Preparation method of super-hydrophobic wear-resistant water-based strippable coating
The water-based polyurethane coating prepared by prepolymer dispersion method combines modified fillers and functional additives to solve the problems of high prices and poor applicability of existing peelable coatings, and realizes superhydrophobic and resistance on various substrates Abrasiveness and self-cleaning properties provide efficient protection.
Patent Information
- Application Number
- CN202411118943.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-15
AI Technical Summary
The existing peelable coatings are expensive and have poor broad spectrum applicability. Commonly used additives have adverse effects on the substrate, making it difficult to achieve excellent hydrophobicity and wear resistance on a variety of substrates.
Using the prepolymer dispersion method, polycarbonate polyol and polyisocyanate are used as comonomers, anionic hydrophilic group-containing aminoalkyl sulfonate is added as chain extenders, and a modified filler and functional additives are combined. Superhydrophobic, wear-resistant aqueous polyurethane dispersions are prepared to form a transparent protective coating without baking.
It achieves efficient peeling, hydrophobicity and wear resistance on a variety of substrates, has self-cleaning properties, and does not cause damage or residue to the substrate, providing good anti-corrosion effect.
Smart Images

Figure BDA0004994454460000191
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a method for preparing a super-hydrophobic, wear-resistant, water-based strippable coating. Background Art
[0002] Strippable coating is a special protective coating that is applied to the surface of the substrate to isolate it from external erosion and prevent it from being scratched, scratched, aged, polluted, dusty, oily, fingerprinted, etc. during production, transportation or storage. It is also called temporary protective coating, which can provide temporary protection for various substrate surfaces, such as plastic, metal, wood, ceramic, glass, rubber, pre-coated parts, etc. The general protection period ranges from a few days to a few months, and after the protection is over, it can be easily peeled off from the substrate surface without negatively affecting the substrate surface. Strippable coating has a wide range of applications. It can be used for indoor and outdoor, short-term and long-term protection of metal and non-metal materials in industry; it also has broad application prospects in civilian use, such as home car color change protection, kitchen tile protection, range hood cleaning-free protection, furniture, electrical appliance refresh services, etc.
[0003] At present, many well-known foreign coating manufacturers in the international market have developed strippable coating materials. Some European and American countries have even widely used such materials in the fields of decks, automobile production, shipbuilding protection, container freight, and wind turbine blade manufacturing to block the impact of dust or welding slag generated by the joint parts of the modules during welding and hot work. However, the prices of this type of strippable coatings from foreign coating manufacturers are generally higher than the market and expensive. At present, many strippable coatings are only suitable for some substrates, and are not strippable for many substrates, and have poor broad-spectrum applicability, which will greatly reduce the application scope of strippable coatings. In addition, most strippable coatings need the help of strippable additives to effectively reduce the adhesion between the paint film and the substrate. Common stripping additives include higher fatty acid esters, waxes, surfactants, silicones, etc. Although these additives have certain effects, they also have greater side effects and have a variety of adverse effects on the surface of the substrate, such as reducing the hydrophobicity of the material and reducing the weather resistance of the material. Therefore, in view of the above technical problems, it is necessary to have a new strippable coating. Summary of the invention
[0004] The technical problem to be solved by the present invention is: in view of the shortcomings of the prior art, a method for preparing a super hydrophobic and wear-resistant water-based strippable coating is provided. The present invention adopts a prepolymer dispersion method, firstly uses polycarbonate polyol and polyisocyanate as copolymer monomers, then adds anionic aminoalkyl sulfonate containing hydrophilic groups as a chain extender to prepare a waterborne polyurethane dispersion, and adds an auxiliary agent with specific properties and a modified filler. The prepared coating has not only a good stripping effect, but also excellent hydrophobicity, excellent wear resistance, and certain self-cleaning performance.
[0005] In order to solve the above technical problems, the technical solution of the present invention is:
[0006] A method for preparing a super hydrophobic, wear-resistant water-based peelable coating comprises the following steps:
[0007] (1) preparing a waterborne polyurethane prepolymer;
[0008] (2) preparing a waterborne polyurethane dispersion using an anionic aminoalkylsulfonate containing a hydrophilic group as a chain extender;
[0009] (3) mixing the aqueous polyurethane dispersion with a modified filler aqueous defoamer, an aqueous leveling agent, an aqueous wetting agent, a hydrophobic agent, an aqueous film-forming aid, a thickener, and deionized water, and adding a pH adjuster to adjust the pH to obtain a super-hydrophobic surface aqueous strippable coating;
[0010] The modified filler is polymer-coated SiO 2 / carbon nanotube composite filler, the coating layer is a polydimethoxysilane layer and a polycaprolactone / epoxy resin layer from the inside to the outside.
[0011] Preferably, the preparation method of the waterborne polyurethane prepolymer is: heating the diol, then vacuuming to remove water, then cooling, adding diisocyanate, and heating to react to obtain the prepolymer.
[0012] Preferably, the preparation conditions of the waterborne polyurethane prepolymer include at least one of the following:
[0013] The diol is a polycarbonate diol;
[0014] The diisocyanate is isophorone diisocyanate;
[0015] Heat the diol to 100-110°C;
[0016] The time for vacuuming and removing water is 1-2h;
[0017] The cooling temperature is 45-55℃;
[0018] The temperature of the temperature-raising reaction is 85-95° C. and the time is 1-2 hours.
[0019] Preferably, the preparation process of the waterborne polyurethane dispersion is specifically as follows: adding anionic aminoalkylsulfonate containing hydrophilic groups as a chain extender to the waterborne polyurethane prepolymer, continuing the reaction, adjusting the R value, and adding a reactive diluent at the same time, waiting for the reaction system to reach the theoretical content of chemical bond NCO groups, cooling, and adding a salt-forming agent to the reaction system, and adding deionized water under stirring conditions to adjust the solid content, thereby obtaining the waterborne polyurethane dispersion.
[0020] Preferably, the preparation of the aqueous polyurethane dispersion includes at least one of the following features:
[0021] The active diluent is N-ethylpyrrolidone;
[0022] The salt-forming agent is triethylamine;
[0023] The reaction time is 4-6 hours.
[0024] The solid content of the aqueous polyurethane dispersion is 35-40%.
[0025] Preferably, in the aqueous polyurethane dispersion, the amounts of the components are as follows by mass percentage: diol 25-35wt%, diisocyanate 8-10wt%, chain extender 1-3wt%, active diluent 12-15wt%, salt former 0.5-1.5wt%, and deionized water 40-50wt%.
[0026] Preferably, the preparation method of the modified filler comprises the following steps:
[0027] S1: acidifying the carbon nanotubes to obtain acidified carbon nanotubes, adding the acidified carbon nanotubes to an aqueous solution of ethyl orthosilicate, then adding a hydrochloric acid solution, stirring and mixing, adding dibutyltin dilaurate and continuing to stir, finally adding polydimethoxysilane, mixing again, filtering, and collecting the filtered precipitate;
[0028] S2: dissolving polycaprolactone and epoxy resin in ethyl acetate to obtain a suspension, adding the filtered precipitate to the suspension, ultrasonically treating, filtering, and drying the filtered solid to obtain a modified filler.
[0029] Preferably, in step S1, the conditions for the acidification treatment include at least one of the following characteristics:
[0030] A nitric acid solution with a concentration of 0.1-0.2 mol / L is used for acidification treatment;
[0031] During the acidification treatment, the mass ratio of carbon nanotubes to solution is (0.05-0.1):1000;
[0032] The temperature during the acidification treatment is 100-110°C and the treatment time is 30-60 minutes.
