A kind of aging-resistant rubber material for sealing ring and preparation method thereof

By introducing load-bearing plasticizers and antioxidants into rubber materials for sealing rings, the material's insufficient performance in high temperature and extremely cold environments and the problem of silica agglomeration are solved, significantly improving cold resistance, thermal stability and mechanical properties. performance, improving the material’s aging resistance.

CN118325210BActive Publication Date: 2024-10-11YANGZHOU SAIPUREN RUBBER & PLASTIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410617396.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-17
Publication Date
2024-10-11
Estimated Expiration
2044-05-17

AI Technical Summary

Technical Problem

Existing rubber materials for sealing rings have poor performance in high temperature and extremely cold environments, and the agglomeration of silica in the rubber matrix affects mechanical properties. Insufficient solubility of antioxidants leads to ‘blooming phenomenon’, damaging material properties.

Method used

It uses a combination of nitrile rubber, polyacrylate rubber, plasticizer, antioxidant, carbon black, zeolite powder, paraffin, zinc oxide, sulfur and accelerator, in which the plasticizer is loaded on the white carbon black and the antioxidant is loaded On halloysite nanotubes, the material properties are improved through structures such as ester groups, ether groups and polysiloxane chains.

Benefits of technology

It improves the cold resistance, thermal stability and mechanical properties of the rubber material, reduces the agglomeration of silica black, suppresses the 'blooming phenomenon', and significantly improves the material's aging resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004845708210000141
    Figure BDA0004845708210000141
  • Figure BDA0004845708210000151
    Figure BDA0004845708210000151
Patent Text Reader

Abstract

The invention discloses a kind of anti-aging rubber material for sealing ring, including the following raw materials by weight: 70-100 parts of nitrile rubber, 30-50 parts of polyacrylate rubber, 10-15 parts of plasticizer, 1-2 parts of antioxidant, 25-35 parts of carbon black, 5-10 parts of zeolite powder, 0.5-1.0 parts of paraffin, 2-3 parts of stearic acid, 3-5 parts of zinc oxide, 2-3 parts of sulfur and 1-2 parts of accelerator. The synthesized plasticizer is obtained by loading a compound containing an ester group, an ether group, a methylene group and a polysiloxane chain on white carbon black, and the cold resistance, thermal stability and mechanical properties of the rubber material are improved. The synthesized antioxidant is obtained by loading a compound containing a dimethyl acridine structure and a benzotriazole structure into halloysite nanotubes, and the aging resistance, weather resistance, thermal stability and mechanical properties of the rubber material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rubber materials, and in particular to an aging-resistant rubber material for a sealing ring and a preparation method thereof. Background Art

[0002] Nitrile rubber is an important component of rubber materials and is widely used in the field of rubber materials for sealing rings. It has good high temperature resistance and oil resistance, but its structure contains unsaturated olefin segments, which leads to its poor brittleness and aging resistance, which is not conducive to long-term use. Therefore, it is necessary to add plasticizers to improve its processing performance. Most of the rubber materials in the prior art have high high temperature resistance. In order to meet the use requirements, higher requirements are put forward for the heat resistance of the plasticizers used in the rubber materials for sealing rings. In addition, in actual use, especially in extremely cold areas, the elasticity of the rubber material will continue to decrease and the hardness will continue to increase as the temperature of the working environment decreases, until it completely loses its elasticity below a certain temperature, thereby losing its use value. Therefore, it is necessary to improve the cold resistance of the rubber material for sealing rings.

[0003] As a commonly used reinforcing filler in rubber materials, white carbon black is easy to aggregate on the surface of the rubber matrix due to its large specific surface area and a large number of hydroxyl functional groups on the surface, which affects the mechanical properties of the rubber. It is necessary and important to modify white carbon black. In order to inhibit the aging of rubber caused by light, heat, oxygen, ozone, etc., antioxidants are usually added to the matrix. In actual use, the existing antioxidants may cause "frosting" due to insufficient solubility in the matrix, which damages the performance of the rubber material. Appropriate modification methods are needed to solve the problems encountered in actual use. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides an aging-resistant rubber material for a sealing ring and a preparation method thereof.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] An anti-aging rubber material for a sealing ring, comprising the following raw materials in parts by weight: 70-100 parts of nitrile rubber, 30-50 parts of polyacrylate rubber, 10-15 parts of plasticizer, 1-2 parts of antioxidant, 25-35 parts of carbon black, 5-10 parts of zeolite powder, 0.5-1.0 parts of paraffin, 2-3 parts of stearic acid, 3-5 parts of zinc oxide, 2-3 parts of sulfur and 1-2 parts of accelerator;

[0007] The accelerator is 2-mercaptobenzothiazole;

[0008] The preparation of the plasticizer comprises the following steps:

[0009] Step A1: In a nitrogen atmosphere, add adipic acid and methanol into a round-bottom flask, start stirring, raise the temperature to 40-50° C., add pyridine and glycidyl acrylate, and react with constant temperature stirring for 9-10 hours to obtain reaction product 1;

[0010] Further, the usage ratio of adipic acid, methanol, pyridine and glycidyl acrylate is 0.1 mol: 200-220 mL: 0.001-0.0012 mol: 0.2 mol;

[0011] During the reaction of step A1, the carboxyl group of adipic acid and the epoxy group of glycidyl acrylate undergo ring-opening to generate a reaction product 1.

