Resin polymer, resin composition and preparation method thereof, modified binder, electrode slurry, pole piece and battery
By using specific resin polymers and resin compositions in lithium-ion batteries, combined with carboxyl-containing binders to form a three-dimensional network structure, the problems of poor stability and insufficient adhesion of resin emulsions in the existing technology are solved, and the battery performance is improved. mechanical properties and cycle life.
Patent Information
- Application Number
- CN202410750391.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-12
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-12
AI Technical Summary
The carboxyl-containing SBR or PAA emulsions used in existing lithium-ion batteries have poor stability, leading to attenuation of battery performance, and the binder has high viscosity, large particle size, and low thermal decomposition temperature, resulting in poor dispersion during the formation of the pole piece. Uniform, poor adhesion and poor cycle performance.
Using specific resin polymers and resin compositions, a three-dimensional network structure is formed through the polymerization of monomers A, B, C and D, combined with a carboxyl-containing binder to improve the mechanical properties and corrosion resistance of the pole piece, and adjust the resin The molecular weight and glass transition temperature of the polymer optimize the stability of the electrode slurry.
It significantly improves the stability of the electrode slurry and the mechanical properties of the pole pieces, extends the cycle life of the battery, alleviates the problem of battery performance attenuation, and increases the thermal decomposition temperature and glass transition temperature of the battery.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] The invention relates to a resin polymer, a resin composition and a preparation method thereof, a modified binder, an electrode slurry, a pole piece and a battery. Background Art
[0002] With the rapid development of new energy, more and more research is being done on lithium-ion batteries. Lithium-ion batteries mainly contain positive electrode materials and negative electrode materials. Among them, the preparation of negative electrode materials requires dispersing negative electrode active materials, binders and conductive agents in a solvent to form a negative electrode slurry, and then preparing negative electrode sheets through a series of processes. Among them, the performance of the negative electrode binder has a great influence on the electrical properties of the negative electrode material. Existing studies have shown that SBR containing carboxyl groups is an important negative electrode binder, and some processes also use SBR and PAA blended as negative electrode binders.
[0003] However, based on the current lithium-ion batteries, during use, the SBR or PAA emulsion containing carboxyl groups will degrade and have poor stability, which will lead to battery performance degradation.
[0004] The prior art (KR20160032877A) discloses a binder for secondary battery electrodes, which is a polymer comprising the following monomers: a monomer containing an oxazoline group, a monomer containing a carboxylic acid group, at least one monomer selected from a (meth)acrylate monomer and a butadiene monomer, and a styrene monomer. However, the binder has defects such as high viscosity, large particle size, and low thermal decomposition temperature, which results in uneven dispersion and poor adhesion during the formation of the electrode sheet, and the battery containing the binder has poor cycle performance. Summary of the invention
[0005] In order to solve the above problems existing in the prior art, the present invention provides a resin polymer, a resin composition and a preparation method thereof, a modified binder, an electrode slurry, a pole piece and a battery. The resin polymer and the resin composition of the present invention have good stability, and the pole piece prepared from the resin polymer and the resin composition of the present invention has excellent mechanical properties and corrosion resistance, and can effectively alleviate the problem of battery performance attenuation.
[0006] The present invention provides a resin polymer, wherein the resin polymer is a linear polymer or a polymer containing a branched chain;
[0007] When the resin polymer is a linear polymer, the main chain of the resin polymer consists of repeating unit a, repeating unit b1, repeating unit c and repeating unit d;
[0008] When the resin polymer is a polymer containing branches, the main chain of the resin polymer consists of repeating units a, repeating units b2, repeating units c and repeating units d; the repeating unit b2 contains a branch E, and the branch E contains one or more of the repeating units a, repeating units b1, repeating units c and repeating units d;
[0009] The structure of the repeating unit a is shown in Formula I:
[0010]
[0011] I
[0012] In each repeating unit a, R1-R4 are each independently hydrogen or a C1-C4 alkyl group;
[0013] The structure of the repeating unit b1 is shown in Formula III:
[0014]
[0015] II1
[0016] The structure of the repeating unit b2 is shown in Formula II2:
[0017]
[0018] II2
[0019] In each repeating unit b1 and b2, R5-R8 are each independently hydrogen or C1-C4 alkyl;
[0020] The structure of the repeating unit c is shown in Formula III:
[0021]
[0022] III
[0023] In each repeating unit c, R9-R 15 Each is independently hydrogen or a C1-C4 alkyl group;
[0024] The structure of the repeating unit d is shown in Formula IV:
[0025] IV
[0026] In each repeating unit d, R 16 and R 17 Each is independently hydrogen or a C1-C4 alkyl group;
[0027] The number average molecular weight of the resin polymer is 5,000-200,000.
[0028] In the present invention, preferably, in the main chain or side chain of the resin polymer, the repeating unit a, the repeating unit b and the repeating unit c are randomly distributed or block distributed.
[0029] In the present invention, based on the total mass of the resin polymer as 100 parts, the repeating unit a is preferably 1-60 parts, more preferably 10-60 parts, for example, 15 parts; the repeating unit b is preferably 20-80 parts, more preferably 35-80 parts, for example, 40 parts, 50 parts or 60 parts; the repeating unit c is preferably 0-30 parts and not 0, for example, 15 parts, 22 parts or 25 parts.
[0030] In the present invention, the C1-C4 alkyl group is, for example, methyl, ethyl, propyl or isopropyl.
[0031] In the present invention, preferably, the number average molecular weight of the resin polymer is 5000-60000, for example, 5238, 21360, 21596, 21745, 22304, 23602, 23620, 23654 or 56821.
[0032] In the present invention, preferably, the glass transition temperature of the resin polymer is -40 to 15°C, more preferably -40 to -5°C, for example, -36°C, -25°C, -24°C, -22°C, -21°C, -20°C or -7°C.
[0033] In the present invention, preferably, the thermal decomposition temperature of the resin polymer is 350-500°C, more preferably 400-450°C, for example 415°C, 420°C, 421°C, 422°C, 425°C, 426°C, 428°C or 434°C.
