Marine anticorrosion coating based on waterborne graphene and its preparation and application
Through the combination of ultrasonic dispersion technology of polysaccharide colloid and graphene and water-based epoxy modified polyurethane emulsion, the problem of graphene agglomeration is solved, and the high stability and corrosion resistance of graphene in marine anti-corrosion coatings are achieved, meeting the requirements meet the needs of marine engineering and take into account environmental protection and economic benefits.
Patent Information
- Application Number
- CN202410592656.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-05-14
AI Technical Summary
The agglomeration problem of graphene in coatings prevents its unique properties from being fully displayed, and the polymerization method has high reaction requirements and is not suitable for large-scale applications.
Using ultrasonic dispersion technology of polysaccharide colloids and graphene, combined with water-based epoxy modified polyurethane emulsion, through the reaction of colloidal dehydrating agent and polysaccharide colloids, stable micelles are formed to wrap graphene to prevent agglomeration, and through spraying technology Achieve uniform adhesion and high stability of the coating.
It effectively improves the dispersion of graphene and the stability of the coating, enhances the corrosion resistance and adhesion of the coating, meets the needs of marine anti-corrosion coatings, and takes into account environmental protection and economic benefits.
Smart Images

Figure CN118325450B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of coating technology, and in particular to a marine anti-corrosion coating based on water-based graphene and its preparation and application. Background Art
[0002] Marine engineering structures face a ruthless marine environment, and their life cycle is accompanied by continuous corrosion under harsh conditions. This corrosion not only causes huge economic losses, but is also likely to cause major safety accidents due to structural failure. The demand for corrosion resistance of offshore oil and gas platforms, ships and marine facilities is constantly increasing. In this context, the development of new and efficient anti-corrosion coatings not only has great engineering value, but also has far-reaching significance for the long-term utilization of resources, environmental protection and the safety of human marine activities.
[0003] Graphene has been widely studied for its unique two-dimensional structure and excellent shielding and barrier capabilities. As an enhancement material for water-based coatings, graphene can not only improve the physical and mechanical properties of the coating, but also improve its anti-corrosion performance, thereby effectively protecting the metal substrate from corrosion in the marine environment. Studies have shown that by introducing graphene nanosheets into the coating, the corrosion resistance and anti-biological contamination ability of the coating can be significantly improved, providing more reliable protection for marine facilities. By adding nanomaterials such as graphene, a dense structure can be formed in the marine anti-corrosion coating, thereby providing a durable physical barrier to resist chemical and biological corrosion against the metal substrate. Water-based graphene coatings have the significant advantage of low volatile organic compound emissions, thus meeting the modern coatings industry's eager demand for environmentally friendly products. Compared with traditional solvent-based coatings, water-based graphene coatings take into account the dual advantages of environmental friendliness and economic benefits and costs, and are a very promising technology under the current trend of green manufacturing and sustainable development.
[0004] However, due to the strong π-π bond between graphene, it is easy to agglomerate and form defects, which cannot form long-term protection. Therefore, the unique properties of graphene cannot be fully manifested. In order to solve the problem of graphene agglomeration and make it dispersed in water, the graphene dispersion technologies that are currently being studied include chemical dispersion and physical dispersion, that is, the functionalization of graphene is achieved through covalent and non-covalent bond modification. The fusion of graphene and coating resin is mainly through blending and polymerization.
[0005] The blending method is to disperse graphene directly in the coating, and the mixing form can be solution or melt blending. Generally, a high-speed magnetic stirring process, a shear emulsification process, a ball milling method or a sand milling dispersion process is used, and the shear force is used to adsorb the polymer chain into the graphene sheet. However, this method has certain defects. On the one hand, graphene has a high surface free energy and is prone to self-agglomeration; on the other hand, there is no chemical bond between graphene and polymer, and the relative position is not firm. Therefore, graphene aggregation is inevitable during the blending process.