[0012] Step A2: Add (2-n-butoxyethoxy)acetic acid to DMF, start stirring, slowly add thionyl chloride, raise the temperature to 40-50°C, stir and react at constant temperature for 4-5h, filter, extract and dry to obtain the acyl chloride product;

[0013] Further, the usage ratio of (2-n-butoxyethoxy)acetic acid, DMF and thionyl chloride is 0.1 mol:150 mL:0.1-0.15 mol;

[0014] During the reaction of step A2, (2-n-butoxyethoxy)acetic acid reacts with thionyl chloride to generate an acyl chloride product;

[0015] Step A3: Add the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution a, then add the above-mentioned acyl chloride product into dimethyl sulfoxide to obtain a mixed solution b, slowly dropwise add the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropwise addition is completed, heat to 40°C, react at constant temperature for 8-10 hours, and distill under reduced pressure to obtain a reaction product 2;

[0016] Further, the usage ratio of the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide is 0.2 mol: 0.01-0.015 mol: 0.2 mol: 70-80 mL; the usage ratio of the acyl chloride product and dimethyl sulfoxide is 0.1 mol: 20-30 mL;

[0017] During the reaction of step A3, the hydroxyl group of the reaction product 1 reacts with the acyl chloride product to generate the reaction product 2;

[0018] Step A4: Add toluene, hydrogen-containing silicone oil, hydroquinone, and cis-dichlorobis(pyridyl)platinum into a three-necked flask, stir and introduce nitrogen protection, slowly add reaction product 2, raise the temperature to 70-80° C., and stir for reaction for 3-4 hours to obtain reaction product 3; add white carbon black into a high-speed stirrer, start stirring, add the reaction product three times in equal amounts into a reactor, stir at room temperature and a stirring frequency of 20 Hz for 20-30 minutes to obtain a product, then place the product in an oven, dry at 60° C. for 30 minutes, and then put it into a sealed bag and store at room temperature to obtain a plasticizer;

[0019] Further, the amount ratio of reaction product 2, toluene, hydrogenated silicone oil, hydroquinone and cis-dichlorobis(pyridyl)platinum is 1-1.5 mol: 100 ml: 1 mol: 0.5 mol: 0.015-0.020 mol; the amount ratio of white carbon black and reaction product 3 is 4-5 g: 2-3 g;

[0020] During the reaction process of step A4, the hydrogen-containing silicone oil reacts with the reaction product 2 under the catalysis of cis-dichlorobis(pyridyl)platinum, and the Si-H bond and the C=C bond are added to generate the reaction product 3; the reaction product 3 is then loaded on the surface of the white carbon black with large specific surface area and porosity to obtain a plasticizer.

[0021] The preparation of the antioxidant comprises the following steps:

[0022] Step B1: 3-nitro-2-(phenylamino)benzoic acid is added to tetrahydrofuran, nitrogen is introduced, reflux stirring is started, the temperature is raised to 50-60°C, and methylmagnesium chloride is added dropwise. After the addition is complete, the reaction is continued for 4-5 hours, water is added to quench, and the reaction product a is obtained by rotary evaporation, extraction, and drying;

[0023] Further, the usage ratio of 3-nitro-2-(phenylamino)benzoic acid, tetrahydrofuran and methylmagnesium chloride is 1 mol:48 mL:6.5 mol;

[0024] During the reaction of step B1, the carboxyl group of 3-nitro-2-(phenylamino)benzoic acid reacts with methylmagnesium chloride to generate a reaction product a containing an alcoholic hydroxyl group;

[0025] Step B2: Add molecular sieve, reaction product a and toluene to a reaction bottle, control the temperature to 20°C, stir and react at constant temperature for 2-3h, filter, distill under reduced pressure and recrystallize to obtain reaction product b; then add reaction product b to ethanol, start stirring, introduce nitrogen, then add Pd / C and hydrazine hydrate, stir and react at room temperature for 7-8h to obtain reaction product c;

[0026] Further, the molecular sieve, reaction product a and toluene are used in a ratio of 2.14 g: 0.9 mol: 610-620 mL, and the molecular sieve is a zeolite molecular sieve; the reaction product b, ethanol, Pd / C and hydrazine hydrate are used in a ratio of 0.1 mol: 90-100 mL: 0.001-0.0015 g: 0.1 mol;

[0027] During the reaction of step B2, the alcoholic hydroxyl group of the reaction product a undergoes a coupling reaction with the para-phenyl group of the connected benzene ring to generate a reaction product b containing a dimethylacridine structure; then, the nitro group of the reaction product b is reduced to an amino group to obtain a reaction product c;

[0028] Step B3: Add 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid to DMF, start stirring, slowly add dichlorothionyl, reflux and stir at 50°C for 4-5h to obtain reaction product d; add reaction product c, potassium carbonate and dimethyl sulfoxide to a flask to obtain mixed solution 1; then add reaction product d to dimethyl sulfoxide to obtain mixed solution 2, slowly dropwise add mixed solution 2 to mixed solution 1 under an ice-water bath, after the dropwise addition is completed, heat to 40°C, react at constant temperature for 6-7h, and distill under reduced pressure to obtain reaction product e;

[0029] Further, the amount ratio of 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid, DMF and dichlorothionyl is 0.1 mol: 150 mL: 0.1-0.15 mol; the amount ratio of reaction product c, potassium carbonate and dimethyl sulfoxide is 0.1 mol: 0.012-0.015 mol: 80-90 mL; the amount ratio of reaction product d and dimethyl sulfoxide is 0.1 mol: 10-20 mL;