[0034] In a preferred embodiment of the present invention, the structural formula of the resin polymer is as shown in Formula V:
[0035]
[0036] Ⅴ
[0037] Wherein, n is preferably 50-500.
[0038] In certain specific embodiments of the present invention, the resin polymer is a straight-chain polymer, and the main chain of the resin polymer contains repeating units a, repeating units b1, repeating units c and repeating units d; in terms of mass fractions, the repeating unit a is 1-60 parts, the repeating unit b is 20-80 parts, the repeating unit c is 0-30 parts and is not 0, and the repeating unit d is 0-30 parts.
[0039] In a specific embodiment of the present invention, the repeating unit a is 15 parts, the repeating unit b is 50 parts, the repeating unit c is 25 parts, and the repeating unit d is 5.5 parts.
[0040] In a specific embodiment of the present invention, the repeating unit a is 15 parts, the repeating unit b is 60 parts, the repeating unit c is 15 parts, and the repeating unit d is 5.5 parts.
[0041] In a specific embodiment of the present invention, the repeating unit a is 15 parts, the repeating unit b is 40 parts, the repeating unit c is 30 parts, and the repeating unit d is 5.5 parts.
[0042] In a specific embodiment of the present invention, the repeating unit a is 15 parts, the repeating unit b is 50 parts, the repeating unit c is 25 parts, and the repeating unit d is 5.5 parts.
[0043] In a specific embodiment of the present invention, the repeating unit a is 15 parts, the repeating unit b is 50 parts, the repeating unit c is 22 parts, and the repeating unit d is 5.5 parts.
[0044] In a specific embodiment of the present invention, the repeating unit a is 15 parts, the repeating unit b is 50 parts, the repeating unit c is 25 parts, and the repeating unit d is 5.9 parts.
[0045] In a specific embodiment of the present invention, the repeating unit a is 15 parts, the repeating unit b is 50 parts, the repeating unit c is 25 parts, and the repeating unit d is 5 parts.
[0046] The present invention also provides a resin composition, which comprises a solvent and the above resin polymer.
[0047] In the present invention, preferably, the viscosity of the resin composition is <300 mPa·s, more preferably 50-300 mPa·s, and further more preferably 100-200 mPa·s, for example, 104 mPa·s, 108 mPa·s, 110 mPa·s, 114 mPa·s, 119 mPa·s or 185 mPa·s.
[0048] In the present invention, preferably, the pH value of the resin composition is 7-9, for example, 7.3, 7.4, 7.6 or 7.9.
[0049] In the present invention, preferably, the solid content of the resin composition is 45%-55%, more preferably 50%-51%, for example, 50.1%, 50.2% or 50.3%. The solid content means the mass percentage of the total mass of solids in the resin composition to the total mass of the resin composition.
[0050] In the present invention, the solvent is, for example, water.
[0051] In the present invention, preferably, the resin composition is an emulsion, wherein the particle size D50 of the droplets in the emulsion is less than 300 nm, more preferably 100-250 nm, for example 149 nm, 160 nm, 171 nm, 173 nm, 182 nm, 189 nm, 195 nm or 230 nm.
[0052] The present invention also provides a method for preparing a resin composition, which comprises the following steps:
[0053] The raw material composition is subjected to a polymerization reaction to obtain a resin composition; the raw material composition comprises reactive monomers and a solvent, and the reactive monomers are monomer A, monomer B, monomer C and monomer D;
[0054] The structural formula of the monomer A is shown in Formula I':
[0055]
[0056] I'
[0057] The structural formula of the monomer B is shown in Formula II':
[0058]
[0059] II'
[0060] The structural formula of the monomer C is shown in Formula III';
[0061]
[0062] III'
[0063] The monomer D has a structural formula as shown in Formula IV';
[0064] IV'
[0065] Among them, R1-R 17 As defined above.
[0066] In the present invention, based on 100 parts by total weight of the raw materials in the raw material composition excluding the solvent, the monomer A is preferably 1-60 parts, more preferably 10-60 parts, for example 15 parts.
[0067] In the present invention, based on 100 parts by total weight of the raw materials in the raw material composition excluding the solvent, the monomer B is preferably 20-80 parts, more preferably 35-80 parts, for example 40 parts, 50 parts or 60 parts.
[0068] In the present invention, based on 100 parts of the total mass of the raw materials in the raw material composition excluding the solvent, the monomer C is preferably 0-30 parts and not 0, for example, 15 parts, 22 parts or 25 parts.
[0069] In the present invention, the monomer A as shown in formula I' is an addition-polymerizable oxazoline and its derivatives, which can react with a carboxyl group to form a three-dimensional network structure.
[0070] In the present invention, the monomer A is preferably one or more of 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline and 2-isopropenyl-5-ethyl-2-oxazoline.
[0071] In the present invention, the reaction between monomer A and carboxyl group is, for example, as shown in the following formula:
[0072]
[0073] In the present invention, the monomer B shown in Formula II' is an olefinic substance capable of double addition and its derivatives. After polymerization, the molecular chain has a rotatable double bond, which can provide toughness to the molecular chain.
[0074] In the present invention, the monomer B is preferably one or more of a conjugated diene, a linear non-conjugated diene and a cyclic diene.
[0075] Wherein, the conjugated diene is preferably one or more of butadiene, isoprene and hexadiene.
[0076] Wherein, the linear non-conjugated diene is preferably 1,4-pentadiene and / or 1,5-hexadiene.
[0077] Wherein, the cyclic diene is preferably one or more of cyclopentadiene, cyclohexadiene and cycloheptadiene.
[0078] In the present invention, the monomer C as shown in formula III' has a rigid structure and can provide good thermal stability. The glass transition temperature of the resin polymer can be adjusted by adjusting the amount of the monomer C.
[0079] In the present invention, the monomer C is preferably one or more of styrene, isopropenylbenzene, allylbenzene, p-methylstyrene, o-methylstyrene and m-methylstyrene.