[0033] Preferably, the concentration of the tetraethyl orthosilicate aqueous solution is 3-4 mol / L, and the mass ratio of the acidified carbon nanotubes to the tetraethyl orthosilicate aqueous solution is (0.1-0.5):1.
[0034] Preferably, the concentration of the hydrochloric acid solution is 0.1-0.2 mol / L, and the volume ratio of the hydrochloric acid solution to the tetraethyl orthosilicate aqueous solution is (0.05-0.1):1.
[0035] Preferably, the volume ratio of dibutyltin dilaurate to polydimethoxysilane is 1:(2-4), and the molar ratio of polydimethoxysilane to tetraethyl orthosilicate is (0.1-0.5):1.
[0036] Preferably, the stirring and mixing temperature is 30° C., the time is 1-2 h, the stirring speed is 400-500 rpm; the time for continuing the stirring treatment is 10-20 min; and the time for remixing is 10-20 min.
[0037] Preferably, in S2, in the suspension, the concentrations of polycaprolactone and epoxy resin are 0.02-0.03 g / ml and 0.007-0.008 g / ml respectively; and the mass ratio of the filtered precipitate to the suspension is 1:(0.01-0.03).
[0038] Preferably, in S2, the power of the ultrasonic treatment is 400-500 W, and the time of the ultrasonic treatment is 1-2 h.
[0039] Preferably, the hydrophobic agent is a lotus leaf hydrophobic agent; the aqueous defoaming agent is a mixture of one or more of an aqueous polyether siloxane defoaming agent, an aqueous mineral oil defoaming agent, and an aqueous polymer polyether defoaming agent; the aqueous leveling agent is an aqueous polyether siloxane leveling agent; the aqueous wetting agent is an aqueous acetylene glycol wetting agent; the aqueous film-forming aid is one of dipropylene glycol butyl ether and dipropylene glycol phenyl ether; the thickener is an aqueous associative polyurethane thickener; and the pH adjuster is dimethylethanolamine.
[0040] Preferably, the amounts of the components in the hydrophobic surface water-based strippable coating are, in mass percentage, 70-85wt% of aqueous polyurethane dispersion, 2-5wt% of modified filler, 8-15wt% of deionized water, 0.1-0.5wt% of aqueous defoamer, 0.1-0.5wt% of aqueous polyether siloxane leveling agent, 0.1-0.5wt% of aqueous acetylene glycol wetting agent, 0.5-2wt% of aqueous oxidized polyethylene wax lotus leaf hydrophobic agent, 3-8wt% of aqueous film-forming aid, 1-2wt% of aqueous associative polyurethane thickener, and 0.3-0.5wt% of pH adjuster.
[0041] Preferably, pigments and fillers are added to the coating to replace part of the aqueous polyurethane dispersion, the mass ratio of the pigments and fillers to the aqueous polyurethane dispersion is (1-5):5, and the total addition amount of the pigments and fillers to the aqueous polyurethane dispersion is 70-85wt% of the coating mass; the pigments and fillers include composite high wear-resistant sand grain powder, 1250 mesh silica powder, rutile titanium dioxide, medium pigment carbon black powder, bentonite, and polyamide pulp, and the mass ratio of the composite high wear-resistant sand grain powder, 1250 mesh silica powder, rutile titanium dioxide, medium pigment carbon black powder, bentonite, and polyamide pulp is 5-8:10-15:10-12:0.2-0.5:1-2:1-2.
[0042] Due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0043] The invention provides a super-hydrophobic, wear-resistant water-based strippable coating and a preparation method thereof. The invention adopts a prepolymer dispersion method, uses polycarbonate polyol and polyisocyanate as comonomers, uses an anionic aminoalkylsulfonate chain extender containing a hydrophilic group to participate in polycondensation, obtains a polyurethane prepolymer with soft and hard segments, then adds a salt-forming agent for neutralization, and adds deionized water for emulsification and dispersion to obtain an aqueous polyurethane dispersion. The invention uses polycarbonate polyol as a raw material, and the synthesized aqueous polyurethane dispersion has a high melting point and glass transition temperature, excellent hydrolysis resistance, weather resistance, wear resistance and biocompatibility. The present invention uses a self-made aqueous polyurethane dispersion as the main film-forming material, and then adds modified fillers, deionized water, aqueous defoamers, aqueous leveling agents, aqueous wetting agents, hydrophobic agents, aqueous film-forming aids, and thickeners to form a continuous, evenly-applied, tough transparent protective coating on the surface of various substrates and complex shapes through spraying, brushing, and rolling. It does not need to be baked, and it dries quickly at room temperature without the release of harmful gases such as aldehydes, benzene, and ammonia. When the drying film protection demand is over, because the coating contains good cohesion, it can be easily peeled off from the surface of the device in one piece, with good continuity, no adhesion, no damage to the substrate, no penetration, and no residue. In addition, the coating prepared by the present invention can be used as a protective layer to effectively isolate the invasion of media such as air, water vapor, salt spray, and microorganisms from the outside, and reduce chemical corrosion to achieve an anti-corrosion effect; and the coating has a certain thickness and elasticity, which can alleviate external force collisions and artificial scratches to achieve a protective effect. Moreover, a certain amount of lotus leaf hydrophobic agent is added to the coating of the present invention, which can effectively block dust, oil stains, rust, etc. on the surface of the device and has self-cleaning properties.
[0044] The modified filler of the present invention is a polymer-coated SiO 2 / carbon nanotube composite filler, firstly, silica is grown in situ on the surface of acidified carbon nanotubes to improve the dispersibility of silica, then a PDMS layer is modified on the surface of silica, and then under certain conditions, a polycaprolactone / epoxy resin layer is modified on the surface of the PDMS layer, so as to form a double hydrophobic protective layer on the surface of silica and carbon nanotubes. PDMS has the characteristics of low surface energy, which can provide a hydrophobic tail, thereby preliminarily improving the hydrophobicity of the surface of the nanomaterial and effectively preventing the adhesion of dirt and other impurities; and polycaprolactone and epoxy resin can also enhance the self-cleaning performance by changing the surface energy of the material. Both polycaprolactone and epoxy resin have good mechanical properties, such as toughness and strength. When they are combined with silica and dispersed in a polyurethane matrix, the internal strength of the composite material can be increased and the ability to resist external wear can be improved. Silica itself is also a hard material. Its presence can serve as a physical barrier to reduce the direct contact and force of the matrix material, thereby improving the wear resistance. , and PDMS has good elasticity, which can absorb and disperse the scratching force and reduce direct damage to the polyurethane matrix. At the same time, the toughness of polycaprolactone and epoxy resin can also help the material not to crack or break when scratched. In summary, the addition of modified fillers improves the wear resistance, self-cleaning and hydrophobicity of the material to a certain extent. DETAILED DESCRIPTION
[0045] In order to more clearly understand the above-mentioned objectives, features and advantages of the present invention, the scheme of the present invention will be further described below. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
[0046] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein; it is obvious that the embodiments in the specification are only part of the embodiments of the present invention, rather than all of the embodiments.