[0006] The polymerization method is to graft active substances with specific functional groups onto the graphene surface in the form of covalent bonds through synthesis methods such as in-situ polymerization, emulsion polymerization or controlled free radical polymerization, and perform functional modifications such as hydrogenation, fluorination, halogenation, free radicals or additional benzene rings on the graphene, thereby achieving the tailoring of the graphene surface structure, improving its reactivity, and effectively improving the solubility, dispersibility and compatibility of graphene inorganic nanofillers in the coating matrix. The polymerization method can ensure that the polymer molecular chain is connected and entangled with the graphene surface, and there is a strong interface interaction between the two, which can effectively solve the dispersion and compatibility problems of graphene in the coating. However, the polymerization method has high requirements for the reaction, and it is difficult to achieve effective control of the position, proportion and grafting rate of the functional groups during the reaction, which is not suitable for large-scale application. Summary of the invention
[0007] The present application provides a water-based graphene marine anti-corrosion coating that can solve the problem of graphite dispersion, and its preparation and application. The water-based graphene marine anti-corrosion coating comprises: component A and component B;
[0008] The component A comprises: 1.5-2.5wt% polysaccharide colloid, 4-6wt% graphene, 3-5wt% stabilizer, 1-1.5wt% preservative, and the balance is water;
[0009] The component B comprises: 73-81wt% of waterborne epoxy modified polyurethane emulsion, 2-4wt% of colloidal dehydrating agent, 0.1-0.2wt% of wetting agent, 10-15wt% of anti-rust pigment, 3-5wt% of film-forming aid, 0.5-2wt% of anti-flash rust aid and 3-6wt% of other additives;
[0010] The mass mixing ratio of component A to component B when used is 1:(3-5).
[0011] As a further embodiment of the present invention, the polysaccharide colloid is one of konjac gum, xanthan gum and carrageenan.
[0012] As a further embodiment of the present invention, the stabilizer is at least one of sodium ethyl sulfate and ethyl glycoside.
[0013] As a further embodiment of the present invention, the water-based epoxy-modified polyurethane emulsion comprises: 6-9wt% epoxy resin and 91-94wt% water-based polyurethane emulsion, and the water-based polyurethane emulsion comprises: 20-23wt% polycarbonate diol, 10-20wt% hydroxyl-containing acrylate emulsion, 8-12wt% polyoxypropylene diol, 0.5-1wt% DMEA, 0.5-1wt% 1,4-butanediol, 18-23wt% IPDI, 14-16wt% HDI, 5-7wt% N,N-dimethylformamide, 1-2wt% triethylamine, 0.5-1wt% 4,4'-diaminodicyclohexylmethane, and the balance water.
[0014] As a further embodiment of the present invention, the colloidal dehydrating agent is at least one of ethyl acetate, n-hexane, ammonium acetate, ammonium sulfate, acetic acid, borax, and calcium chloride.
[0015] As a further embodiment of the present invention, the wetting agent is a silicone surfactant;
[0016] The anti-rust pigment is at least one of barium sulfate, mica, talcum powder, aluminum tripolyphosphate, and molybdenum-modified zinc phosphate.
[0017] In addition, the present invention also provides a method for preparing a marine anticorrosive coating based on water-based graphene, wherein the preparation of component A comprises the following steps:
[0018] S101: adding graphene, a stabilizer and a preservative into water and performing ultrasonic dispersion treatment for 3-4 hours to obtain a graphene aqueous solution;
[0019] S102: heating the graphene aqueous solution to 30-45° C., slowly adding the polysaccharide colloid during ultrasonic dispersion treatment, and continuing ultrasonic stirring for 1-2 hours, and obtaining a graphene colloid solution, i.e., component A, after cooling.
