A forging process for high temperature alloy
Through microwave preheating and powder spraying technology combined with solid solution treatment and nitriding annealing, the problem of strength and hardness unevenness in high-temperature alloy forging is solved, the overall performance and forging efficiency of the alloy are improved, and high-quality and efficient forging of high-temperature alloys are achieved .
Patent Information
- Application Number
- CN202410352479.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-26
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-03-26
AI Technical Summary
In the existing high-temperature alloy forging process, forgings are prone to uneven strength and hardness during the forging process, and hot die forging technology is subject to mold cost and heating time, resulting in forgings that are prone to cracking and cold die structure, affecting the quality and qualification of the alloy. Rate.
Microwave preheating combined with high-temperature electric furnace heating is used, and powder spraying is used to form the coating. Through solid solution treatment, regression re-aging, nitriding annealing and other processes, the precipitated phase and element distribution of the forgings are adjusted to improve material performance.
By improving the process, the strength, hardness uniformity and stress corrosion resistance of high-temperature alloys are improved, the tensile strength and yield strength of the alloys are enhanced, and the forging efficiency and finished product quality are improved.
Smart Images

Figure CN118321475B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a forging process of a high-temperature alloy. Background Art
[0002] High-temperature alloy is a kind of difficult-to-process material widely used in aerospace and other fields. Common high-temperature alloys are excellent in temperature bearing capacity, strength, and durability. However, while having excellent mechanical properties and temperature bearing capacity, the complex alloying ratio and high alloying will greatly increase the difficulty of hot working and forming, and put forward high requirements on forging and heat treatment processes. Therefore, choosing the right forging process for high-quality, efficient, and high-quality lean production has become the key to the development of high-temperature alloys.
[0003] In the existing high-temperature alloy forging process, the heating temperature before forging is generally high to compensate for the temperature drop of the forging during the transfer process; the forging is heated near the γ' phase dissolution temperature for a long time, which will cause coarse grains in local areas of the forging after forging. The existing hot die forging technology is restricted by factors such as die cost and heating time. The die preheating temperature is low, and the blank cools down rapidly after contacting the die to form a deformation dead zone, which is easy to cause cracking of the forging and cold die structure, resulting in increased unevenness of the strength and hardness of the high-temperature alloy. Therefore, it is urgent to provide a forging process for high-temperature alloys to effectively achieve consistency in forging quality, improve the qualified rate of forging finished products, and effectively improve the quality of forging finished products. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present invention aims to provide a forging process for a high-temperature alloy.
[0005] A forging process for a high temperature alloy comprises the following steps:
[0006] Step 1: Cutting: Take the alloy ingot after smelting process, cut the alloy ingot into required size, and obtain alloy blank;
[0007] The alloy ingot comprises, by mass percentage, 30-42% of iron, 18-25% of Cr, 1.5-2.5% of titanium, 1.2-2.5% of aluminum, 0.5-2% of thallium, 0.5-1.5% of hafnium, 0.02%-0.1% of zirconium, 0.03-0.1% of carbon, 0.001-0.006% of boron, and the balance is nickel;
[0008] Step 2, microwave preheating: use industrial microwave equipment to preheat the blank with microwaves, then transfer it to a high-temperature electric furnace and heat it to 1190-1210°C for 2-3 hours to obtain the preheated blank;
[0009] Step 3: Powder spraying: Use high-energy plasma to spray powder on the preheated blank to form a coating with a thickness of 148-152 μm;
[0010] Step 4, first forging stage: the preheated blank is subjected to solution treatment at 1050-1210℃ for 1-3h, the blank is placed in the cavity of the forging die and upset and stretched by a 1250T press to form a forging, and immediately subjected to regression and re-aging after room temperature water quenching, and the temperature is raised to 700-830℃ at a heating rate of 10-15℃ / h, and the aging treatment is carried out for 2-6h to complete the first forging stage;
[0011] Step 5, second forging stage: heat the forging to 1100-1160℃, put it back into the cavity of the forging die, and then use a 1250T press to upset the material, then widen, stretch and shape it to the required size. After forging, it is solution treated at 820-850℃ for 6-10h, air-cooled to room temperature, nitrided, annealed at 650-800℃ for 50s, and stored to complete the forging of the high-temperature alloy.
[0012] Furthermore, the smelting process is a double smelting process of vacuum induction melting + vacuum consumable remelting, or a triple smelting process of vacuum induction melting + protective atmosphere electroslag melting + vacuum consumable melting.
[0013] Furthermore, the cutting includes laser cutting and / or wire cutting.
