultrasonicated for 0.5 h, then the anhydrous ethanol was cleaned with deionized water and dried.
[0082] Cathode catalyst layer preparation:
[0083] Weigh 0.8g of industrial grade nano titanium carbonitride particles (purity ≥ 99.9%; specific surface area 50~85m 2 / g, particle size of 30~60nm) in a beaker, add anhydrous ethanol and ultrasonicate for 10min, wash with deionized water 3 times after ultrasonication; mix the washed titanium carbonitride with 37wt% hydrochloric acid) according to the feed ratio of 0.8g:40mL, ultrasonicate for 10min, and then heat at 45℃ for 1h under Ar atmosphere; the obtained mixture is filtered and washed with deionized water until neutral, and then vacuum dried at 50℃ for 4h, and the obtained acid-treated nano-titanium carbonitride particles are ground in a ball mill to obtain acid-treated titanium carbonitride, which is stored in a vacuum glove box; under ultrasonic stirring at 25℃, add 2mL of anhydrous ethanol 1 mL of tetrabutyl titanate and 10 mg of sodium dodecyl sulfate were added, and then 0.6 mL of glacial acetic acid was added to obtain an amorphous titanium dioxide precursor solution; 0.3 mL of the amorphous titanium dioxide precursor solution was mixed with 0.8 g of acid-treated nano-titanium carbonitride particles, deionized water was added to the mixed system, and the mixture was stirred for 2 h. After forming a colloid, it was dried in a vacuum oven at 50°C for 12 h; after grinding, the resulting mixture was transferred to a crucible and heat-treated in air at 85°C for 2 h to obtain an amorphous titanium dioxide-coated titanium carbonitride nanocomposite material, wherein the loading amount of the amorphous titanium dioxide on the surface of the titanium carbonitride was 1.4 wt.%.
[0084] Take 20.75 mg of amorphous titanium dioxide-coated titanium carbonitride nanocomposite material, add 0.036 mL of deionized water and 0.045 mL of isopropanol, and then add 10 μL of 10 wt.% Nafion solution, that is, the mass ratio of cathode catalyst, Nafion, deionized water and isopropanol is 4:7:7:2, and mix them uniformly by constant temperature and ultrasonic at 20°C to obtain cathode catalyst slurry;
[0085] The cathode catalyst slurry was coated on the polyimide film to make the cathode catalyst loading reach 0.83 mg / cm 2 , and dried at 70°C to obtain a cathode catalytic layer.
[0086] Anode catalyst layer preparation:
[0087] Dissolving iridium chloride in deionized water to make its molar percentage be 1 mol%, adding HCl to the obtained iridium chloride solution to adjust the pH value of the solution to 1.5, then adding titanium tetrachloride to the obtained solution, transferring the obtained mixture to a high-pressure reactor, heating it in an oven at 200° C. for 8 h, and after the heating is completed, cooling it to room temperature, washing the obtained suspension with deionized water through a centrifuge, and drying the obtained product at 60° C. to obtain an anode catalyst, i.e., an iridium-doped titanium dioxide nanocomposite material;
[0088] 0.033 mL of deionized water and 0.041 mL of isopropanol were added to 12.5 mg of the iridium-doped titanium dioxide nanocomposite material, and then 12 μL of 10 wt.% Nafion solution was added, i.e., the mass ratio of the anode catalyst, Nafion, deionized water and isopropanol was 3:8:8:1, and the mixture was uniformly mixed by constant temperature ultrasound at 20° C. for 60 min to obtain an anode catalyst slurry.
[0089] The coating process was adopted to scrape the anode catalyst slurry onto the proton exchange membrane with a coating machine. The loading amount of the anode catalyst was determined by weighing the proton exchange membrane before and after coating, and the anode loading amount reached 0.5 mg / cm 2 , obtaining an anode catalyst layer;
[0090] The transfer matrix on the cathode catalyst layer was removed, and the prepared cathode catalyst layer was adhered to the other side of the proton exchange membrane with the anode catalyst layer at 135°C and 6 MPa for 120 s. The cathode gas diffusion layer was attached to the cathode catalyst layer side, and the anode diffusion layer was attached to the anode catalyst layer side to obtain a membrane electrode. The amount of precious metal used was 0.0075 mg / cm relative to the overall membrane electrode. 2 .