[0080] In the present invention, preferably, the raw material composition further comprises an auxiliary agent, and the auxiliary agent comprises one or more of an emulsifier, an initiator and a chain transfer agent.
[0081] Wherein, the initiator is preferably a peroxide and / or an azo compound.
[0082] The peroxide may be one or more of hydrogen peroxide, potassium persulfate, sodium persulfate, ammonium persulfate, benzoyl peroxide, lauroyl peroxide, dicumyl peroxide, di-tert-butyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide and diisopropylbenzene hydroperoxide.
[0083] The azo compound is, for example, 2,2'-azobisisobutylnitrile, 2,2'-azobis-(2,4-dimethylvaleronitrile), azobiscyanovaleric acid and 2,2'-azobis(2-amidinopropane) dihydrochloride.
[0084] Among them, the emulsifier is preferably one or more of sodium dihexyl sulfosuccinate, sodium dodecylbenzene sulfonate, fatty alcohol ether sulfate, dodecylphenol polyoxyethylene ether, octylphenol polyoxyethylene ether, sodium secondary alkyl sulfonate, alkyl diphenyl ether disulfonate and aliphatic carboxylate.
[0085] Wherein, when the emulsifier is sodium dodecylbenzene sulfonate and dodecylphenol polyoxyethylene ether, the mass ratio of the sodium dodecylbenzene sulfonate to the dodecylphenol polyoxyethylene ether is 1:1 or 2:1.
[0086] Wherein, the chain transfer agent is preferably one or more of n-dodecyl mercaptan, tert-dodecyl mercaptan, diisopropyl xanthate disulfide and α-methylstyrene linear dimer.
[0087] Wherein, in terms of mass parts, the initiator is preferably 0.1-5 parts, for example, 1 part, 1.5 parts or 4 parts; the emulsifier is preferably 0.5-6 parts, for example, 3 parts or 4 parts; the chain transfer agent is preferably 0.05-1 parts, for example, 0.1 parts or 0.5 parts.
[0088] In the present invention, the solvent may be a conventional solvent in the art, such as water.
[0089] Preferably, the solvent is 100 parts based on 100 parts of the total mass of the raw materials in the raw material composition excluding the solvent.
[0090] Wherein, based on 100 parts of the total mass of the raw materials in the raw material composition excluding the solvent, the monomer D is preferably 0-30 parts, more preferably 0-15 parts, for example 5 parts, 5.5 parts or 5.9 parts.
[0091] Wherein, the monomer D as shown in formula IV' is an acrylic monomer and its derivatives, and the acrylic monomer and its derivatives can adjust the mechanical properties of the resin polymer, such as thermal stability, film-forming property, wettability and corrosion resistance.
[0092] In certain specific embodiments of the present invention, the reactive monomers include monomer A, monomer B, monomer C and monomer D, wherein R1, R2 and R4-R 17 is selected from hydrogen, R3 is selected from methyl; based on the total mass of the raw materials in the raw material composition excluding the solvent as 100 parts, the monomer A is 1-60 parts, the monomer B is 20-80 parts, the monomer C is 0-30 parts and is not 0, and the monomer D is 0-30 parts.
[0093] In certain specific embodiments of the present invention, the reactive monomers include monomer A, monomer B, monomer C and monomer D, wherein R1-R 17 Selected from hydrogen; based on the total mass of the raw materials in the raw material composition excluding the solvent as 100 parts, the monomer A is 1-60 parts, the monomer B is 20-80 parts, the monomer C is 0-30 parts and is not 0, and the monomer D is 0-30 parts.
[0094] Among them, in a specific embodiment of the present invention, based on the total mass of the raw materials in the raw material composition excluding the solvent as 100 parts, the monomer A is 15 parts, the monomer B is 50 parts, the monomer C is 25 parts, and the monomer D is 5.5 parts.
[0095] Among them, in a specific embodiment of the present invention, based on the total mass of the raw materials in the raw material composition excluding the solvent as 100 parts, the monomer A is 15 parts, the monomer B is 60 parts, the monomer C is 25 parts, and the monomer D is 5.5 parts.
[0096] Among them, in a specific embodiment of the present invention, based on the total mass of the raw materials in the raw material composition excluding the solvent as 100 parts, the monomer A is 15 parts, the monomer B is 40 parts, the monomer C is 30 parts, and the monomer D is 5.5 parts.
[0097] Among them, in a specific embodiment of the present invention, based on the total mass of the raw materials in the raw material composition excluding the solvent as 100 parts, the monomer A is 15 parts, the monomer B is 50 parts, the monomer C is 25 parts, and the monomer D is 5.5 parts.
[0098] Among them, in a specific embodiment of the present invention, based on the total mass of the raw materials in the raw material composition excluding the solvent as 100 parts, the monomer A is 15 parts, the monomer B is 50 parts, the monomer C is 22 parts, and the monomer D is 5.5 parts.
[0099] Among them, in a specific embodiment of the present invention, based on the total mass of the raw materials in the raw material composition excluding the solvent as 100 parts, the monomer A is 15 parts, the monomer B is 50 parts, the monomer C is 25 parts, and the monomer D is 5.9 parts.
[0100] Among them, in a specific embodiment of the present invention, based on the total mass of the raw materials in the raw material composition excluding the solvent as 100 parts, the monomer A is 15 parts, the monomer B is 50 parts, the monomer C is 25 parts, and the monomer D is 5 parts.
[0101] In the present invention, preferably, the resin composition is prepared by free radical emulsion polymerization or solution polymerization.
[0102] In the present invention, the polymerization reaction temperature is preferably 40-120°C, such as 70°C or 80°C.
[0103] In the present invention, the polymerization reaction pressure is preferably 0.2-4 MPa, more preferably 1.5-3 MPa, for example 2 MPa or 2.5 MPa.
[0104] In the present invention, the polymerization reaction time is preferably 5-20 min, more preferably 8-11 min, for example 9 min or 10 min.