[0047] In order to solve the problems pointed out in the background technology, the present invention provides a method for preparing a super-hydrophobic, wear-resistant water-based strippable coating. The present invention adopts a prepolymer dispersion method, with polycarbonate polyol and polyisocyanate as comonomers, and uses an aminoalkylsulfonate anionic chain extender containing a hydrophilic group to participate in polycondensation to obtain an aqueous polyurethane dispersion, which has a high melting point and glass transition temperature, excellent hydrolysis resistance, weather resistance, wear resistance and biocompatibility. In addition, the present invention also adds a certain amount of functional additives and polycaprolactone / epoxy resin / PDMS modified silica / carbon nanotubes as modified fillers in the aqueous polyurethane dispersion, and the obtained coating not only has good dispersibility, but also does not need to be baked, dries quickly at room temperature, and does not release harmful gases such as aldehydes, benzene, and ammonia. The coating has good peelability and does not stick when peeled off. It has no damage, no penetration, and no residue on the substrate. It can isolate the invasion of external media such as air, water vapor, salt spray, and microorganisms, and reduce chemical corrosion, and has a good anti-corrosion effect. In addition, the coating has a certain thickness and elasticity, which can alleviate external force collisions and man-made scratches to achieve a protective effect, and has a certain self-cleaning performance.
[0048] A method for preparing a super hydrophobic, wear-resistant water-based peelable coating comprises the following steps:
[0049] (1) preparing a waterborne polyurethane prepolymer;
[0050] (2) preparing a waterborne polyurethane dispersion using an anionic aminoalkylsulfonate containing a hydrophilic group as a chain extender;
[0051] (3) mixing the aqueous polyurethane dispersion with a modified filler aqueous defoamer, an aqueous leveling agent, an aqueous wetting agent, a hydrophobic agent, an aqueous film-forming aid, a thickener, and deionized water, and adding a pH adjuster to adjust the pH to obtain a super-hydrophobic surface aqueous strippable coating;
[0052] The modified filler is polymer-coated SiO 2 / carbon nanotube composite filler, the coating layer is a polydimethoxysilane layer and a polycaprolactone / epoxy resin layer from the inside to the outside.
[0053] In some embodiments, the preparation method of the waterborne polyurethane prepolymer is: heating the diol, then vacuuming to remove water, then cooling, adding diisocyanate, and heating to react to obtain the prepolymer.
[0054] In some embodiments, the preparation conditions of the waterborne polyurethane prepolymer include at least one of the following:
[0055] The diol is a polycarbonate diol;
[0056] The diisocyanate is isophorone diisocyanate;
[0057] Heat the diol to 100-110°C;
[0058] The time for vacuuming and removing water is 1-2h;
[0059] The cooling temperature is 45-55℃;
[0060] The temperature of the temperature-raising reaction is 85-95° C. and the time is 1-2 hours.
[0061] In the preparation of waterborne polyurethane prepolymer, the selection of diol and diisocyanate has a certain influence on the performance of waterborne polyurethane prepolymer. The type of diol will affect the molecular weight and flexibility of the prepolymer, and then affect the hardness and wear resistance of the final polyurethane. The selection of diisocyanate will affect the cross-linking structure and chemical temperature resistance of the polyurethane. The present invention uses polycarbonate diol and isophorone diisocyanate as polymerization monomers, and the polycarbonate diol is dehydrated under certain conditions to improve the water resistance of the polyurethane. In addition, the present invention also improves the water resistance, weather resistance and wear resistance of the final waterborne polyurethane dispersion by controlling the cross-linking temperature and cross-linking time.
[0062] In some embodiments, the preparation process of the aqueous polyurethane dispersion is specifically as follows: adding anionic aminoalkylsulfonate containing hydrophilic groups as a chain extender to the aqueous polyurethane prepolymer, continuing the reaction, adjusting the R value, and adding an active diluent at the same time, waiting for the reaction system to reach the theoretical content of chemical bond NCO groups, cooling, and adding a salt-forming agent to the reaction system, adding deionized water under stirring conditions to adjust the solid content, and obtaining an aqueous polyurethane dispersion.
[0063] In some embodiments, the preparation of the aqueous polyurethane dispersion includes at least one of the following features:
[0064] The active diluent is N-ethylpyrrolidone;
[0065] The salt-forming agent is triethylamine;
[0066] The reaction time is 4-6 hours.
[0067] The solid content of the aqueous polyurethane dispersion is 35-40%.
[0068] The present invention uses polycarbonate diol as diol, which has a regular structure and only produces CO 2, unlike other polyester polyols, carboxylic acid is not produced after hydrolysis, which is accumulated in the polymer to accelerate the hydrolysis of the polymer, and it has excellent water resistance, chemical solvent resistance, heat and humidity aging resistance, oil resistance, wear resistance, weather resistance, biological stability and compatibility. The present invention adopts isophorone diisocyanate (IPDI) as raw material, which does not contain benzene rings in its molecule, fundamentally enhances the yellowing resistance of waterborne polyurethane, and improves the light stability, weather resistance and mechanical properties of polyurethane. The present invention adopts N-ethylpyrrolidone (NEP) as active diluent, which has strong polarity and can be miscible with water and general organic solvents in any proportion. The present invention adopts anionic aminoalkyl sulfonate containing hydrophilic groups as chain extender, which contains two amino groups (primary amine + secondary amine), can be introduced into the polyurethane main chain as an excellent hydrophilic monomer, enhances the hydrophilicity of the system, thereby achieving self-emulsification effect, making polyurethane particles achieve perfect phase transition in water, and the obtained emulsion particle size is relatively small.
[0069] In some embodiments, in the aqueous polyurethane dispersion, the amounts of the components are as follows by mass percentage: diol 25-35wt%, diisocyanate 8-10wt%, chain extender 1-3wt%, active diluent 12-15wt%, salt former 0.5-1.5wt%, deionized water 40-50wt%.
[0070] In the preparation of waterborne polyurethane dispersion, diols are used as the main hydroxyl compounds to react with diisocyanates to form polyurethane segments. Too low a dosage of diols will result in incomplete polymer segments, while too high a dosage may increase viscosity or affect dispersion performance. Diisocyanates are used as hard segments of polyurethanes and react with diols to form polyurethane segments, affecting the hardness, wear resistance and mechanical properties of the product. Too low a dosage will result in a decrease in the physical properties of the product, while too high a dosage may affect the dispersion performance and weather resistance of the coating. Chain extenders are used to control the molecular weight of polyurethane, affecting its viscosity and mechanical properties. Too low a dosage will result in insufficient polymer molecular weight, while too high a dosage may increase the viscosity of the dispersion or affect the dispersion performance. Reactive diluents are used to adjust the viscosity and fluidity of the dispersion to ensure suitable application performance. Too low a dosage will result in too high a dispersion concentration, while too high a concentration may affect the drying performance and water resistance of the coating. Salt formers are used to adjust the pH value of the dispersion, affecting dispersion performance and stability. Too low a dosage will result in an unstable dispersion, while too high a dosage may affect its solubility and processing performance. Deionized water is used as a solvent and a dispersion medium to ensure uniform dispersion and stability of each component. Too low a dosage will result in insufficient dispersion concentration, while too high a dosage may affect the solid content and performance stability of the coating. The present invention optimizes the dosage of each component to obtain an excellent performance of an aqueous polyurethane dispersion, thereby improving the performance of a coating with an aqueous polyurethane dispersion as the main film-forming substance.