[0030] In the reaction process of step B3, 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid reacts with thionyl chloride to generate a reaction product d containing an acyl chloride; the reaction product d containing an acyl chloride then reacts with the amino group of the reaction product c to generate a reaction product e;

[0031] Step B4: adding the reaction product e to acetone, stirring for 20-30 minutes to obtain a mixed solution, then pouring the halloysite nanotube powder into the mixed solution, continuing to stir for 1-1.5 hours, opening the vent valve and starting the vacuum pump at the same time, continuously evacuating for 30-40 minutes, then closing the vent valve, turning off the vacuum pump, and keeping the solution stirred for 15 minutes to break the vacuum, the reaction product e is loaded on the halloysite nanotubes, and an antioxidant is obtained;

[0032] Further, the amount ratio of the reaction product e, acetone and halloysite nanotube powder is 10 g: 100 mL: 6.5-7.0 g, and the above vacuuming and breaking operations are repeated 3 times;

[0033] During the reaction of step B4, after vacuuming, the lumen of the halloysite nanotube is in a vacuum state. After the vacuum is broken, the mixed liquid enters the lumen of the halloysite nanotube under the action of atmospheric pressure, so that the reaction product e in the mixed liquid is loaded into the halloysite nanotube to obtain an antioxidant.

[0034] Beneficial effects of the invention: The invention discloses an anti-aging rubber material for a sealing ring, comprising the following raw materials: nitrile rubber, polyacrylate rubber, plasticizer, antioxidant, carbon black, zeolite powder, paraffin, stearic acid, zinc oxide, sulfur and accelerator. The synthesized plasticizer is obtained by loading the reaction product 3 on white carbon black, and contains ester group, ether group, methylene group and polysiloxane chain. The polar ester group can interact with the cyano polar group in the nitrile rubber molecule, weakening the polar force between the nitrile rubber molecular chains; the presence of the extremely flexible polysiloxane chain, ether group and the flexible polymethylene fatty carbon chain plays an isolating and shielding role between the nitrile rubber molecular chains, further weakening the interaction between the rubber molecular chains, having a good plasticizing effect, making the rubber molecular segments easier to slide freely, resulting in a lower glass transition temperature and improving the cold resistance of the rubber material; the polysiloxane chain has a high thermal stability, which helps the plasticizer maintain structural stability in a high temperature environment, can better play a role in improving the performance of the rubber material and improve the thermal stability of the rubber material; the white carbon black nanoparticles loaded with the reaction product 3 are physically isolated by the reaction product 3, reducing the agglomeration of white carbon black in the rubber material and improving the mechanical properties of the rubber material.

[0035] The synthesized antioxidant is obtained by loading the reaction product e into the halloysite nanotube, which contains a dimethyl acridine structure and a benzotriazole structure. The dimethyl acridine structure has good resistance to heat aging, oxygen aging and flexural aging, and has a positive effect on improving the aging resistance of rubber materials. Amine antioxidants such as dimethyl acridine structures containing secondary amines have high solubility in polar nitrile rubber, which helps to inhibit the "blooming phenomenon". Benzotriazole has a wide range of ultraviolet absorption properties, which improves the light stability of rubber materials. Its synergistic use with amine antioxidants such as dimethyl acridine structures that have free radical capture properties helps to improve the weather resistance and thermal stability of rubber materials. Halloysite nanotubes have a special tube wall structure and a certain amount of gas in the tube cavity, so that after loading the reaction product e, the reaction product e has the effect of slowly releasing it from the halloysite nanotubes, further inhibiting the "blooming phenomenon" and making the rubber material have better aging resistance. Halloysite nanotubes have a large modulus, high strength and a nanotube structure, which has a positive effect on improving the mechanical properties of rubber materials. DETAILED DESCRIPTION

[0036] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Example 1

[0038] A plasticizer, the preparation of which comprises the following steps:

[0039] Step A1: In a nitrogen atmosphere, adipic acid and methanol were added into a round-bottom flask, stirring was started, the temperature was raised to 40°C, pyridine and glycidyl acrylate were added, and the reaction was stirred at a constant temperature for 9 hours to obtain reaction product 1; the amount ratio of adipic acid, methanol, pyridine and glycidyl acrylate was 0.1 mol: 200 mL: 0.001 mol: 0.2 mol;

[0040] Step A2: Add (2-n-butoxyethoxy)acetic acid to DMF, start stirring, slowly add thionyl chloride, raise the temperature to 40°C, stir and react for 4 hours at constant temperature, filter, extract and dry to obtain an acyl chloride product; the dosage ratio of (2-n-butoxyethoxy)acetic acid, DMF and thionyl chloride is 0.1 mol:150 mL:0.1 mol;

[0041] Step A3: adding the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution a, then adding the above-mentioned acyl chloride product into dimethyl sulfoxide to obtain a mixed solution b, slowly dropping the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropping is completed, heating to 40°C, reacting at a constant temperature for 8h, and distilling under reduced pressure to obtain a reaction product 2; the amount ratio of the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide is 0.2mol:0.01mol:0.2mol:70mL; the amount ratio of the acyl chloride product and dimethyl sulfoxide is 0.1mol:20mL;

[0042] Step A4: Add toluene, hydrogen-containing silicone oil, hydroquinone, and cis-dichlorobis(pyridyl)platinum into a three-necked flask, stir and introduce nitrogen protection, slowly add reaction product 2, heat to 70°C, and stir for reaction for 3 hours to obtain reaction product 3; add white carbon black into a high-speed stirrer, start stirring, add 3 equal amounts of the reaction product into a reactor three times, stir for 20 minutes at room temperature and a stirring frequency of 20 Hz to obtain a product, then place the product in an oven, dry at 60°C for 30 minutes, and then store in a sealed bag at room temperature to obtain a plasticizer; the amount ratio of reaction product 2, toluene, hydrogen-containing silicone oil, hydroquinone and cis-dichlorobis(pyridyl)platinum is 1 mol:100 ml:1 mol:0.5 mol:0.015 mol; the amount ratio of white carbon black and reaction product 3 is 4 g:2 g.