[0105] In the present invention, preferably, the polymerization reaction is carried out in a microcoil. The microcoil polymerization has good mass transfer effect, uniform material mixing, controllable pressure during the reaction process, and the resin composition is polymerized through the micro-pipe coil to obtain the target product, which has a simple process, a high conversion rate, and synthetic adjustability; and the microcoil of the present invention can also overcome the problem that monomer B (such as butadiene) is difficult to polymerize in the conventional autoclave preparation.
[0106] In certain preferred embodiments of the present invention, the method for preparing the resin composition comprises the following steps: mixing the monomer A, monomer C and an auxiliary agent to obtain a pre-emulsion; mixing the pre-emulsion and the monomer B in a microcoil and performing a polymerization reaction to obtain a resin composition.
[0107] The speed at which the pre-emulsion is introduced into the microcoil is preferably 10-300 mL / min, more preferably 80-100 mL / min, for example 90 mL / min.
[0108] The speed at which the monomer B is introduced into the microcoil is preferably 5-100 mL / min, for example, 30 mL / min or 40 mL / min.
[0109] The present invention also provides a resin composition prepared by the method for preparing the resin composition.
[0110] In the present invention, preferably, the viscosity of the resin composition is <300 mPa·s, more preferably 50-300 mPa·s, and further more preferably 100-200 mPa·s, for example, 104 mPa·s, 108 mPa·s, 110 mPa·s, 114 mPa·s, 119 mPa·s or 185 mPa·s.
[0111] In the present invention, preferably, the pH value of the resin composition is 7-9, for example, 7.3, 7.4, 7.6 or 7.9.
[0112] In the present invention, preferably, the solid content of the resin composition is 45%-55%, more preferably 50%-51%, for example, 50.1%, 50.2% or 50.3%.
[0113] In the present invention, preferably, the solvent is water.
[0114] In the present invention, preferably, the resin composition is an emulsion; wherein the particle size of the droplets in the emulsion is less than 300 nm.
[0115] The present invention also provides a method for preparing a resin polymer, which comprises the following steps: removing the solvent from the resin composition to obtain the resin polymer.
[0116] In the present invention, preferably, the method of removing the solvent is heating evaporation.
[0117] The present invention also provides a modified binder, which comprises a binder and the above resin polymer, wherein the binder contains a carboxyl group.
[0118] In the present invention, preferably, the pH value of the binder is 4-6.5.
[0119] In the present invention, preferably, the binder is SBR and / or PAA. In the present invention, SBR means an ethylene copolymer containing a structural unit derived from an ethylenically unsaturated carboxylic acid monomer and a structural unit derived from a monomer copolymerizable with the ethylenically unsaturated carboxylic acid monomer.
[0120] In the present invention, PAA is polyacrylic acid, and its chemical formula is (C3H4O2)n.
[0121] Wherein, the viscosity of the SBR is preferably 20-500 mPa·s.
[0122] The number average molecular weight of the SBR is preferably 2000-200000, more preferably 2000-100000, and even more preferably 5000-20000.
[0123] The particle size D50 of the SBR is preferably 50-800 nm, more preferably 100-300 nm.
[0124] In the present invention, preferably, the mass percentage of the resin polymer to the mass percentage of the binder is 0.5%-25%, more preferably 0.5%-10%.
[0125] The present invention also provides an electrode slurry, which comprises an electrode active substance, a solvent and the modified binder.
[0126] The present invention also provides a pole piece, which is made by using the above-mentioned electrode slurry.
[0127] The present invention also provides a battery, which comprises the above-mentioned pole piece.
[0128] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0129] The reagents and raw materials used in the present invention are commercially available.
[0130] The positive and progressive effects of the present invention are:
[0131] The invention provides a specific resin composition and a resin polymer, which are obtained by polymerizing monomers A, B, C and D simultaneously, wherein the presence of monomer A enables the resin polymer to form a three-dimensional network structure, the monomer B provides toughness for the molecular chain of the resin polymer, the presence of monomer C can adjust the glass transition temperature of the resin polymer, and the presence of monomer D can adjust the mechanical properties of the resin polymer; the monomers A, B, C and D cooperate with each other, so that the resin polymer has strong controllable performance, can be compounded with binders with different functions, and can reduce the degree of degradation of the resin polymer and improve its stability, so that the resin polymer has excellent thermal decomposition temperature and glass transition temperature.
[0132] The resin polymer is used in combination with a binder containing a carboxyl group as an electrode binder, which can react with the carboxyl group and form a three-dimensional cross-linked network structure during the formation of the electrode sheet, thereby improving the stability of the electrode slurry. At the same time, this structure can increase the mechanical properties and corrosion resistance of the electrode sheet, slow down the volume change caused by the negative electrode material during the cycle, and further alleviate the problem of battery performance attenuation, thereby improving the battery performance and cycle life.
[0133] The preparation method of the resin composition and the resin polymer provided by the present invention is to polymerize monomers A, B, C and D simultaneously. If monomers B, C and D are polymerized first and then polymerized with monomer A, the obtained resin polymer used in the battery pole piece will make the pole piece's peel strength, tensile strength, elongation at break and cycle performance all inferior to the present invention; if monomers A, B, C and D are polymerized together with monomers containing carboxylic acid groups and directly used as electrode adhesives, a small amount of or even no three-dimensional cross-linked network structure will be formed during the electrode formation process, thereby failing to form a strong binding effect, and the above method will also cause the composition to contain some particles that are not easily soluble in solvents, thereby affecting the cycle performance of the battery.