[0071] In some embodiments, the method for preparing the modified filler comprises the following steps:
[0072] S1: acidifying the carbon nanotubes to obtain acidified carbon nanotubes, adding the acidified carbon nanotubes to an aqueous solution of ethyl orthosilicate, then adding a hydrochloric acid solution, stirring and mixing, adding dibutyltin dilaurate and continuing to stir, finally adding polydimethoxysilane, mixing again, filtering, and collecting the filtered precipitate;
[0073] S2: dissolving polycaprolactone and epoxy resin in ethyl acetate to obtain a suspension, adding the filtered precipitate to the suspension, ultrasonically treating, filtering, and drying the filtered solid to obtain a modified filler.
[0074] In some embodiments, in step S1, the conditions of the acidification treatment include at least one of the following characteristics:
[0075] A nitric acid solution with a concentration of 0.1-0.2 mol / L is used for acidification treatment;
[0076] During the acidification treatment, the mass ratio of carbon nanotubes to solution is (0.05-0.1):1000;
[0077] The temperature during the acidification treatment is 100-110°C and the treatment time is 30-60 minutes.
[0078] In some embodiments, the concentration of the tetraethyl orthosilicate aqueous solution is 3-4 mol / L, and the mass ratio of the acidified carbon nanotubes to the tetraethyl orthosilicate aqueous solution is (0.1-0.5):1.
[0079] In some embodiments, the concentration of the hydrochloric acid solution is 0.1-0.2 mol / L, and the volume ratio of the hydrochloric acid solution to the tetraethyl orthosilicate aqueous solution is (0.05-0.1):1.
[0080] In some embodiments, the volume ratio of dibutyltin dilaurate to polydimethoxysilane is 1:(2-4), and the molar ratio of polydimethoxysilane to tetraethyl orthosilicate is (0.1-0.5):1.
[0081] In some embodiments, the stirring and mixing temperature is 30° C., the time is 1-2 hours, the stirring speed is 400-500 rpm; the time for continuing the stirring treatment is 10-20 minutes; and the time for re-mixing is 10-20 minutes.
[0082] In step S1, the present invention firstly improves the activity of the carbon nanotube surface without destroying the carbon nanotube structure by reasonably optimizing the acidification treatment conditions, so as to facilitate the deposition of silicon dioxide. In addition, the present invention also optimizes the conditions for preparing silicon dioxide by hydrolysis, thereby obtaining a silicon dioxide / carbon nanotube material with good dispersibility, and finally modifies a layer of PDMS on its surface to improve the hydrophobicity and wear resistance of the material. During modification, the amount of PDMS added is too high or too low. When modifying PDMS on the surface of silicon dioxide, an excessive amount of PDMS added will not only increase the cost, but also the insufficient reaction of part of PDMS with silicon dioxide, so that the bonding between the PDMS layer and silicon dioxide is weak, and peeling phenomenon is prone to occur, which reduces the adhesion and durability of the material. If the amount of PDMS added is too low, it is impossible to form a sufficient PDMS coating layer, resulting in incomplete coating of the silicon dioxide surface, affecting the hydrophobicity and protective performance of the material. It is necessary to reasonably control the amount of PDMS used.
[0083] In some embodiments, in S2, in the suspension, the concentrations of polycaprolactone and epoxy resin are 0.02-0.03 g / ml and 0.007-0.008 g / ml, respectively; the mass ratio of the filtered precipitate to the suspension is 1:(0.01-0.03).
[0084] In some embodiments, in S2, the power of the ultrasonic treatment is 400-500 W, and the time of the ultrasonic treatment is 1-2 h.
[0085] In some embodiments, the hydrophobic agent is a lotus leaf hydrophobic agent; the aqueous defoaming agent is a mixture of one or more of an aqueous polyether siloxane defoaming agent, an aqueous mineral oil defoaming agent, and an aqueous polymer polyether defoaming agent; the aqueous leveling agent is an aqueous polyether siloxane leveling agent; the aqueous wetting agent is an aqueous acetylene glycol wetting agent; the aqueous film-forming aid is one of dipropylene glycol butyl ether and dipropylene glycol phenyl ether; the thickener is an aqueous associative polyurethane thickener; and the pH adjuster is dimethylethanolamine.
[0086] In order to improve the hydrophobicity of the material and its compatibility with the coating matrix, the present invention also modifies the polycaprolactone / epoxy resin layer outside the PDMS layer. During the modification, the addition of too much polycaprolactone / epoxy resin will reduce the surface hydrophobicity and wear resistance of the material. This is mainly because the polycaprolactone / epoxy resin layer on the surface of the material is uneven. If the amount of polycaprolactone and epoxy resin added is insufficient, it will lead to insufficient coating, thereby affecting the wear resistance and hydrophobicity of the coating.
[0087] In some embodiments, the amounts of the components in the super-hydrophobic surface water-based peelable coating are as follows: 70-85wt% of aqueous polyurethane dispersion, 2-5wt% of modified filler, 8-15wt% of deionized water, 0.1-0.5wt% of aqueous defoamer, 0.1-0.5wt% of aqueous polyether siloxane leveling agent, 0.1-0.5wt% of aqueous acetylene glycol wetting agent, 0.5-2wt% of aqueous oxidized polyethylene wax lotus leaf hydrophobic agent, 3-8wt% of aqueous film-forming aid, 1-2wt% of aqueous associative polyurethane thickener, and 0.3-0.5wt% of pH adjuster.
[0088] In some embodiments, pigments and fillers are also added to the coating to replace part of the aqueous polyurethane dispersion, and the mass ratio of the pigments and fillers to the aqueous polyurethane dispersion is (1-5):5, and the total addition amount of the pigments and fillers and the aqueous polyurethane dispersion is 70-85wt% of the coating mass; the pigments and fillers include composite high wear-resistant sand grain powder, 1250 mesh silica powder, rutile titanium dioxide, medium pigment carbon black powder, bentonite, and polyamide pulp, and the mass ratio of the composite high wear-resistant sand grain powder, 1250 mesh silica powder, rutile titanium dioxide, medium pigment carbon black powder, bentonite, and polyamide pulp is 5-8:10-15:10-12:0.2-0.5:1-2:1-2.
[0089] The present invention adds a certain amount of lotus leaf hydrophobic agent to the aqueous polyurethane dispersion to improve the hydrophobicity of the material. The lotus leaf hydrophobic agent has extremely strong lotus leaf hydrophobicity and anti-scratch performance. When added to the aqueous coating, the paint film can have the characteristics of anti-water stains and stains, self-cleaning and maintenance, and can make the coating film have anti-fouling ability and anti-sticking characteristics, and protect the neatness of the coating surface; dimethylethanolamine is added as a pH regulator, which has the characteristic of less odor compared with other amine neutralizers; the addition of the aqueous acetylene glycol wetting agent can effectively reduce the dynamic surface tension of the system, and at the same time has excellent substrate wetting ability. The present invention also adds an appropriate amount of modified filler for modification, which improves the hydrophobicity of the coating and also provides the wear resistance, corrosion resistance and self-cleaning performance of the coating.