[0014] Furthermore, the specific process parameters of the microwave preheating are: microwave preheating time 45s, pre-pressing height 60mm, microwave preheating power 6×750W.
[0015] Furthermore, the main gas of high energy plasma spraying is N2, and the auxiliary gas and carrier gas are Ar2; the spraying power is 30Kw, the distance is 100mm, the main gas flow rate is 60L / min, the auxiliary gas flow rate is 25L / min, and the carrier gas flow rate is 2L / min.
[0016] Furthermore, in the first forging stage and the second forging stage, the forgings are wrapped with thermal insulation asbestos in each forging process.
[0017] Furthermore, the nitridation treatment is carried out in a H2+N2+NH3 atmosphere at 750°C for 120s.
[0018] Furthermore, the coating is a NiCrAlY coating.
[0019] The beneficial effects achieved by the present invention are as follows: 1. The present invention improves the forging process, performs pre-forging at the solid solution temperature, then performs regression and re-aging, and finally performs final forging, and finally adopts solid solution treatment. The regression and re-aging can improve the strength and hardness non-uniformity of the forgings, and at the same time improve the stress corrosion resistance. Pre-forging in solid solution is beneficial to improving the precipitation strengthening and dislocation strengthening of the material. Solid solution after final forging is beneficial to improving the tensile strength and yield strength of the alloy, and further improving the overall performance of the high-temperature alloy.
[0020] 2. The present invention uses nitriding annealing treatment, which can promote and inhibit the secondary crystallization of some elements after nitriding treatment, is beneficial to the inward diffusion of elements in the annealing stage, and improves the uniformity of the performance of the high-temperature alloy.
[0021] 3. The present invention adopts a microwave preheating and then heating process, and utilizes the directional characteristics of microwave heating to quickly heat the blank, so that the temperature distribution inside the blank can be uniform, thereby improving the heating efficiency.
[0022] 4. The present invention adopts an aging treatment process, which can adjust the precipitation phase of the forging, eliminate the anisotropy of the high-temperature alloy, and help to bring out the excellent performance of the high-temperature alloy.
[0023] 5. The present invention can improve the forging efficiency of high-temperature alloys by combining a variety of process technologies. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a principle block diagram of the forging process of the high-temperature alloy used in the embodiment of the present invention. DETAILED DESCRIPTION
[0025] The present invention is further described in detail below with reference to specific embodiments.
[0026] Example 1: A forging process of a high temperature alloy, such as Figure 1 As shown, the following steps are included:
[0027] Step 1: Cutting
[0028] The alloy ingots smelted by the smelting process are taken, and the alloy ingots are cut into required sizes to obtain alloy billets; the smelting process is a double smelting process of vacuum induction melting + vacuum consumable remelting; the alloy ingots include, by mass percentage: 30-42% iron, 18-25% Cr, 1.5-2.5% titanium, 1.2-2.5% aluminum, 0.5-2% thallium, 0.5-1.5% hafnium, 0.02%-0.1% zirconium, 0.03-0.1% carbon, 0.001-0.006% boron, and the balance is nickel; the cutting process is electric spark wire cutting;
[0029] Step 2: Microwave preheating
[0030] The blank was preheated by microwave using industrial microwave equipment, with a microwave preheating time of 45 seconds, a pre-pressing height of 60 mm, and a microwave preheating power of 6×750 W. The blank was then heated to 1190°C in a high-temperature electric furnace and kept at this temperature for 3 hours to obtain a preheated blank.
[0031] Step 3: Powder coating
[0032] The preheated blank was powder sprayed by high-energy plasma. The main gas of high-energy plasma spraying was N2, and the auxiliary gas and carrier gas were Ar2. The spraying power was 30Kw, the distance was 100mm, the main gas flow rate was 60L / min, the auxiliary gas flow rate was 25L / min, and the carrier gas flow rate was 2L / min, forming a coating with a thickness of 148μm.
[0033] Step 4: First forging stage
[0034] The preheated blank was solution treated at 1050℃ for 3h, and then placed in the cavity of the forging die and upset and stretched in a 1250T press to form a forging. After water quenching at room temperature, it was immediately subjected to regression and re-aging. The temperature was raised to 700℃ at a heating rate of 10℃ / h, and then kept for 4h for aging treatment to complete the first forging stage.
[0035] Step 5: Second forging stage
[0036] The forging is heated to 1100℃, put back into the cavity of the forging die, and then upset by a 1250T press, then widened, stretched and shaped to the required size. After forging, it is solution treated at 820℃ for 7h, air-cooled to room temperature, and nitrided. In an atmosphere of H2+N2+NH3, it is nitrided at 750℃ for 120s, annealed at 650℃ for 50s, and stored to complete the forging of the high-temperature alloy. In the first forging stage and the second forging stage, the forgings are wrapped with thermal insulation asbestos during each forging process.