[0134] In addition, the molecular weight of the resin polymer needs to be controlled within the range of 5000-200000 in the present invention. If the molecular weight is too high, the migration effect of the resin polymer will be deteriorated during the formation of the electrode, resulting in a lower density of the three-dimensional grid structure and poorer adhesion. If the molecular weight is too low, its tensile strength and elongation at break will be reduced, resulting in poorer mechanical properties and electrolyte resistance, thereby reducing the cycle performance of the battery. DETAILED DESCRIPTION
[0135] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0136] Examples 1-10
[0137] (1) Resin composition
[0138] The preparation method of the resin composition comprises the following steps:
[0139] The raw material composition is subjected to polymerization reaction to obtain a resin composition; the raw material composition includes reactive monomers and auxiliary agents; the reactive monomers include monomer A, monomer B, monomer C and monomer D; the auxiliary agents include emulsifiers, initiators, chain transfer agents and solvents; the emulsifiers are sodium dodecylbenzene sulfonate and dodecylphenol polyoxyethylene ether; the initiator is ammonium persulfate; the chain transfer agent is dodecyl mercaptan; and the solvent is water. Specifically, monomer A, monomer C, monomer D and auxiliary agents are mixed to obtain a pre-emulsion; the pre-emulsion and monomer B are mixed in a microcoil and subjected to polymerization reaction to obtain a resin composition;
[0140] Wherein, the mass fractions of monomer A, monomer B, monomer C and monomer D in the reaction monomers, and the mass ratio of sodium dodecylbenzene sulfonate and dodecylphenol polyoxyethylene ether are listed in Table 1, and the time, temperature, pressure, speed of the pre-emulsion passing into the microcoil, and speed of monomer B passing into the microcoil of the polymerization reaction of Examples 1-10 are listed in Table 2;
[0141] The structural formula of monomer A is shown in Formula I':
[0142]
[0143] I'
[0144] The structural formula of monomer B is shown in Formula II':
[0145]
[0146] II'
[0147] The structural formula of monomer C is shown in Formula III';
[0148]
[0149] III'
[0150] The structural formula of monomer D is shown in Formula IV';
[0151]
[0152] IV'.
[0153] Among them, in Examples 1-9, the resin composition is prepared by the above method, R1-R 17 Selected from hydrogen.
[0154] Among them, in Example 10, the resin composition is prepared by the above method, R1-R 17 Except R3 which is selected from methyl, the others are selected from hydrogen.
[0155] In Table 1, the total number of parts of monomer A, monomer B, monomer C, monomer D, emulsifier, initiator and chain transfer agent is 100 parts, and the number of parts of solvent is 100 parts.
[0156] Table 1
[0157]
[0158] Table 2
[0159]
[0160] (2) Resin polymer
[0161] The preparation method of the resin polymer is: heating and evaporating the resin composition.
[0162] The resin polymers of Examples 1-10 are prepared by the above-mentioned preparation method, and the obtained resin polymers are all linear polymers, and their main chains contain repeating units a, repeating units b1, repeating units c and repeating units d;
[0163] The structure of repeating unit a is shown in Formula I:
[0164]
[0165] I
[0166] The structure of repeating unit b1 is shown in formula II1:
[0167]
[0168] II1
[0169] The structure of the repeating unit c is shown in Formula III:
[0170]
[0171] III
[0172] The structure of the repeating unit d is shown in Formula IV:
[0173]
[0174] IV.
[0175] Among them, in Examples 1-9, R1-R 17 Selected from hydrogen.
[0176] Among them, in Example 10, R1-R 17 Except R3 which is selected from methyl, the others are selected from hydrogen.
[0177] The specific contents of repeating unit a, repeating unit b1, repeating unit c and repeating unit d are listed in the following Table 3 in terms of mass fractions:
[0178] Table 3
[0179]
[0180] (3) Modified binder
[0181] The preparation method of the modified binder is: mixing the resin polymer of Examples 1-10 and the binder; wherein the mass percentage of the resin polymer to the mass percentage of the binder is 5%.
[0182] The binder is SBR, which is purchased from Japan Co., Ltd. with a model number of AL3001. The pH value of SBR is 6, the viscosity of SBR is 100 mPa·s, the number average molecular weight of SBR is 10,000, and the particle size D50 of SBR is 200 nm.
[0183] Among them, the test method for the viscosity of SBR is: using a rotational viscometer for testing, the rotor model is selected as rotor No. 2, the speed is 60rpm / min, model: NDJ-8S, manufacturer: Shanghai Changji Geological Instrument Co., Ltd.
[0184] The test method for the particle size D50 of SBR is: using a laser particle size analyzer to test the particle size, equipment model: BT-9300S, equipment manufacturer: Dandong Better Instrument Co., Ltd.
[0185] (4) Negative electrode slurry
[0186] The preparation method of the negative electrode slurry is as follows: 96 g of natural graphite as a negative electrode active ingredient, 1.5 g of CMC, and 2.5 g of the modified binder of Examples 1-10 are uniformly mixed to obtain the negative electrode slurry.
[0187] (5) Negative electrode
[0188] The preparation method of the negative electrode sheet is as follows: setting the scraper thickness to 200 μm, coating the negative electrode slurry of Examples 1-10 on one side of a copper foil with a thickness of 8 μm, drying at 90° C., rolling, and cutting to obtain a negative electrode sheet with a diameter of 12 mm.
[0189] Comparative Example 1
[0190] The preparation method of the resin polymer of Comparative Example 1 comprises the following steps:
[0191] The raw material composition is subjected to polymerization reaction to obtain a resin polymer; the raw material composition includes reactive monomers, and the reactive monomers include monomer B, monomer C and monomer D, wherein the types of monomer B, monomer C and monomer D are the same as those in Example 10. Specifically, monomer B, monomer C, monomer D and an auxiliary agent are mixed to obtain a pre-emulsion; the pre-emulsion is mixed in a microcoil tube and subjected to polymerization reaction, and the resin polymer is obtained after the solvent is removed.
[0192] The resin composition of Comparative Example 1 is prepared by mixing the above resin polymer and 15 parts of substance A to form a blend solution. The type of substance A is the same as the monomer A in Example 10. In which, by mass, substance A is 15 parts, the parts of monomer B, monomer C and monomer D are listed in Table 1, and the process parameters of the polymerization reaction are listed in Table 2.