[0091] Figure 3 30% PTFE hydrophobic carbon paper obtained by hydrophobic treatment in Example 1 is shown in FIG. Figure 3 As shown, the contact angle of the hydrophobic carbon paper is 148.1°, indicating that the treated carbon paper has strong hydrophobicity, which is beneficial to control the amount of water and oxygen in the membrane electrode.
[0092] Example 2
[0093] Cathode catalyst layer preparation:
[0094] 37.5 mg of amorphous titanium dioxide-coated titanium carbonitride nanocomposite material was added to 0.038 mL of deionized water and 0.047 mL of isopropanol, and then 11.9 μL of 10 wt.% Nafion solution was added, i.e., the mass ratio of cathode catalyst, Nafion, deionized water and isopropanol was 3:3:3:1, and the mixture was uniformly mixed by constant temperature ultrasonication at 20°C to obtain cathode catalyst slurry;
[0095] The cathode catalyst slurry was coated on the polyimide film to make the cathode catalyst loading reach 1.5 mg / cm 2 , drying at 60°C to obtain a cathode catalyst layer;
[0096] Anode catalyst layer preparation:
[0097] 0.23 mL of deionized water and 0.24 mL of isopropanol were added to 17.5 mg of iridium-doped titanium dioxide nanocomposite material, and then 16.7 μL of 10 wt.% Nafion solution was added, i.e., the mass ratio of anode catalyst, Nafion, deionized water and isopropanol was 3:40:32:3, and the mixture was uniformly mixed by constant temperature ultrasonication at 20°C for 60 min to obtain an anode catalyst slurry;
[0098] The coating process was adopted to scrape the anode catalyst slurry onto the proton exchange membrane with a coating machine. The loading amount of the anode catalyst was determined by weighing the proton exchange membrane before and after coating, and the anode loading amount reached 0.7 mg / cm 2 , obtaining an anode catalyst layer;
[0099] The transfer matrix on the cathode catalyst layer was removed, and the prepared cathode catalyst layer was adhered to the other side of the proton exchange membrane with the anode catalyst layer at 130°C and 5 MPa for 90 s. The cathode gas diffusion layer was attached to the cathode catalyst layer side, and the anode diffusion layer was attached to the anode catalyst layer side to obtain a membrane electrode. The amount of precious metal used relative to the whole membrane electrode was 0.0105 mg / cm 2 ;
[0100] The rest is the same as in Example 1.
[0101] Application Example 1
[0102] The membrane electrode prepared in Example 1 was placed in a 0.1 M sodium sulfate electrolyte and subjected to a 20 mA / cm 2 Hydrogen peroxide was prepared by constant current; 10 mL of the reaction solution was taken out from the electrolytic cell every 40 min using a pipette, and the hydrogen peroxide yield was measured by UV-visible spectrophotometry at 405 nm. The results are shown in Figure 4 .
[0103] Figure 4 The data graph of the concentration of hydrogen peroxide produced by the membrane electrode prepared in Example 1 in 0.1M sodium sulfate electrolyte at different times; Figure 4 It can be seen that the concentration of hydrogen peroxide increases with time, and the concentration of hydrogen peroxide can reach 3000 mg / L at 240 minutes.
[0104] Application Example 2
[0105] The membrane electrode prepared in Example 2 was placed in a 0.1 M sodium sulfate electrolyte and subjected to a 20 mA / cm 2 Hydrogen peroxide was prepared by constant current; 10 mL of the reaction solution was taken out from the electrolytic cell every 40 min using a pipette, and the hydrogen peroxide yield was measured by UV-visible spectrophotometry at 405 nm. The results are shown in Figure 5 .
[0106] Figure 5 The data graph of the concentration of hydrogen peroxide produced by the membrane electrode prepared in Example 2 in 0.1M sodium sulfate electrolyte at different times; Figure 5 It can be seen that the concentration of hydrogen peroxide increases with time, and the concentration of hydrogen peroxide can reach 2300 mg / L at 240 minutes.