[0090] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0091] In the following examples and comparative examples, the sources of raw materials or performance parameters are as follows:
[0092] Polycarbonate diol: Covestro Desmophen-C1200; Isophorone diisocyanate: Wanhua Water-based defoaming agent: BYK-024; water-based polyether siloxane leveling agent: BYK-333; lotus leaf hydrophobic agent: water-based lotus leaf hydrophobic agent XH-5012, Dongguan Xuyihua Chemical Co., Ltd.; water-based film-forming agent: dipropylene glycol butyl ether; water-based associative polyurethane thickener: Hemmings-299-water-based polyurethane associative thickener; anionic aminoalkyl sulfonate chain extender containing hydrophilic groups: Xingusheng hydrophilic chain extender aminosulfonate AAS-Na, Guangzhou Xingusheng Chemical Technology Co., Ltd.; carbon nanotubes: evasive carbon nanotubes purchased from Jiangsu Xianfeng Nanomaterial Technology Co., Ltd., with a diameter of 5-15nm, an inner diameter of 2-5nm, a purity of >95%, a length of 0.5-2μm, and a specific surface area of >200m 2 / g, tap density: 0.27g / cm 3 , true density: ~2.1g / cm3, conductivity:>100s / cm; composite high wear-resistant sand grain powder: Twax-4000, Nanjing Tianshi New Material Technology Co., Ltd.; bentonite: Hemmings LT-bentonite; polyamide pulp: Desbaron-AQ-630; polydimethoxysilane: PMX-10, Shanghai Hongzhuang Chemical Technology Co., Ltd.; polycaprolactone: weight average molecular weight is 30,000.
[0093] Example 1
[0094] 1. Preparation of modified filler:
[0095] The carbon nanotubes and 0.15 mol / L nitric acid solution were mixed in a mass ratio of 0.05:1000, and the mixture was immersed in a dark place at a temperature of 100°C for 30 minutes; after the treatment, the solid was dried to obtain acidified carbon nanotubes; 0.2 g of the acidified carbon nanotubes was added to 1 g of 3.5 mol / L ethyl orthosilicate aqueous solution, and then a 0.15 mol / L hydrochloric acid solution was added (the volume ratio of the hydrochloric acid solution to the ethyl orthosilicate aqueous solution was 0.1:1), and the mixture was stirred and mixed at 30°C and 450 rpm for 1 hour, and dibutyltin dilaurate was added. (the volume ratio of dibutyltin dilaurate to polydimethoxysilane is 1:3), continue stirring for 10 minutes, finally add polydimethoxysilane (the molar ratio of polydimethoxysilane to tetraethyl orthosilicate is 0.3:1), mix for another 10 minutes, then filter, and collect the filtered precipitate; dissolve 1g of polycaprolactone and 0.35g of epoxy resin in 50ml of ethyl acetate to obtain a suspension, add the above filtered precipitate to the suspension (the mass ratio of the filtered precipitate to the suspension is 1:0.01), ultrasonically treat at 500W for 1h, then filter, and dry the filtered solid to obtain a modified filler;
[0096] 2. Preparation of waterborne polyurethane prepolymer:
[0097] In a double-layer jacketed reactor equipped with a mechanical stirrer, add 25g of polycarbonate diol, heat to 100°C, stir evenly, then vacuum and remove water for 2h, cool to 45-55°C, slowly add 8g of IPDI, and after IPDI is completely added, raise the system temperature to 90°C, keep warm and stir for 2h to obtain a waterborne polyurethane prepolymer;
[0098] 3. Preparation of waterborne polyurethane dispersion:
[0099] Slowly add 1 g of anionic aminoalkylsulfonate chain extender containing hydrophilic groups to the above waterborne polyurethane prepolymer, continue to react at 90° C. for 5 h, adjust the R value, and add 12 g of N-ethylpyrrolidone to dilute the viscosity of the reaction system. Determine by di-n-butylamine titration that the reaction system reaches the theoretical content of chemical bond NCO groups, cool down, add triethylamine to adjust the pH of the reaction system to 7, continue to add deionized water to the reaction system under high-speed stirring to emulsify it, and finally obtain a waterborne polyurethane dispersion with a solid content of 38%;
[0100] 4. Preparation of super hydrophobic, wear-resistant water-based strippable varnish coating:
[0101] Fix the stirring rod of the high-speed disperser in the center of the dispersion container, and slowly add 15g of deionized water, 70g of aqueous polyurethane dispersion, 2g of modified filler, 0.3g of aqueous defoamer, 0.3g of aqueous polyether siloxane leveling agent, 0.4g of aqueous acetylene glycol wetting agent, 2g of lotus leaf hydrophobic agent, and 8g of aqueous film-forming aid in sequence at a stirring speed of 500 rpm, increase the stirring speed to 1000 rpm and disperse at high speed for 15 minutes, add 1.5g of aqueous associative polyurethane thickener and 0.5g of dimethylethanolamine, increase the stirring speed to 1200 rpm and continue to disperse for 30 minutes to obtain a super hydrophobic, wear-resistant water-based strippable varnish coating.
[0102] Example 2
[0103] 1. Preparation of modified filler:
[0104] The carbon nanotubes and 0.2 mol / L nitric acid solution were mixed in a mass ratio of 0.07:1000, and the mixture was immersed in a dark place at 100°C for 30 min. After the treatment, the solid was dried to obtain the acidified carbon nanotubes. 0.23 g of the acidified carbon nanotubes was added to 1 g of 3.5 mol / L ethyl orthosilicate aqueous solution, and then 0.1 mol / L hydrochloric acid solution was added (the volume ratio of the hydrochloric acid solution to the ethyl orthosilicate aqueous solution was 0.1:1), and the mixture was stirred at 30°C and 450 rpm for 1 h, and dibutyltin dilaurate ( The volume ratio of dibutyltin dilaurate to polydimethoxysilane is 1:3), and the stirring treatment is continued for 10 minutes. Finally, polydimethoxysilane (the molar ratio of polydimethoxysilane to tetraethyl orthosilicate is 0.4:1) is added, and mixed for another 10 minutes, and then filtered to collect the filtered precipitate; 1.2g of polycaprolactone and 0.35g of epoxy resin are dissolved in 50ml of ethyl acetate to obtain a suspension, and the filtered precipitate is added to the suspension (the mass ratio of the filtered precipitate to the suspension is 1:0.02), and ultrasonically treated at 500W for 1h, and then filtered. The filtered solid is dried to obtain a modified filler;
[0105] 2. Preparation of waterborne polyurethane prepolymer:
[0106] In a double-layer jacketed reactor equipped with a mechanical stirrer, add 30g of polycarbonate diol, heat to 100°C, stir evenly, then vacuum and remove water for 2h, cool to 50°C, slowly add 9wt% IPDI, and after IPDI is completely added, raise the system temperature to 90°C, keep warm and stir for 2h to obtain a waterborne polyurethane prepolymer;
[0107] 3. Preparation of waterborne polyurethane dispersion:
[0108] Slowly add 3g of anionic aminoalkylsulfonate chain extender containing hydrophilic group to the above waterborne polyurethane prepolymer, continue to react at 90°C for 5h, adjust the R value, and add 14gwt% N-ethylpyrrolidone to dilute the viscosity of the reaction system, and determine the reaction system to reach the theoretical content of chemical bond NCO groups by di-n-butylamine titration method, cool down, add triethylamine to adjust the pH of the reaction system to 7, and continue to add deionized water to the reaction system under high-speed stirring to emulsify it, and finally obtain a waterborne polyurethane dispersion with a solid content of 40g;
[0109] 4. Preparation of super hydrophobic, wear-resistant water-based strippable varnish coating:
[0110] Fix the stirring rod of the high-speed disperser in the center of the dispersion container, and slowly add 10g of deionized water, 75g of aqueous polyurethane dispersion, 3g of modified filler, 0.5g of aqueous defoamer, 0.5g of aqueous polyether siloxane leveling agent, 0.5g of aqueous acetylene glycol wetting agent, 1g of lotus leaf hydrophobic agent, and 7g of aqueous film-forming aid in sequence at a stirring speed of 500 rpm, increase the stirring speed to 1000 rpm and disperse at high speed for 15min, add 2g of aqueous associative polyurethane thickener and 0.5g of dimethylethanolamine, increase the stirring speed to 1200 rpm and continue to disperse for 30min to obtain a super-hydrophobic, wear-resistant water-based strippable varnish coating.