[0193] The binder, electrode slurry and electrode sheet of Comparative Example 1 are the same as those of Example 10 except for the resin polymer.
[0194] Comparative Example 2
[0195] (1) Resin composition
[0196] The preparation method of the resin composition of Comparative Example 2 comprises the following steps:
[0197] The reaction monomers and the additives were mixed in a microcoil and polymerized at 70°C and 2 MPa for 9 min.
[0198] The reaction monomers include 15g of monomer A, 45g of monomer B, 15g of monomer C, 5.5g of monomer D, and 15g of SBR, and the types of monomer A, monomer B, monomer C, monomer D, and SBR are the same as those in Example 2;
[0199] The auxiliary agent includes 1 g of ammonium persulfate, 2 g of sodium dodecylbenzene sulfonate, 2 g of dodecylphenol polyoxyethylene ether, 0.5 g of dodecyl mercaptan and 100 g of water.
[0200] (2) Negative electrode slurry
[0201] The preparation method of the negative electrode slurry is as follows: 96 g of natural graphite as a negative electrode active ingredient, 1.5 g of CMC, and 2.5 g of the modified binder of Comparative Example 2 are uniformly mixed to obtain the negative electrode slurry.
[0202] (3) Negative electrode
[0203] The preparation method of the negative electrode sheet is as follows: setting the scraper thickness to 200 μm, coating the negative electrode slurry of Comparative Example 2 on one side of a copper foil with a thickness of 8 μm, drying at 90° C., rolling, and cutting to obtain a negative electrode sheet with a diameter of 12 mm.
[0204] Comparative Example 3
[0205] (1) Resin composition
[0206] The preparation method of the resin composition of Comparative Example 3 comprises the following steps:
[0207] The reaction monomers and the additives were mixed in a microcoil and polymerized at 70°C and 2 MPa for 10 min.
[0208] The reaction monomers include 5 g of 2-isopropenyl-2-oxazoline, 5 g of acrylic acid, 60 g of butadiene, and 30 g of styrene;
[0209] The auxiliary agent includes 1 g of ammonium persulfate, 2 g of sodium dodecylbenzene sulfonate, 2 g of dodecylphenol polyoxyethylene ether, 0.5 g of dodecyl mercaptan and 100 g of water.
[0210] (2) Negative electrode slurry
[0211] The preparation method of the negative electrode slurry is as follows: 96 g of natural graphite as a negative electrode active ingredient, 1.5 g of CMC, and 2.5 g of the resin composition of Comparative Example 3 are uniformly mixed to obtain the negative electrode slurry.
[0212] (3) Negative electrode
[0213] The preparation method of the negative electrode sheet is as follows: setting the scraper thickness to 200 μm, coating the negative electrode slurry of Comparative Example 3 on one side of a copper foil with a thickness of 8 μm, drying at 90° C., rolling, and cutting to obtain a negative electrode sheet with a diameter of 12 mm.
[0214] Effect Example 1
[0215] 1. Solid content test: The solid content of the resin compositions prepared in Examples 1-10 and Comparative Examples 1-3 was tested according to the standard SH / T1154-1999 for the determination of total solid content of synthetic rubber latex.
[0216] 2. Viscosity test: The viscosity of the resin compositions prepared in Examples 1-10 and Comparative Examples 1-3 was tested according to the standard SH / T 1152-1999 (2005) for the determination of viscosity of synthetic latex.
[0217] 3. pH value test: The pH values of the resin compositions prepared in Examples 1-10 and Comparative Examples 1-3 were tested according to the standard SH / T 1150-1999 for determination of pH value of synthetic rubber latex.
[0218] 4. Particle size D50 test of resin composition: The particle size D50 of the resin compositions prepared in Examples 1-10 and Comparative Examples 1-3 was tested using a BT-9300S laser particle size analyzer, wherein the particle size D50 refers to the particle size D50 of droplets in the resin composition emulsion.
[0219] 5. Determination of number average molecular weight: The resin polymers of Examples 1-10 and Comparative Examples 1-3 were dissolved in THF (tetrahydrofuran) to form a uniform solution, and measured by gel permeation chromatography (GPC) (model: Waters 515 series, manufacturer: Waters Corporation, USA).
[0220] 6. Testing method for thermal decomposition temperature: The thermal decomposition temperature of the resin polymers prepared in Examples 1-10 and Comparative Examples 1-3 was tested using TGA (model: DSC3, manufacturer: Mettler). Under a nitrogen atmosphere, the heating rate was set to 10°C / min, and the temperature was raised from 30°C to 800°C to obtain a thermogravimetric curve of the resin composition. The thermal decomposition temperature was obtained by analyzing the initial decomposition temperature and the termination decomposition temperature of the sample.
[0221] 7. Test method for glass transition temperature: The glass transition temperature of the resin polymers prepared in Examples 1-10 and Comparative Examples 1-3 was tested using DSC (model: TGA2, manufacturer: Mettler) equipment. Under a nitrogen atmosphere, the heating rate was set to 10°C / min, the temperature was increased from 30°C to 200°C, then decreased from 200°C to 30°C, and finally increased from 30°C to 200°C to obtain a DSC curve of the resin composition. The glass transition temperature of the sample can be obtained by analyzing the curve.
[0222] The physical properties of the resin polymers and resin compositions prepared in Examples 1-10 and Comparative Examples 1-3 are listed in Table 4 below:
[0223] Table 4
[0224]
[0225] It can be seen from Table 4 that the resin polymers provided by Examples 1-10 have excellent thermal decomposition temperatures and glass transition temperatures.
[0226] Compared with Example 10, the preparation methods of the resin composition of Comparative Example 1 are different. The resin polymer and glass transition temperature of Comparative Example 1 are both reduced, indicating that the thermal stability of the resin polymer of Comparative Example 1 is worse than that of Example 10.