[0043] Example 2

[0044] A plasticizer, the preparation of which comprises the following steps:

[0045] Step A1: In a nitrogen atmosphere, adipic acid and methanol were added into a round-bottom flask, stirring was started, the temperature was raised to 45°C, pyridine and glycidyl acrylate were added, and the mixture was stirred at a constant temperature for 9.5 hours to obtain reaction product 1; the amount ratio of adipic acid, methanol, pyridine and glycidyl acrylate was 0.1 mol: 210 mL: 0.0011 mol: 0.2 mol;

[0046] Step A2: Add (2-n-butoxyethoxy)acetic acid to DMF, start stirring, slowly add dithionyl chloride, raise the temperature to 45°C, stir and react for 4.5 hours at constant temperature, filter, extract and dry to obtain an acyl chloride product; the dosage ratio of (2-n-butoxyethoxy)acetic acid, DMF and dithionyl chloride is 0.1 mol:150 mL:0.13 mol;

[0047] Step A3: adding the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution a, then adding the above-mentioned acyl chloride product into dimethyl sulfoxide to obtain a mixed solution b, slowly dropping the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropping is completed, heating to 40°C, reacting at constant temperature for 9 hours, and distilling under reduced pressure to obtain a reaction product 2; the amount ratio of the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide is 0.2 mol: 0.013 mol: 0.2 mol: 75 mL; the amount ratio of the acyl chloride product and dimethyl sulfoxide is 0.1 mol: 25 mL;

[0048] Step A4: Add toluene, hydrogen-containing silicone oil, hydroquinone, and cis-dichlorobis(pyridyl)platinum into a three-necked flask, stir and introduce nitrogen protection, slowly add reaction product 2, heat to 75°C, and stir for reaction for 3.5 hours to obtain reaction product 3; add white carbon black into a high-speed stirrer, start stirring, add 3 equal amounts of the reaction product into a reactor three times, stir for 25 minutes at room temperature and a stirring frequency of 20 Hz to obtain a product, then place the product in an oven, dry at 60°C for 30 minutes, and then store in a sealed bag at room temperature to obtain a plasticizer; the amount ratio of reaction product 2, toluene, hydrogen-containing silicone oil, hydroquinone and cis-dichlorobis(pyridyl)platinum is 1.2 mol:100 ml:1 mol:0.5 mol:0.017 mol; the amount ratio of white carbon black and reaction product 3 is 4.5 g:2.5 g.

[0049] Example 3

[0050] A plasticizer, the preparation of which comprises the following steps:

[0051] Step A1: In a nitrogen atmosphere, adipic acid and methanol were added into a round-bottom flask, stirring was started, the temperature was raised to 50°C, pyridine and glycidyl acrylate were added, and the reaction was stirred at a constant temperature for 10 hours to obtain reaction product 1; the amount ratio of adipic acid, methanol, pyridine and glycidyl acrylate was 0.1 mol: 220 mL: 0.0012 mol: 0.2 mol;

[0052] Step A2: Add (2-n-butoxyethoxy)acetic acid to DMF, start stirring, slowly add thionyl chloride, raise the temperature to 50°C, stir and react for 5 hours at constant temperature, filter, extract and dry to obtain an acyl chloride product; the dosage ratio of (2-n-butoxyethoxy)acetic acid, DMF and thionyl chloride is 0.1 mol:150 mL:0.15 mol;

[0053] Step A3: adding the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution a, then adding the above-mentioned acyl chloride product into dimethyl sulfoxide to obtain a mixed solution b, slowly dropping the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropping is completed, heating to 40°C, reacting at a constant temperature for 10 hours, and distilling under reduced pressure to obtain a reaction product 2; the amount ratio of the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide is 0.2 mol: 0.015 mol: 0.2 mol: 80 mL; the amount ratio of the acyl chloride product and dimethyl sulfoxide is 0.1 mol: 30 mL;

[0054] Step A4: Add toluene, hydrogen-containing silicone oil, hydroquinone, and cis-dichlorobis(pyridyl)platinum into a three-necked flask, stir and introduce nitrogen protection, slowly add reaction product 2, heat to 80°C, stir and react for 4 hours to obtain reaction product 3; add white carbon black into a high-speed stirrer, start stirring, add 3 equal amounts of the reaction product into a reactor three times, stir for 30 minutes at room temperature and a stirring frequency of 20 Hz to obtain a product, then place the product in an oven, dry at 60°C for 30 minutes, and then store in a sealed bag at room temperature to obtain a plasticizer; the amount ratio of reaction product 2, toluene, hydrogen-containing silicone oil, hydroquinone and cis-dichlorobis(pyridyl)platinum is 1.5 mol:100 ml:1 mol:0.5 mol:0.020 mol; the amount ratio of white carbon black and reaction product 3 is 5 g:3 g.