[0111] Example 3
[0112] 1. Preparation of modified filler:
[0113] The carbon nanotubes and 0.2 mol / L nitric acid solution were mixed in a mass ratio of 0.1:1000, and the mixture was immersed in a dark place at 100°C for 30 min. After the treatment, the solid was dried to obtain the acidified carbon nanotubes. 0.3 g of the acidified carbon nanotubes was added to 1 g of 3.5 mol / L ethyl orthosilicate aqueous solution, and then 0.1 mol / L hydrochloric acid solution was added (the volume ratio of the hydrochloric acid solution to the ethyl orthosilicate aqueous solution was 0.06:1), and the mixture was stirred at 30°C and 450 rpm for 1 h, and dibutyltin dilaurate (Dibutyltin dilaurate) was added. The volume ratio of dibutyltin cinnamate to polydimethoxysilane is 1:2), and the stirring treatment is continued for 10 minutes. Finally, polydimethoxysilane (the molar ratio of polydimethoxysilane to tetraethyl orthosilicate is 0.3:1) is added, and mixed for another 10 minutes, and then filtered to collect the filtered precipitate; S2: 1.5g polycaprolactone and 0.35g epoxy resin are dissolved in 50ml ethyl acetate to obtain a suspension, and the filtered precipitate is added to the suspension (the mass ratio of the filtered precipitate to the suspension is 1:0.03), ultrasonically treated at 400W for 2h, and then filtered. The filtered solid is dried to obtain a modified filler;
[0114] 2. Preparation of waterborne polyurethane prepolymer:
[0115] In a double-layer jacketed reactor equipped with a mechanical stirrer, add 30g of polycarbonate diol, heat to 100°C, stir evenly, then vacuum and remove water for 2h, cool to 40°C, slowly add 10g of IPDI, and after IPDI is completely added, raise the system temperature to 90°C, keep warm and stir for 2h to obtain a waterborne polyurethane prepolymer;
[0116] 3. Preparation of waterborne polyurethane dispersion:
[0117] Slowly add 2 g of anionic aminoalkylsulfonate chain extender containing hydrophilic groups to the above waterborne polyurethane prepolymer, continue to react at 90° C. for 5 h, adjust the R value, and add 15 g of N-ethylpyrrolidone to dilute the viscosity of the reaction system. Determine by di-n-butylamine titration that the reaction system reaches the theoretical content of chemical bond NCO groups, cool down, add triethylamine to adjust the pH of the reaction system to 7, continue to add deionized water to the reaction system under high-speed stirring to emulsify it, and finally obtain a waterborne polyurethane dispersion with a solid content of 40%;
[0118] 4. Preparation of super hydrophobic, wear-resistant water-based strippable varnish coating:
[0119] Fix the stirring rod of the high-speed disperser in the center of the dispersion container, and slowly add 13.5g of deionized water, 70g of aqueous polyurethane dispersion, 5g of modified filler, 0.5g of aqueous defoamer, 0.5g of aqueous polyether siloxane leveling agent, 0.5g of aqueous acetylene glycol wetting agent, 2g of lotus leaf hydrophobic agent, and 6g of aqueous film-forming aid in sequence at a stirring speed of 500 rpm, increase the stirring speed to 1000 rpm and disperse at high speed for 15min, add 1.5g of aqueous associative polyurethane thickener and 0.5g of dimethylethanolamine dropwise, increase the stirring speed to 1200 rpm and continue to disperse for 30min to obtain a super-hydrophobic, wear-resistant water-based strippable varnish coating.
[0120] Example 4
[0121] 1. Preparation of modified filler:
[0122] The carbon nanotubes and 0.1 mol / L nitric acid solution were mixed in a mass ratio of 0.1:1000, and the mixture was immersed in a dark place at 100°C for 30 min. After the treatment, the solid was dried to obtain the acidified carbon nanotubes. 0.4 g of the acidified carbon nanotubes was added to 1 g of 3.5 mol / L ethyl orthosilicate aqueous solution, and then a 0.15 mol / L hydrochloric acid solution was added (the volume ratio of the hydrochloric acid solution to the ethyl orthosilicate aqueous solution was 0.08:1), and the mixture was stirred at 30°C and 450 rpm for 1 h, and dibutyltin dilaurate (dibutyltin dilaurate) was added. The volume ratio of dibutyltin laurate to polydimethoxysilane is 1:3), and the stirring treatment is continued for 10 minutes. Finally, polydimethoxysilane (the molar ratio of polydimethoxysilane to tetraethyl orthosilicate is 0.3:1) is added, and mixed for 10 minutes, and then filtered to collect the filtered precipitate; S2: 1.5g polycaprolactone and 0.35g epoxy resin are dissolved in 50ml ethyl acetate to obtain a suspension, and the filtered precipitate is added to the suspension (the mass ratio of the filtered precipitate to the suspension is 1:0.025), ultrasonically treated at 500W for 1h, and then filtered. The filtered solid is dried to obtain a modified filler;
[0123] 2. Preparation of waterborne polyurethane prepolymer:
[0124] In a double-layer jacketed reactor equipped with a mechanical stirrer, add 30g of polycarbonate diol, heat to 100°C, stir evenly, then vacuum and remove water for 2h, cool to 50°C, slowly add 10g of IPDI, and after IPDI is completely added, raise the system temperature to 90°C, keep warm and stir for 2h to obtain a waterborne polyurethane prepolymer;
[0125] 3. Preparation of waterborne polyurethane dispersion:
[0126] Slowly add 3 g of anionic aminoalkylsulfonate chain extender containing hydrophilic groups to the above waterborne polyurethane prepolymer, continue to react at 90° C. for 5 h, adjust the R value, and add 15 g of N-ethylpyrrolidone to dilute the viscosity of the reaction system. Determine by di-n-butylamine titration that the reaction system reaches the theoretical content of chemical bond NCO groups, cool down, add triethylamine to adjust the pH of the reaction system to 7, continue to add deionized water to the reaction system under high-speed stirring to emulsify it, and finally obtain an aqueous polyurethane dispersion with a solid content of 40 g;
[0127] 4. Preparation of super hydrophobic, wear-resistant water-based strippable varnish coating:
[0128] Fix the stirring rod of the high-speed disperser in the center of the dispersion container, and slowly add 10g of deionized water, 72.9g of aqueous polyurethane dispersion, 4.5g of modified filler, 0.4g of aqueous defoamer, 0.4g of aqueous polyether siloxane leveling agent, 0.4g of aqueous acetylene glycol wetting agent, 2g of lotus leaf hydrophobic agent, and 7g of aqueous film-forming aid in sequence at a stirring speed of 500 rpm, increase the stirring speed to 1000 rpm and disperse at high speed for 15min, add 2g of aqueous associative polyurethane thickener and 0.4g of dimethylethanolamine dropwise, increase the stirring speed to 1200 rpm and continue to disperse for 30min to obtain a super-hydrophobic, wear-resistant water-based strippable varnish coating.