[0227] Since the resin composition of Comparative Example 3 reacts with carboxyl-containing acrylic acid first, its molecular weight is too large, and the viscosity of the resin composition is significantly increased compared with Examples 1-10, and the thermal decomposition temperature of the resin composition is also significantly reduced.
[0228] Effect Example 2
[0229] 1. Slurry stability test method: Test the viscosity of the electrode slurries prepared in Examples 1-10 and Comparative Examples 1-3. The viscosity is measured according to standard SH / T 1152-1999 (2005) for the determination of the viscosity of synthetic latex. The viscosity is tested every hour. A viscosity change percentage within 10% indicates that the electrode slurry has good stability.
[0230] 2. Tensile properties and elastic modulus: The electrode slurries prepared in Examples 1-10 and Comparative Examples 1-3 were dried to form films, and the tensile strength and elastic modulus were measured according to the standard GB / T528-2009.
[0231] 3. Test method for electrode peel strength: The negative electrode sheets prepared in the above-mentioned Examples 1-10 and Comparative Examples 1-3 were cut into 100×20 mm strips for later use, and a 3M rubber sheet of the same size was pasted on a rectangular stainless steel plate. VHB double-sided tape (wipe clean with alcohol before sticking), roll back and forth three times with a 2Kg standard roller to make the tape fit tightly with the steel plate, then accurately fit the pole piece (active material side) with the other side of the tape, roll back and forth three times with a 2Kg standard roller, and roll three times in the same way. Place it in a micro-controlled electronic universal testing machine (model: CMT4204, manufacturer: Meters Industrial Systems (China) Co., Ltd.), place a section of the steel plate in the fixture below the machine, clamp the steel plate vertically to the ground, gently tear it from the bottom to the middle of the pole piece, bend it 180° to the fixture above the machine, control the machine to adjust the position of the upper fixture, open the test software, set the test conditions (tensile rate 20mm / min, horizontal and vertical coordinates show displacement distance and force respectively), reset all initial parameters to zero, and start the test. The measured peel force is the peel strength.
[0232] Effect Example 3: Cyclic Performance Test Method
[0233] Preparation of lithium-ion batteries:
[0234] (1) The negative electrode sheet adopts the negative electrode sheet of the above-mentioned embodiments 1-10 and comparative examples 1-3;
[0235] (2) Preparation of positive electrode sheets: 90 g of positive electrode active material lithium iron phosphate, 5 g of binder polyvinylidene fluoride (PVDF) and 5 g of conductive agent acetylene black were added to 80 g of N-methylpyrrolidone to prepare a uniform positive electrode slurry. The scraper thickness was set to 120 μm and coated on one side of an aluminum foil with a thickness of 16 μm. The slurry was then dried at 120°C, rolled and cut to prepare positive electrode discs with a diameter of 12 mm. The weight of the active material lithium iron phosphate was about 2.5 mg to 3.5 mg.
[0236] (3) Battery assembly: The negative electrode and positive electrode sheets prepared above were used as the negative electrode and positive electrode, Celgard2400 microporous membrane was used as the separator, and 1.0 mol / L LiPF6 solution was used as the electrolyte. The solvent of the electrolyte was prepared by mixing ethylene carbonate (EC), diethyl carbonate (DEC) and ethyl methyl carbonate (EMC) in a volume ratio of 1:1:1. The positive electrode sheet, negative electrode sheet, separator and electrolyte were assembled into a CR2032 button cell in an argon-filled glove box to test the electrical properties of the lithium-ion battery. During the test, the cut-off voltage of the charging process was 3.65V, and the cut-off voltage of the discharging process was 2.0V.
[0237] At 50°C, the lithium ion batteries prepared in the above Examples 1-10 and Comparative Examples 1-3 were first activated by 0.1C charge and discharge at room temperature, and then charged at a constant current and constant voltage rate of 1C at 50°C with a cut-off voltage of 3.65V. They were discharged from 3.655V to 2.0V at a current of 1C, and cycled to record the first discharge capacity. The test was stopped when the remaining capacity was less than 80%, and the number of cycles was recorded.
[0238] The above test results of Examples 1-10 and Comparative Examples 1-3 are listed in Table 5 below:
[0239] Table 5
[0240]
[0241] According to the data in Table 5, the electrode slurry provided by Examples 1-10 has high stability, the electrode slurry provided by Examples 1-10 has high tensile properties and elastic modulus after drying and film formation, and the battery provided by Examples 1-10 has good cycle performance and high peel strength of the electrode sheet.
[0242] Compared with Example 10, the molecular weight of Comparative Example 1 is reduced, and the mechanical properties and cycle performance of its pole piece are not as good as those of Example 10. This may be because in the binder, the propenyl oxazoline in Comparative Example 1 exists in the form of a monomer, while the propenyl oxazoline is in a liquid state. Due to the presence of small liquid molecules, the molecular chain entanglement connection becomes poor, thereby reducing the peel strength; and because the propenyl oxazoline exists in the form of a monomer, the side reactions of the battery system will increase, resulting in deterioration of battery performance and decreased cycle performance.
[0243] Compared with Example 2, Comparative Example 2 has poor slurry stability, and the peel strength, tensile strength and elongation at break all decrease significantly, indicating that the mechanical properties and corrosion resistance of the pole piece of Comparative Example 2 decrease significantly, thereby reducing the performance and cycle life of the battery. Comparative Example 2 and Example 2 use the same type of monomers and additives, but the cycle performance of its battery decreases from 954 cycles to 294 cycles. This is probably because the SBR containing carboxyl groups in Comparative Example 2 has reacted with the oxazoline monomers first, resulting in a large amount of consumption of the groups that can react with the carboxyl groups. Therefore, in the process of forming the pole piece, when the three-dimensional network structure formed by the carboxyl groups and the groups that can react with the carboxyl groups is required to bond the active material and the current collector, a strong bonding force cannot be formed, resulting in a decrease in the mechanical properties and corrosion resistance of the pole piece; and the above method will also cause the composition to contain some particles that are not easily soluble in the solvent, resulting in deterioration of the battery performance and decreased cycle performance.