[0055] Example 4

[0056] An antioxidant, the preparation of which comprises the following steps:

[0057] Step B1: 3-nitro-2-(phenylamino)benzoic acid was added to tetrahydrofuran, nitrogen was introduced, reflux stirring was started, the temperature was raised to 50°C, and methylmagnesium chloride was added dropwise. After the addition was completed, the reaction was continued for 4 hours, water was added to quench, and the reaction product a was obtained by rotary evaporation, extraction, and drying. The amount ratio of 3-nitro-2-(phenylamino)benzoic acid, tetrahydrofuran and methylmagnesium chloride was 1 mol:48 mL:6.5 mol.

[0058] Step B2: Add molecular sieve, reaction product a and toluene to a reaction bottle, control the temperature to 20°C, stir and react at constant temperature for 2h, filter, distill under reduced pressure and recrystallize to obtain reaction product b; then add reaction product b to ethanol, start stirring, introduce nitrogen, add Pd / C and hydrazine hydrate, stir and react at room temperature for 7h to obtain reaction product c; the amount ratio of molecular sieve, reaction product a and toluene is 2.14g:0.9mol:610mL, and the molecular sieve is a zeolite molecular sieve; the amount ratio of reaction product b, ethanol, Pd / C and hydrazine hydrate is 0.1mol:90mL:0.001g:0.1mol;

[0059] Step B3: Add 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid to DMF, start stirring, slowly add dichlorothionyl, reflux and stir at 50°C for 4 hours to obtain a reaction product d; add the reaction product c, potassium carbonate and dimethyl sulfoxide to a flask to obtain a mixed solution 1; then add the reaction product d to dimethyl sulfoxide to obtain a mixed solution 2, slowly dropwise add the mixed solution 2 to the mixed solution 1 under an ice-water bath, and after the dropwise addition is completed, heat to 40°C, constant temperature reaction for 6h, reduced pressure distillation to obtain reaction product e; the amount ratio of 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid, DMF and dichlorothionyl is 0.1mol:150mL:0.1mol; the amount ratio of reaction product c, potassium carbonate and dimethyl sulfoxide is 0.1mol:0.012mol:80mL; the amount ratio of reaction product d and dimethyl sulfoxide is 0.1mol:10mL;

[0060] Step B4: Add the reaction product e to acetone and stir for 20 minutes to obtain a mixed solution, then pour the halloysite nanotube powder into the above mixed solution, continue stirring for 1 hour, open the vent valve and start the vacuum pump at the same time, continuously evacuate for 30 minutes, then close the vent valve, turn off the vacuum pump, keep stirring the solution for 15 minutes, and the reaction product e is loaded on the halloysite nanotube to obtain an antioxidant; the dosage ratio of the reaction product e, acetone and halloysite nanotube powder is 10g:100mL:6.5g, and the above evacuation and vacuum breaking operations are repeated 3 times.

[0061] Example 5

[0062] An antioxidant, the preparation of which comprises the following steps:

[0063] Step B1: 3-nitro-2-(phenylamino)benzoic acid was added to tetrahydrofuran, nitrogen was introduced, reflux stirring was started, the temperature was raised to 55°C, and methylmagnesium chloride was added dropwise. After the addition was completed, the reaction was continued for 4.5 hours, water was added to quench, and the reaction product a was obtained by rotary evaporation, extraction, and drying. The amount ratio of 3-nitro-2-(phenylamino)benzoic acid, tetrahydrofuran and methylmagnesium chloride was 1 mol:48 mL:6.5 mol.

[0064] Step B2: Add molecular sieve, reaction product a and toluene to a reaction bottle, control the temperature to 20°C, stir and react at constant temperature for 2.5h, filter, distill under reduced pressure and recrystallize to obtain reaction product b; then add reaction product b to ethanol, start stirring, introduce nitrogen, add Pd / C and hydrazine hydrate, stir and react at room temperature for 7.5h to obtain reaction product c; the amount ratio of molecular sieve, reaction product a and toluene is 2.14g:0.9mol:615mL, and the molecular sieve is a zeolite molecular sieve; the amount ratio of reaction product b, ethanol, Pd / C and hydrazine hydrate is 0.1mol:95mL:0.0013g:0.1mol;

[0065] Step B3: Add 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid to DMF, start stirring, slowly add dichlorothionyl, reflux and stir at 50°C for 4.5h to obtain reaction product d; add reaction product c, potassium carbonate and dimethyl sulfoxide to a flask to obtain a mixed solution 1; then add reaction product d to dimethyl sulfoxide to obtain a mixed solution 2, slowly dropwise add the mixed solution 2 to the mixed solution 1 under an ice-water bath, and after the dropwise addition is completed, heat to 40°C, constant temperature reaction for 6.5h, reduced pressure distillation to obtain reaction product e; the usage ratio of 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid, DMF and dichlorothionyl is 0.1mol:150mL:0.13mol; the usage ratio of reaction product c, potassium carbonate and dimethyl sulfoxide is 0.1mol:0.013mol:85mL; the usage ratio of reaction product d and dimethyl sulfoxide is 0.1mol:15mL;

[0066] Step B4: Add the reaction product e to acetone and stir for 25 minutes to obtain a mixed solution, then pour the halloysite nanotube powder into the above mixed solution, continue stirring for 1.2 hours, open the vent valve and start the vacuum pump at the same time, continuously evacuate for 35 minutes, then close the vent valve, turn off the vacuum pump, keep stirring the solution for 15 minutes, and the reaction product e is loaded on the halloysite nanotube to obtain an antioxidant; the dosage ratio of the reaction product e, acetone and halloysite nanotube powder is 10g:100mL:6.7g, and the above evacuation and vacuum breaking operations are repeated 3 times.