[0107] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A membrane electrode for catalyzing a two-electron oxygen reduction reaction, characterized in that: It comprises a cathode gas diffusion layer, a cathode catalyst layer, a proton exchange membrane, an anode catalyst layer and an anode gas diffusion layer which are stacked in sequence; the cathode catalyst in the cathode catalyst layer is a nano-composite material of amorphous titanium dioxide coated with titanium carbonitride; The anode catalyst in the anode catalyst layer is a precious metal-doped titanium dioxide nanocomposite material; The preparation method of the cathode catalyst comprises the following steps: mixing titanium carbonitride with an acid solution, performing acid treatment, mixing the obtained acid-treated titanium carbonitride, an amorphous titanium dioxide precursor solution and water, sequentially drying and grinding the obtained colloid, and then performing heat treatment to obtain an amorphous titanium dioxide-coated titanium carbonitride nanocomposite material; The components of the amorphous titanium dioxide precursor solution include an alcohol solvent, a titanium source, sodium dodecyl sulfate and glacial acetic acid; The amount ratio of the amorphous titanium dioxide precursor solution to the acid-treated titanium carbonitride is (0.02-0.55) mL:0.8 g; The loading amount of the amorphous titanium dioxide on the surface of titanium carbonitride is 0.2-5 wt.%.
2. The membrane electrode according to claim 1, characterized in that: The cathode gas diffusion layer is made of hydrophobic carbon paper, the contact angle of the hydrophobic carbon paper is 120-150°, and the porosity is 60-80%.
3. The membrane electrode according to claim 1, characterized in that: The noble metal includes iridium, ruthenium or platinum; The method for preparing the anode catalyst comprises the following steps: A noble metal salt aqueous solution, an acid solution and titanium tetrachloride are mixed and heat treated to obtain a noble metal-doped titanium dioxide nanocomposite material; The heat treatment is carried out at a temperature of 200 to 250° C. and for a time of 6 to 10 hours.
4. The membrane electrode according to claim 1, characterized in that: The proton exchange membrane is a perfluorosulfonic acid proton membrane with a thickness of 50 to 200 μm; the material used for the anode gas diffusion layer is titanium fiber felt, the titanium fiber felt has a thickness of 0.25 to 0.40 mm, a porosity of 50 to 70%, and a diameter of the titanium fiber in the titanium fiber felt of 30 to 60 μm.
5. The method for preparing a membrane electrode for catalyzing a two-electron oxygen reduction reaction according to any one of claims 1 to 4, characterized in that: The following steps are involved: Mixing a cathode catalyst, a first mixed solvent and a first Nafion solution, coating the obtained cathode catalyst slurry on a transfer substrate, and drying to obtain a cathode catalyst layer; The anode catalyst, the second mixed solvent and the second Nafion solution are mixed, and the obtained anode catalyst slurry is coated on one side of the proton exchange membrane, and dried to obtain an anode catalyst layer; After removing the transfer matrix on the cathode catalyst layer, the cathode catalyst layer is bonded to the other side of the proton exchange membrane with the anode catalyst layer by hot pressing, the cathode gas diffusion layer is bonded to the cathode catalyst layer side, and the anode gas diffusion layer is bonded to the anode catalyst layer side to obtain a membrane electrode that catalyzes a two-electron oxygen reduction reaction.
6. The preparation method according to claim 5, characterized in that: The mass ratio of the cathode catalyst to the Nafion in the first Nafion solution is 1:(1-2); the loading amount of the cathode catalyst on the transfer substrate is 0.05-1.5 mg / cm 2 ; The mass ratio of the anode catalyst to the Nafion in the second Nafion solution is 1:(3-14); the loading amount of the anode catalyst on the proton exchange membrane is 0.25-0.7 mg / cm 2 .
7. The preparation method according to claim 5, characterized in that: The temperature of the hot pressing is 100-170° C., the pressure is 0-10 MPa, and the pressing time is 60-240 seconds.
8. Use of the membrane electrode for catalyzing the two-electron oxygen reduction reaction according to any one of claims 1 to 4 or the membrane electrode for catalyzing the two-electron oxygen reduction reaction prepared by the preparation method according to any one of claims 5 to 7 in the two-electron oxygen reduction reaction.
9. The use according to claim 8, characterized in that: The application method comprises: constructing an electrochemical reaction system by combining a membrane electrode with a neutral electrolyte or an alkaline electrolyte, connecting the membrane electrode with a direct current power supply, and catalyzing oxygen reduction to obtain hydrogen peroxide.