[0244] Compared with the present invention, the main difference between Comparative Example 3 is that all monomers and carboxyl-containing monomers are reacted together in Comparative Example 3, and in addition, Comparative Example 3 does not contain the monomer D of the present application, which ultimately leads to a significant decrease in the mechanical properties and corrosion resistance of the electrode of Comparative Example 3, thereby reducing the performance and cycle life of the battery.
[0245] Although the specific embodiments of the present invention are described above, it should be understood by those skilled in the art that this is only for illustration and the protection scope of the present invention is defined by the appended claims. Those skilled in the art may make various changes or modifications to these embodiments without departing from the principles and essence of the present invention, but these changes and modifications all fall within the protection scope of the present invention.
Claims
1. A resin polymer, It is characterized in that The resin polymer is a linear polymer; the main chain of the resin polymer is composed of repeating units a, repeating units b 1 , repeating unit c and repeating unit d; The structure of the repeating unit a is shown in Formula I: In each repeating unit a, R 1 -R 4 Each is independently hydrogen or a C1-C4 alkyl group; The repeating unit b 1 The structure is as shown in Formula II 1 As shown: Each repeating unit b 1 In, R 5 -R 8 Each is independently hydrogen or a C1-C4 alkyl group; The structure of the repeating unit c is shown in Formula III: In each repeating unit c, R 9 -R 15 Each is independently hydrogen or a C1-C4 alkyl group; The structure of the repeating unit d is shown in Formula IV: In each repeating unit d, R 16 and R 17 Each is independently hydrogen or a C1-C4 alkyl group; The number average molecular weight of the resin polymer is 5000-200000; Based on 100 parts of the total mass of the resin polymer, the repeating unit a is 1-60 parts, and the repeating unit b is 1 The repeating unit c is 0-30 parts and is not 0.
2. The resin polymer according to claim 1, It is characterized in that In the main chain of the resin polymer, the repeating unit a, the repeating unit b 1 and the repeating unit c is randomly distributed or block distributed; and / or, the C1-C4 alkyl group is methyl, ethyl, propyl or isopropyl; And / or, the number average molecular weight of the resin polymer is 5000-60000; And / or, the glass transition temperature of the resin polymer is -40 to 15°C; And / or, the thermal decomposition temperature of the resin polymer is 350-500°C.
3. A resin composition, It is characterized in that It comprises a solvent and the resin polymer as claimed in claim 1 or 2.
4. The resin composition according to claim 3, It is characterized in that The viscosity of the resin composition is <300 mPa·s; And / or, the pH value of the resin composition is 7-9; And / or, the solid content of the resin composition is 45%-55%; and / or, the solvent is water; And / or, the resin composition is an emulsion; wherein the particle size D50 of droplets in the emulsion is less than 300 nm.
5. A method for preparing a resin composition, It is characterized in that It includes the following steps: The raw material composition is subjected to polymerization reaction to obtain a resin composition; the raw material composition comprises a reaction monomer, a solvent and an auxiliary agent, the auxiliary agent is one or more of an emulsifier, an initiator and a chain transfer agent, and the reaction monomer is a monomer A, a monomer B, a monomer C and a monomer D; The structural formula of the monomer A is shown in Formula I': The structural formula of the monomer B is shown in Formula II': The structural formula of the monomer C is shown in Formula III'; The monomer D has a structural formula as shown in Formula IV'; Among them, R 1 -R 17 Each is independently hydrogen or a C1-C4 alkyl group; The resin composition comprises a resin polymer, and the number average molecular weight of the resin polymer is 5000-200000; Based on 100 parts of the total weight of the raw materials in the raw material composition excluding the solvent, the monomer A is 1-60 parts, the monomer B is 20-80 parts, and the monomer C is 0-30 parts and is not 0.
6. The method for preparing the resin composition according to claim 5, It is characterized in that The monomer A is one or more of 2-vinyl-2-oxazoline, 2-vinyl-4-methyl-2-oxazoline, 2-vinyl-5-methyl-2-oxazoline, 2-isopropenyl-2-oxazoline, 2-isopropenyl-4-methyl-2-oxazoline and 2-isopropenyl-5-ethyl-2-oxazoline; and / or, the monomer B is a conjugated diene; and / or, the monomer C is one or more of styrene, isopropenylbenzene, allylbenzene, p-methylstyrene, o-methylstyrene and m-methylstyrene; And / or, the solvent is water.
7. The method for preparing the resin composition according to claim 5, It is characterized in that The resin composition is prepared by free radical emulsion polymerization or solution polymerization; And / or, the polymerization reaction temperature is 40-120°C; And / or, the polymerization reaction pressure is 0.2-4Mpa; And / or, the polymerization reaction time is 5-20min; And / or, the preparation method of the resin composition comprises the following steps: mixing the raw materials except monomer B in the raw material composition to obtain a pre-emulsion; and separately and simultaneously introducing the pre-emulsion and the monomer B into a microcoil tube for mixing and performing a polymerization reaction to obtain a resin composition.
8. A resin composition obtained by the method for preparing the resin composition according to any one of claims 5 to 7.
9. A method for preparing a resin polymer, It is characterized in that The method comprises the following steps: removing the solvent from the resin composition as described in any one of claims 3, 4 and 8.
10. A modified binder, It is characterized in that It comprises a binder and the resin polymer according to claim 1 or 2, wherein the binder contains a carboxyl group.
11. The modified binder according to claim 10, It is characterized in that The pH value of the binder is 4-6.5; And / or, the mass percentage of the resin polymer to the mass percentage of the binder is 0.5%-25%; And / or, the binder is SBR and / or PAA.
12. An electrode slurry, It is characterized in that The invention comprises an electrode active material, a solvent and the modified binder as claimed in claim 10 or 11.
13. A pole piece, It is characterized in that It is prepared using the electrode slurry as claimed in claim 12.
14. A battery, It is characterized in that It comprises the pole piece as claimed in claim 13.