[0129] Example 5
[0130] 1. Preparation of modified filler:
[0131] The carbon nanotubes and 0.1 mol / L nitric acid solution were mixed in a mass ratio of 0.1:1000, and the mixture was immersed in a dark place at 100°C for 30 min. After the treatment, the solid was dried to obtain the acidified carbon nanotubes. 0.4 g of the acidified carbon nanotubes was added to 1 g of 3.5 mol / L ethyl orthosilicate aqueous solution, and then a 0.15 mol / L hydrochloric acid solution was added (the volume ratio of the hydrochloric acid solution to the ethyl orthosilicate aqueous solution was 0.08:1), and the mixture was stirred at 30°C and 450 rpm for 1 h, and dibutyltin dilaurate (dibutyltin dilaurate) was added. The volume ratio of dibutyltin laurate to polydimethoxysilane is 1:3), and the stirring treatment is continued for 10 minutes. Finally, polydimethoxysilane (the molar ratio of polydimethoxysilane to tetraethyl orthosilicate is 0.3:1) is added, and mixed for 10 minutes, and then filtered to collect the filtered precipitate; S2: 1.5g polycaprolactone and 0.35g epoxy resin are dissolved in 50ml ethyl acetate to obtain a suspension, and the filtered precipitate is added to the suspension (the mass ratio of the filtered precipitate to the suspension is 1:0.025), ultrasonically treated at 500W for 1h, and then filtered. The filtered solid is dried to obtain a modified filler;
[0132] 2. Preparation of waterborne polyurethane prepolymer:
[0133] In a double-layer jacketed reactor equipped with a mechanical stirrer, add 30g of polycarbonate diol, heat to 100°C, stir evenly, then vacuum and remove water for 2h, cool to 50°C, slowly add 10g of IPDI, and after IPDI is completely added, raise the system temperature to 90°C, keep warm and stir for 2h to obtain a waterborne polyurethane prepolymer;
[0134] 3. Preparation of waterborne polyurethane dispersion:
[0135] Slowly add 3 g of anionic aminoalkylsulfonate chain extender containing hydrophilic groups to the above waterborne polyurethane prepolymer, continue to react at 90° C. for 5 h, adjust the R value, and add 15 g of N-ethylpyrrolidone to dilute the viscosity of the reaction system. Determine by di-n-butylamine titration that the reaction system reaches the theoretical content of chemical bond NCO groups, cool down, add triethylamine to adjust the pH of the reaction system to 7, continue to add deionized water to the reaction system under high-speed stirring to emulsify it, and finally obtain an aqueous polyurethane dispersion with a solid content of 40 g;
[0136] 4. Preparation of color paste:
[0137] Add 10g of deionized water to the stirring container, fix the stirring rod of the high-speed disperser in the center of the dispersion container, slowly add 0.4g of aqueous defoamer and 0.4g of aqueous acetylene glycol wetting agent in sequence at a stirring speed of 500 rpm, increase the stirring speed to 1000 rpm and disperse at high speed for 5 minutes, reduce the stirring speed of the disperser to 500 rpm, add 3.6g of composite high wear-resistant sand grain powder, 4.5g of 1250 mesh silicon powder, 4.5g of rutile titanium dioxide, 0.09g of medium pigment carbon black powder, 0.45g of bentonite, and 0.45g of polyamide pulp, increase the stirring speed to 1500 rpm and disperse for 30 minutes, then put it into a sand mill and grind it to a fineness of ≤15um, which is qualified to obtain a water-based resin-free ice gray slurry;
[0138] 5. Preparation of super hydrophobic, wear-resistant water-based peelable ice-gray surface coating:
[0139] The above-mentioned color paste is added into a stirring kettle, and then 59.31g of the above-prepared aqueous polyurethane dispersion, 4.5g of modified filler, 0.4g of dimethylethanolamine, 0.4g of aqueous polyether siloxane leveling agent, 2g of lotus leaf hydrophobic agent, and 7g of aqueous film-forming aid are added into the stirring kettle at 500 rpm, and the stirring speed is increased to 1000 rpm for high-speed dispersion for 15 minutes, 2g of aqueous associative polyurethane thickener is added dropwise, and the stirring speed is increased to 1200 rpm for continued dispersion for 30 minutes to obtain a super hydrophobic, wear-resistant water-based strippable ice-gray surface coating.
[0140] Comparative Example 1
[0141] Compared with Example 1, the difference is that no modified filler is added in this comparative example, and other conditions are the same as those in Example 1.
[0142] Comparative Example 2
[0143] Compared with Example 1, the difference is that in this comparative example, when preparing the modified filler, no acidified carbon nanotubes are added, and other conditions are the same as those in Example 1.
[0144] Comparative Example 3
[0145] Compared with Example 1, the difference is that in this comparative example, when preparing the modified filler, the PDMS layer and the polycaprolactone / epoxy resin layer are not modified, and other conditions are the same as those in Example 1.
[0146] Comparative Example 4
[0147] Compared with Example 1, the difference is that when preparing the modified filler, only the PDMS layer is modified, and the polycaprolactone / epoxy resin layer is not modified. Other conditions are the same as those in Example 1.
[0148] Comparative Example 5
[0149] Compared with Example 1, the difference is that when preparing the modified filler, only the polycaprolactone / epoxy resin layer is modified, and the PDMS layer is not modified. Other conditions are the same as those in Example 1.
[0150] The coatings obtained in the above embodiments and comparative examples were tested for performance, and the test methods and test results are as follows:
[0151] The sample substrate used in the experiment is a 150mm×70mm×2mm tinplate. The surface of the substrate needs to be treated before the experiment: first, use sandpaper of moderate coarseness and fineness to grind the iron plate horizontally and vertically, then wipe the polished surface with xylene, and finally wipe it clean with anhydrous ethanol and put it in a vacuum drying oven for drying. Before spraying, adjust the air output of the spray gun, place the iron plate in the fume hood, turn on the fan and water curtain box, keep the distance between the spray gun and the iron plate appropriate, and then use the spray gun to spray the sample substrate with an "S" shape. The number of sprays for each sample plate is the same to ensure that the spray thickness of the coating sample is consistent, and the film thickness is controlled to be 30μm. After spraying, wait for the sample surface to dry and place it in a ventilated place for drying.
[0152] Water contact angle: tested according to the method of national standard GB / T 23744-2009.
[0153] Peelability test: During the period from December to May of the following year in northern China, the samples were placed in an open-air outdoor environment for 6 months, and then torn by hand to check whether the film layer can be completely removed.
[0154] Wear resistance: GB / T1768, test conditions: 60r / min, load 1000g, CS-10 grinding wheel.
[0155] Tensile strength: A 100N force sensor (Instron 5567A, USA) was used to perform the tensile test on a material testing machine. A constant strain rate of 50 mm / min was used. To ensure data accuracy, each sample was tested at least 3 times.
[0156] The test results are shown in Table 1.
[0157] Table 1
[0158]
[0159] It can be seen from the data in Table 1 above that, compared with the comparative example, the present invention adds an appropriate amount of filler to the coating and performs certain treatment on the filler. The prepared coating not only has good hydrophobicity, but also has excellent wear resistance, good mechanical properties and good stripping effect.
[0160] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.
Claims
1. A method for preparing a super hydrophobic, wear-resistant water-based peelable coating, characterized in that: The following steps are involved: (1) heating the diol, then vacuuming to remove water, then cooling, adding diisocyanate, and heating to react to obtain a waterborne polyurethane prepolymer; (2) preparing a waterborne polyurethane dispersion using an anionic aminoalkylsulfonate containing a hydrophilic group as a chain extender; (3) mixing the aqueous polyurethane dispersion with a modified filler, an aqueous defoamer, an aqueous leveling agent, an aqueous wetting agent, a hydrophobic agent, an aqueous film-forming aid, a thickener, and deionized water, and adding a pH adjuster to adjust the pH to obtain a super-hydrophobic surface water-based strippable coating; The modified filler is a polymer-coated SiO2 / carbon nanotube composite filler, and the coating layer is a polydimethoxysilane layer and a polycaprolactone / epoxy resin layer from the inside to the outside.