[0037] Example 2: A forging process for a high temperature alloy, such as Figure 1 As shown, the following steps are included:
[0038] Step 1: Cutting
[0039] The alloy ingots smelted by the smelting process are taken, and the alloy ingots are cut into required sizes to obtain alloy billets; the smelting process is a double smelting process of vacuum induction melting + vacuum consumable remelting; the alloy ingots include, by mass percentage: 30-42% iron, 18-25% Cr, 1.5-2.5% titanium, 1.2-2.5% aluminum, 0.5-2% thallium, 0.5-1.5% hafnium, 0.02%-0.1% zirconium, 0.03-0.1% carbon, 0.001-0.006% boron, and the balance is nickel; the cutting process is electric spark wire cutting;
[0040] Step 2: Microwave preheating
[0041] The blank was preheated by microwave using industrial microwave equipment, with a microwave preheating time of 45 seconds, a pre-pressing height of 60 mm, and a microwave preheating power of 6×750 W. The blank was then heated to 1200°C in a high-temperature electric furnace and kept at this temperature for 3 hours to obtain a preheated blank.
[0042] Step 3: Powder coating
[0043] The preheated blank was powder sprayed by high-energy plasma. The main gas of high-energy plasma spraying was N2, and the auxiliary gas and carrier gas were Ar2. The spraying power was 30Kw, the distance was 100mm, the main gas flow rate was 60L / min, the auxiliary gas flow rate was 25L / min, and the carrier gas flow rate was 2L / min, forming a coating with a thickness of 148μm.
[0044] Step 4: First forging stage
[0045] The preheated blank was solution treated at 1150℃ for 3h, and then placed in the cavity of the forging die and upset and stretched in a 1250T press to form a forging. After quenching at room temperature, it was immediately subjected to regression and aging treatment. The temperature was raised to 750℃ at a heating rate of 12℃ / h, and then kept for 4h for aging treatment to complete the first forging stage.
[0046] Step 5: Second forging stage
[0047] The forging is heated to 1120℃, put back into the cavity of the forging die, and then upset by a 1250T press, then widened, stretched and shaped to the required size. After forging, it is solution treated at 830℃ for 7h, air-cooled to room temperature, and nitrided. In an H2+N2+NH3 atmosphere, it is nitrided at 750℃ for 120s, annealed at 700℃ for 50s, and stored to complete the forging of the high-temperature alloy. In the first forging stage and the second forging stage, the forgings are wrapped with thermal insulation asbestos during each forging process.
[0048] Example 3: A forging process of a high temperature alloy, such as Figure 1 As shown, the following steps are included:
[0049] Step 1: Cutting
[0050] The alloy ingots smelted by the smelting process are taken, and the alloy ingots are cut into required sizes to obtain alloy billets; the smelting process is a double smelting process of vacuum induction melting + vacuum consumable remelting; the alloy ingots include, by mass percentage: 30-42% iron, 18-25% Cr, 1.5-2.5% titanium, 1.2-2.5% aluminum, 0.5-2% thallium, 0.5-1.5% hafnium, 0.02%-0.1% zirconium, 0.03-0.1% carbon, 0.001-0.006% boron, and the balance is nickel; the cutting process is electric spark wire cutting;
[0051] Step 2: Microwave preheating
[0052] The blank was preheated by microwave using industrial microwave equipment, with a microwave preheating time of 45 seconds, a pre-pressing height of 60 mm, and a microwave preheating power of 6×750 W. The blank was then heated to 1190°C in a high-temperature electric furnace and kept at this temperature for 2.5 hours to obtain a preheated blank.
[0053] Step 3: Powder coating
[0054] The preheated blank was powder sprayed by high-energy plasma. The main gas of high-energy plasma spraying was N2, and the auxiliary gas and carrier gas were Ar2. The spraying power was 30Kw, the distance was 100mm, the main gas flow rate was 60L / min, the auxiliary gas flow rate was 25L / min, and the carrier gas flow rate was 2L / min, forming a coating with a thickness of 148μm.
[0055] Step 4: First forging stage
[0056] The preheated blank was solution treated at 1050℃ for 2h, and then placed in the cavity of the forging die and upset and stretched in a 1250T press to form a forging. After water quenching at room temperature, it was immediately subjected to regression and re-aging. The temperature was raised to 700℃ at a heating rate of 10℃ / h, and then kept for 3h for aging treatment to complete the first forging stage.