[0067] Example 6

[0068] An antioxidant, the preparation of which comprises the following steps:

[0069] Step B1: 3-nitro-2-(phenylamino)benzoic acid was added to tetrahydrofuran, nitrogen was introduced, reflux stirring was started, the temperature was raised to 60°C, and methylmagnesium chloride was added dropwise. After the addition was completed, the reaction was continued for 5 hours, water was added to quench, and the reaction product a was obtained by rotary evaporation, extraction, and drying. The amount ratio of 3-nitro-2-(phenylamino)benzoic acid, tetrahydrofuran and methylmagnesium chloride was 1 mol:48 mL:6.5 mol.

[0070] Step B2: Add molecular sieve, reaction product a and toluene to a reaction bottle, control the temperature to 20°C, stir and react at constant temperature for 3h, filter, distill under reduced pressure and recrystallize to obtain reaction product b; then add reaction product b to ethanol, start stirring, introduce nitrogen, add Pd / C and hydrazine hydrate, stir and react at room temperature for 8h to obtain reaction product c; the amount ratio of molecular sieve, reaction product a and toluene is 2.14g:0.9mol:620mL, and the molecular sieve is a zeolite molecular sieve; the amount ratio of reaction product b, ethanol, Pd / C and hydrazine hydrate is 0.1mol:100mL:0.0015g:0.1mol;

[0071] Step B3: Add 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid to DMF, start stirring, slowly add dichlorothionyl, reflux and stir at 50°C for 5 hours to obtain a reaction product d; add the reaction product c, potassium carbonate and dimethyl sulfoxide to a flask to obtain a mixed solution 1; then add the reaction product d to dimethyl sulfoxide to obtain a mixed solution 2, slowly dropwise add the mixed solution 2 to the mixed solution 1 under an ice-water bath, and after the dropwise addition is completed, heat to 40℃, constant temperature reaction for 7h, reduced pressure distillation to obtain reaction product e; the usage ratio of 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid, DMF and dichlorothionyl is 0.1mol:150mL:0.15mol; the usage ratio of reaction product c, potassium carbonate and dimethyl sulfoxide is 0.1mol:0.015mol:90mL; the usage ratio of reaction product d and dimethyl sulfoxide is 0.1mol:20mL;

[0072] Step B4: Add the reaction product e to acetone and stir for 30 minutes to obtain a mixed solution, then pour the halloysite nanotube powder into the above mixed solution, continue stirring for 1.5 hours, open the vent valve and start the vacuum pump at the same time, continuously evacuate for 40 minutes, then close the vent valve, turn off the vacuum pump, keep stirring the solution for 15 minutes, and the reaction product e is loaded on the halloysite nanotube to obtain an antioxidant; the dosage ratio of the reaction product e, acetone and halloysite nanotube powder is 10g:100mL:7.0g, and the above evacuation and vacuum breaking operations are repeated 3 times.

[0073] Example 7

[0074] An aging-resistant rubber material for a sealing ring, comprising the following raw materials in parts by weight: 70 parts of nitrile rubber, 30 parts of polyacrylate rubber, 10 parts of plasticizer, 1 part of antioxidant, 25 parts of carbon black, 5 parts of zeolite powder, 0.5 parts of paraffin, 2 parts of stearic acid, 3 parts of zinc oxide, 2 parts of sulfur and 1 part of accelerator, wherein the accelerator is 2-mercaptobenzothiazole;

[0075] The sealing ring is made of aging-resistant rubber material, and its preparation includes the following steps:

[0076] The nitrile rubber and the polyacrylate rubber were mixed and kneaded at 40°C for 10 min; then the plasticizer obtained in Example 1, the antioxidant obtained in Example 4, carbon black, zeolite powder, paraffin, stearic acid and zinc oxide were added and kneaded at 100°C for 8 min; finally, sulfur and an accelerator were added and vulcanized at 140°C and 10 MPa for 30 min to obtain an aging-resistant rubber material for a sealing ring.

[0077] Example 8

[0078] An aging-resistant rubber material for a sealing ring, comprising the following raw materials in parts by weight: 85 parts of nitrile rubber, 40 parts of polyacrylate rubber, 12 parts of a plasticizer, 1.5 parts of an antioxidant, 30 parts of carbon black, 7 parts of zeolite powder, 0.7 parts of paraffin, 2.5 parts of stearic acid, 4 parts of zinc oxide, 2.5 parts of sulfur and 1.5 parts of an accelerator, wherein the accelerator is 2-mercaptobenzothiazole;

[0079] The sealing ring is made of aging-resistant rubber material, and its preparation includes the following steps:

[0080] Mix nitrile rubber and polyacrylate rubber, and knead them at 45°C for 12 minutes; then add the plasticizer obtained in Example 2, the antioxidant obtained in Example 5, carbon black, zeolite powder, paraffin, stearic acid, and zinc oxide, and mix them at 110°C for 10 minutes; finally add sulfur and accelerator, and vulcanize at 150°C and 15MPa for 35 minutes to obtain an aging-resistant rubber material for a sealing ring.