2. A method for preparing a super hydrophobic, wear-resistant water-based strippable coating according to claim 1, characterized in that: In step (1), at least one of the following features is included: The diol is a polycarbonate diol; The diisocyanate is isophorone diisocyanate; Heat the diol to 100-110°C; The time for vacuuming and removing water is 1-2h; The cooling temperature is 45-55℃; The temperature of the temperature-raising reaction is 85-95° C. and the time is 1-2 hours.
3. A method for preparing a super-hydrophobic, wear-resistant water-based strippable coating according to claim 1, characterized in that: In step (2), the preparation process of the aqueous polyurethane dispersion is specifically as follows: adding anionic aminoalkylsulfonate containing hydrophilic groups as a chain extender to the aqueous polyurethane prepolymer, continuing the reaction, adjusting the R value, and adding a reactive diluent at the same time, until the reaction system reaches the theoretical content of chemical bond NCO groups, cooling, and adding a salt-forming agent to the reaction system, and adding deionized water under stirring conditions to adjust the solid content, so as to obtain the aqueous polyurethane dispersion; the amounts of the components used are respectively as follows: 25-35wt% of diol, 8-10wt% of diisocyanate, 1-3wt% of chain extender, 12-15wt% of reactive diluent, 0.5-1.5wt% of salt-forming agent, and 40-50wt% of deionized water.
4. A method for preparing a super hydrophobic, wear-resistant water-based strippable coating according to claim 3, characterized in that: The preparation of the waterborne polyurethane dispersion includes at least one of the following characteristics: The active diluent is N-ethylpyrrolidone; The salt-forming agent is triethylamine; The reaction time is 4-6 hours. The solid content of the aqueous polyurethane dispersion is 35-40%.
5. A method for preparing a super hydrophobic, wear-resistant water-based strippable coating according to claim 3, characterized in that: The preparation method of the modified filler comprises the following steps: S1: acidifying the carbon nanotubes to obtain acidified carbon nanotubes, adding the acidified carbon nanotubes to an aqueous solution of ethyl orthosilicate, then adding a hydrochloric acid solution, stirring and mixing, adding dibutyltin dilaurate and continuing to stir, finally adding polydimethoxysilane, mixing again, filtering, and collecting the filtered precipitate; S2: dissolving polycaprolactone and epoxy resin in ethyl acetate to obtain a suspension, adding the filtered precipitate to the suspension, ultrasonically treating, filtering, and drying the filtered solid to obtain a modified filler.
6. A method for preparing a super hydrophobic, wear-resistant water-based strippable coating according to claim 5, characterized in that: In step S1, the conditions for the acidification treatment include at least one of the following characteristics: A nitric acid solution with a concentration of 0.1-0.2 mol / L is used for acidification treatment; During the acidification treatment, the mass ratio of carbon nanotubes to solution is (0.05-0.1):1000; The temperature during acidification treatment is 100-110°C and the treatment time is 30-60 minutes; The concentration of the tetraethyl orthosilicate aqueous solution is 3-4 mol / L, and the mass ratio of the acidified carbon nanotubes to the tetraethyl orthosilicate aqueous solution is (0.1-0.5):1; The concentration of the hydrochloric acid solution is 0.1-0.2 mol / L, and the volume ratio of the hydrochloric acid solution to the ethyl orthosilicate aqueous solution is (0.05-0.1):1; The volume ratio of dibutyltin dilaurate to polydimethoxysilane is 1:(2-4), and the molar ratio of polydimethoxysilane to tetraethyl orthosilicate is (0.1-0.5):1; The stirring and mixing temperature is 30° C., the time is 1-2 hours, and the stirring speed is 400-500 rpm; the time for continuing the stirring treatment is 10-20 minutes; and the time for re-mixing is 10-20 minutes.
7. A method for preparing a super-hydrophobic, wear-resistant water-based strippable coating according to claim 5, characterized in that: S2 includes at least one of the following characteristics: In the suspension, the concentrations of polycaprolactone and epoxy resin are 0.02-0.03 g / ml and 0.007-0.008 g / ml respectively; the mass ratio of filtered precipitate to suspension is 1:(0.01-0.03); The power of the ultrasonic treatment is 400-500 W, and the time of the ultrasonic treatment is 1-2 h.
8. The method for preparing a super-hydrophobic, wear-resistant water-based strippable coating according to claim 1, characterized in that: The hydrophobic agent is a lotus leaf hydrophobic agent; the aqueous defoaming agent is a mixture of one or more aqueous polyether siloxane defoaming agents, aqueous mineral oil defoaming agents, and aqueous polymer polyether defoaming agents; the aqueous leveling agent is an aqueous polyether siloxane leveling agent; the aqueous wetting agent is an aqueous acetylene glycol wetting agent; the aqueous film-forming aid is one of dipropylene glycol butyl ether and dipropylene glycol phenyl ether; the thickener is an aqueous associative polyurethane thickener; and the pH adjuster is dimethylethanolamine.
9. A method for preparing a super hydrophobic, wear-resistant water-based strippable coating according to claim 1, characterized in that: The amounts of the components in the hydrophobic surface water-based strippable coating are as follows, in percentage by mass: 70-85wt% of water-based polyurethane dispersion, 2-5wt% of modified filler, 8-15wt% of deionized water, 0.1-0.5wt% of water-based defoamer, 0.1-0.5wt% of water-based polyether siloxane leveling agent, 0.1-0.5wt% of water-based acetylene glycol wetting agent, 0.5-2wt% of water-based oxidized polyethylene wax lotus leaf hydrophobic agent, 3-8wt% of water-based film-forming aid, 1-2wt% of water-based associative polyurethane thickener, and 0.3-0.5wt% of pH regulator.
10. The method for preparing a super-hydrophobic, wear-resistant water-based strippable coating according to claim 9, characterized in that: Pigments and fillers are also added to the coating to replace part of the aqueous polyurethane dispersion, the mass ratio of the pigments and fillers to the aqueous polyurethane dispersion is (1-5):5, and the total addition amount of the pigments and fillers and the aqueous polyurethane dispersion is 70-85wt% of the coating mass; the pigments and fillers include composite high-wear-resistant sand-texture powder, 1250-mesh silicon micropowder, rutile titanium dioxide, medium-pigment carbon black powder, bentonite, and polyamide pulp, and the mass ratio of the composite high-wear-resistant sand-texture powder, 1250-mesh silicon micropowder, rutile titanium dioxide, medium-pigment carbon black powder, bentonite, and polyamide pulp is 5-8:10-15:10-12:0.2-0.5:1-2:1-2.
Citation Information
Patent Citations
Preparation method of carbon nanotube-loaded nano silver wire modified polyurethane antistatic emulsion
CN110643016A
Super-hydrophobic coating and preparation method and application thereof, and super-hydrophobic coating and preparation method and application thereof
CN114106676A
Preparation method of waterborne epoxy modified organic silicon high-temperature-resistant anticorrosive paint
CN116285679A
Cited By
Polyurethane wear-resistant and corrosion-resistant film for front edge of wind power blade and preparation method thereof
CN119242021A