[0057] Step 5: Second forging stage
[0058] The forging is heated to 1100℃, put back into the cavity of the forging die, and then upset by a 1250T press, then widened, stretched and shaped to the required size. After forging, it is solution treated at 820℃ for 9h, air-cooled to room temperature, and nitrided. In an atmosphere of H2+N2+NH3, it is nitrided at 750℃ for 120s, annealed at 650℃ for 50s, and stored to complete the forging of the high-temperature alloy. In the first forging stage and the second forging stage, the forgings are wrapped with thermal insulation asbestos during each forging process.
[0059] Performance Testing
[0060] The high temperature alloys forged in Example 1, Example 2 and Example 3 were selected as test specimens for performance testing. The test results met the following conditions:
[0061] Under room temperature tensile state: tensile strength (MPa) ≤ 1117, yield strength (MPa) ≤ 731, elongation (%) ≤ 20, section shrinkage (%) ≤ 23;
[0062] Under 760℃ high temperature tensile state: tensile strength (MPa) ≤820, yield strength (MPa) ≤607, elongation (%) ≤8, section shrinkage (%) ≤10.
[0063] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A forging process for a high temperature alloy, The following steps are involved: Step 1: Cutting: Take the alloy ingot after smelting process, cut the alloy ingot into required size, and obtain alloy blank; The alloy ingot comprises, by mass percentage, 30-42% of iron, 18-25% of Cr, 1.5-2.5% of titanium, 1.2-2.5% of aluminum, 0.5-2% of thallium, 0.5-1.5% of hafnium, 0.02%-0.1% of zirconium, 0.03-0.1% of carbon, 0.001-0.006% of boron, and the balance is nickel; Step 2, microwave preheating: use industrial microwave equipment to preheat the blank with microwaves, then transfer it to a high-temperature electric furnace and heat it to 1190-1210°C for 2-3 hours to obtain the preheated blank; Step 3: Powder spraying: Use high-energy plasma to spray powder on the preheated blank to form a coating with a thickness of 148-152 μm; Step 4, first forging stage: the preheated blank is subjected to solution treatment at 1050-1210℃ for 1-3h, the blank is placed in the cavity of the forging die and upset and stretched by a 1250T press to form a forging, and immediately subjected to regression and re-aging after room temperature water quenching, and the temperature is raised to 700-830℃ at a heating rate of 10-15℃ / h, and the aging treatment is carried out for 2-6h to complete the first forging stage; Step 5, second forging stage: heat the forging to 1100-1160℃, put it back into the cavity of the forging die, and then use a 1250T press to upset the material, then widen, stretch and shape it to the required size. After forging, it is solution treated at 820-850℃ for 6-10h, air-cooled to room temperature, nitrided, annealed at 650-800℃ for 50s, and stored to complete the forging of the high-temperature alloy.
2. A forging process for a high temperature alloy according to claim 1, It is characterized in that The smelting process is a double smelting process of vacuum induction melting + vacuum consumable remelting, or a triple smelting process of vacuum induction melting + protective atmosphere electroslag melting + vacuum consumable melting.
3. A forging process for a high temperature alloy according to claim 1, It is characterized in that The cutting includes laser cutting and / or wire cutting.
4. A forging process for a high temperature alloy according to claim 1, It is characterized in that The specific process parameters of the microwave preheating are: microwave preheating time 45s, pre-pressing height 60mm, microwave preheating power 6×750W.
5. A forging process for a high temperature alloy according to claim 1, It is characterized in that The main gas of high-energy plasma spraying is N2, and the auxiliary gas and carrier gas are Ar2; the spraying power is 30Kw, the distance is 100mm, the main gas flow rate is 60L / min, the auxiliary gas flow rate is 25L / min, and the carrier gas flow rate is 2L / min.
6. A forging process for a high temperature alloy according to claim 1, It is characterized in that In the first forging stage and the second forging stage, the forgings are wrapped with thermal insulation asbestos in each forging process.
7. A forging process for a high temperature alloy according to claim 1, It is characterized in that The nitridation treatment is carried out in a H2+N2+NH3 atmosphere at 750°C for 120 seconds.
8. A forging process for a high temperature alloy according to claim 1, It is characterized in that The coating is a NiCrAlY coating.
Citation Information
Patent Citations
Die-forging forming method for high-temperature alloy
CN112247037A
FREE-FORGING PROCESSING METHOD OF Ni GROUP THERMOSTABLE ALLOY MEMBER
JP2014161861A