[0081] Example 9

[0082] An aging-resistant rubber material for a sealing ring comprises the following raw materials in parts by weight: 100 parts of nitrile rubber, 50 parts of polyacrylate rubber, 15 parts of plasticizer, 2 parts of antioxidant, 35 parts of carbon black, 10 parts of zeolite powder, 1.0 part of paraffin, 3 parts of stearic acid, 5 parts of zinc oxide, 3 parts of sulfur and 2 parts of accelerator, wherein the accelerator is 2-mercaptobenzothiazole;

[0083] The sealing ring is made of aging-resistant rubber material, and its preparation includes the following steps:

[0084] Mix nitrile rubber and polyacrylate rubber, and knead them at 50°C for 15 minutes; then add the plasticizer obtained in Example 3, the antioxidant obtained in Example 6, carbon black, zeolite powder, paraffin, stearic acid, and zinc oxide, and mix them at 120°C for 12 minutes; finally add sulfur and accelerator, and vulcanize at 160°C and 20MPa for 40 minutes to obtain an aging-resistant rubber material for a sealing ring.

[0085] Comparative Example 1

[0086] This comparative example is a commercially available rubber material for sealing rings.

[0087] Comparative Example 2

[0088] Compared with Example 9, the plasticizer is replaced with di[2-(2-butoxyethoxy)ethyl adipate], that is, the polysiloxane chain and white carbon black are not introduced, and the rest is exactly the same as Example 9 to obtain an aging-resistant rubber material for a sealing ring.

[0089] Comparative Example 3

[0090] Compared with Example 9, the antioxidant is replaced with 9,9-dimethylacridine, that is, the benzotriazole structure and the halloysite nanotubes are not introduced, and the rest is exactly the same as Example 9 to obtain an anti-aging rubber material for a sealing ring.

[0091] The effect of the aging-resistant rubber material for the sealing ring prepared by the present invention is further tested, and the test results are as follows.

[0092] In order to test the aging-resistant rubber material for the sealing ring prepared by the present invention, the cold resistance (brittle fracture point temperature) is measured according to the standard GB / T 15256-2014 "Determination of low-temperature brittleness of vulcanized rubber or thermoplastic rubber"; after hot air aging at 180°C × 168h, the thermal stability (retention rate of elongation at break after hot air aging) is measured according to the standard GB / T 528-2009 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber", and the results are recorded in Table 1;

[0093] Table 1:

[0094]

[0095]

[0096] Ultraviolet aging method: The rubber materials obtained in Examples 7-9 and Comparative Examples 1-3 were placed in an ultraviolet radiation environment with an intensity of 0.89 W / m 2 After treatment at a temperature of 50°C and an aging time of 7 days, the change rate of tensile strength and the change rate of elongation at break were determined according to the GB / T528-2009 standard method and recorded in Table 1;

[0097] According to the data in Table 1, compared with Example 1, Example 7, Example 8 and Example 9, it can be seen that the aging-resistant rubber material for sealing rings prepared by the present invention has excellent mechanical properties, cold resistance, thermal stability and aging resistance compared with commercially available rubber materials for sealing rings; compared with Example 2, Example 9 can be seen that the introduction of polysiloxane chains and white carbon black can significantly improve the thermal stability and mechanical properties of the prepared rubber material; compared with Example 3, Example 9 can be seen that the introduction of benzotriazole structure and halloysite nanotube structure can improve the aging resistance of the rubber material, which has a positive effect on improving the thermal stability and mechanical properties.

[0098] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. An aging-resistant rubber material for a sealing ring, Features: The invention comprises the following raw materials in parts by weight: 70-100 parts of nitrile rubber, 30-50 parts of polyacrylate rubber, 10-15 parts of plasticizer, 1-2 parts of antioxidant, 25-35 parts of carbon black, 5-10 parts of zeolite powder, 0.5-1.0 parts of paraffin wax, 2-3 parts of stearic acid, 3-5 parts of zinc oxide, 2-3 parts of sulfur and 1-2 parts of accelerator; the accelerator is 2-mercaptobenzothiazole; The preparation of the plasticizer comprises the following steps: Step A1: In a nitrogen atmosphere, add adipic acid and methanol into a round-bottom flask, start stirring, raise the temperature to 40-50° C., add pyridine and glycidyl acrylate, and react with constant temperature stirring for 9-10 hours to obtain reaction product 1; Step A2: Add (2-n-butoxyethoxy)acetic acid to DMF, start stirring, slowly add thionyl chloride, raise the temperature to 40-50°C, stir and react at constant temperature for 4-5h, filter, extract and dry to obtain the acyl chloride product; Step A3: Add the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide into a flask to obtain a mixed solution a, then add the above-mentioned acyl chloride product into dimethyl sulfoxide to obtain a mixed solution b, slowly dropwise add the mixed solution b into the mixed solution a in an ice-water bath at 0°C, after the dropwise addition is completed, heat to 40°C, react at constant temperature for 8-10 hours, and distill under reduced pressure to obtain a reaction product 2; Step A4: Add toluene, hydrogen-containing silicone oil, hydroquinone, and cis-dichlorobis(pyridyl)platinum into a three-necked flask, stir and introduce nitrogen protection, slowly add reaction product 2, raise the temperature to 70-80° C., and stir for reaction for 3-4 hours to obtain reaction product 3; add white carbon black into a high-speed stirrer, start stirring, add the reaction product three times in equal amounts into a reactor, stir at room temperature and a stirring frequency of 20 Hz for 20-30 minutes to obtain a product, then place the product in an oven, dry at 60° C. for 30 minutes, and then put it into a sealed bag and store at room temperature to obtain a plasticizer; The preparation of the antioxidant comprises the following steps: Step B1: 3-nitro-2-(phenylamino)benzoic acid is added to tetrahydrofuran, nitrogen is introduced, reflux stirring is started, the temperature is raised to 50-60°C, and methylmagnesium chloride is added dropwise. After the addition is complete, the reaction is continued for 4-5 hours, water is added to quench, and the reaction product a is obtained by rotary evaporation, extraction, and drying; Step B2: Add molecular sieve, reaction product a and toluene to a reaction bottle, control the temperature to 20°C, stir and react at constant temperature for 2-3h, filter, distill under reduced pressure and recrystallize to obtain reaction product b; then add reaction product b to ethanol, start stirring, introduce nitrogen, then add Pd / C and hydrazine hydrate, stir and react at room temperature for 7-8h to obtain reaction product c; Step B3: Add 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid to DMF, start stirring, slowly add dichlorothionyl, reflux and stir at 50°C for 4-5h to obtain reaction product d; add reaction product c, potassium carbonate and dimethyl sulfoxide to a flask to obtain mixed solution 1; then add reaction product d to dimethyl sulfoxide to obtain mixed solution 2, slowly dropwise add mixed solution 2 to mixed solution 1 under an ice-water bath, after the dropwise addition is completed, heat to 40°C, react at constant temperature for 6-7h, and distill under reduced pressure to obtain reaction product e; Step B4: Add the reaction product e to acetone, stir for 20-30 minutes to obtain a mixed solution, then pour the halloysite nanotube powder into the above mixed solution, continue stirring for 1-1.5 hours, open the vent valve and start the vacuum pump at the same time, continuously evacuate for 30-40 minutes, then close the vent valve, turn off the vacuum pump, keep stirring the solution to break the vacuum for 15 minutes, and the reaction product e is loaded on the halloysite nanotubes to obtain an antioxidant.

2. The aging-resistant rubber material for a sealing ring according to claim 1, Features: In step A1, the usage ratio of adipic acid, methanol, pyridine and glycidyl acrylate is 0.1 mol: 200-220 mL: 0.001-0.0012 mol: 0.2 mol.

3. The aging-resistant rubber material for a sealing ring according to claim 1, Features: In step A2, the usage ratio of (2-n-butoxyethoxy)acetic acid, DMF and thionyl chloride is 0.1 mol:150 mL:0.1-0.15 mol.

4. The aging-resistant rubber material for a sealing ring according to claim 1, Features: In step A3, the usage ratio of the reaction product 1, pyridine, triethylamine and dimethyl sulfoxide is 0.2 mol: 0.01-0.015 mol: 0.2 mol: 70-80 mL; the usage ratio of the acyl chloride product and dimethyl sulfoxide is 0.1 mol: 20-30 mL.

5. The aging-resistant rubber material for a sealing ring according to claim 1, Features: In step A4, the usage ratio of reaction product 2, toluene, hydrogenated silicone oil, hydroquinone and cis-dichlorobis(pyridyl)platinum is 1-1.5 mol:100 ml:1 mol:0.5 mol:0.015-0.020 mol; the usage ratio of white carbon black and reaction product 3 is 4-5 g:2-3 g.

6. The aging-resistant rubber material for a sealing ring according to claim 1, Features: In step B1, the usage ratio of 3-nitro-2-(phenylamino)benzoic acid, tetrahydrofuran and methylmagnesium chloride is 1 mol:48 mL:6.5 mol.

7. The aging-resistant rubber material for a sealing ring according to claim 1, Features: In step B2, the molecular sieve, reaction product a and toluene are used in a ratio of 2.14 g: 0.9 mol: 610-620 mL, and the molecular sieve is a zeolite molecular sieve; the reaction product b, ethanol, Pd / C and hydrazine hydrate are used in a ratio of 0.1 mol: 90-100 mL: 0.001-0.0015 g: 0.1 mol.

8. The aging-resistant rubber material for a sealing ring according to claim 1, Features: In step B3, the amount ratio of 3-(2-benzotriazolyl)-4-hydroxy-5-tert-butylbenzenepropionic acid, DMF and dichlorothionyl is 0.1mol:150mL:0.1-0.15mol; the amount ratio of reaction product c, potassium carbonate and dimethyl sulfoxide is 0.1mol:0.012-0.015mol:80-90mL; the amount ratio of reaction product d and dimethyl sulfoxide is 0.1mol:10-20mL; in step B4, the amount ratio of reaction product e, acetone and halloysite nanotube powder is 10g:100mL:6.5-7.0g, and the above vacuuming and breaking operations are repeated 3 times.

9. The method for preparing an aging-resistant rubber material for a sealing ring according to claim 1, Features: The steps include: Mix nitrile rubber and polyacrylate rubber, and knead them at 40-50°C for 10-15 minutes; then add plasticizer, antioxidant, carbon black, zeolite powder, paraffin, stearic acid, zinc oxide, and knead them at 100-120°C for 8-12 minutes; finally add sulfur and accelerator, and vulcanize at 140-160°C and 10-20MPa for 30-40 minutes to obtain the aging-resistant rubber material for the sealing ring.