[0020] As a further embodiment of the present invention, the preparation of the waterborne epoxy-modified polyurethane emulsion comprises the following steps:
[0021] S201: After vacuuming polycarbonate diol, hydroxyl-containing acrylic emulsion, and polyoxypropylene diol to remove moisture, IPDI, HDI, and DMEA are added to react to generate a prepolymer;
[0022] S202: Add epoxy resin to the prepolymer, slowly raise the temperature to 60-70°C, add N,N-dimethylformamide acetone solution, and react for 2-3h;
[0023] S203: maintaining the temperature at 60-70°C, adding 1,4-butanediol, and continuing the reaction for 1-1.5 hours to generate an epoxy-modified polyurethane prepolymer;
[0024] S204: lowering the temperature to 40°C, adding triethylamine to the epoxy-modified polyurethane prepolymer for neutralization for 20 minutes, adding deionized water for emulsification for 15-20 minutes under high-speed stirring, continuing to add 4,4'-diaminodicyclohexylmethane monomer for chain extension, and finally removing the remaining solvent acetone in the reaction system under reduced pressure to obtain a water-based epoxy-modified polyurethane emulsion.
[0025] The present invention also provides an application of a marine anticorrosive coating based on water-based graphene, which is sprayed by a two-component spraying device according to a mass ratio of component A to component B of 1: (3-5) and a spraying temperature of 40-50°C.
[0026] The technical solution provided by this application has the following beneficial effects:
[0027] In the present application, graphene is first dispersed by ultrasound to temporarily disperse the graphene in water, and then a polysaccharide colloid is added to gradually increase the viscosity of the solution, and finally the aqueous solution is made into a colloidal state. Since the colloidal solution has good stability and dispersibility, in the colloidal solution, the graphene is wrapped in a stable micelle or solvent molecule layer. This protective film can reduce the mutual contact between the graphene particles, thereby preventing the graphene from agglomerating.
[0028] The polysaccharide colloid in the present application is compounded with konjac gum and one of xanthan gum and carrageenan to form a thermoreversible elastic gel, so that during storage at low temperatures, the viscosity of the colloidal solution increases, so that the graphene is dispersed stably for a long time, and the graphene is prevented from migrating and agglomerating again during long-term storage;
[0029] Component B in the present application contains a colloidal dehydrating agent. When the coating is sprayed, the colloidal dehydrating agent reacts with the colloid of component A and forms a precipitate with the protein or polysaccharide in the colloid, so that the colloid is dehydrated and solidified, which facilitates the evaporation of water and ensures the adhesion of the coating to the substrate. At the same time, after the colloid is dehydrated, the density of the colloid increases, the film-forming performance is good, and the colloid no longer has a water absorption function, which further improves the stability and corrosion resistance of the coating;
[0030] Since polysaccharide colloids contain hydroxyl groups, the present application uses aqueous polyurethane emulsion as the base material of the coating, so that the hydroxyl groups in the polysaccharide colloids react with the isocyanate groups in the polyurethane emulsion to increase the crosslinking degree of the coating and further improve the performance of the coating. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0032] Figure 1 The dispersion of component A in Examples 1-5 of the present invention after being placed for 30 days;
[0033] Figure 2 The dispersion of component A in comparative examples 1-2 and 4-5 of the present invention after being placed for 30 days;
[0034] Figure 3 This is an ultra-depth-of-field microscope photograph of component A in Example 1-5 of the present invention after being placed for 30 days;
[0035] Figure 4 It is an ultra-depth microscope photo of component A in comparative examples 1-2, comparative examples 4-5, and comparative example 7 of the present invention after being placed for 30 days;
[0036] Figure 5 This is a photo of the anti-corrosion coating prepared in Examples 1-5 of the present invention after salt spray resistance without scribe line;
[0037] Figure 6 This is a photo of the anti-corrosion coatings prepared in Examples 1-5 of the present invention after being scribed with salt spray resistance;
[0038] Figure 7 This is a photograph of the anti-corrosion coating prepared in Comparative Examples 1-9 of the present invention after salt spray resistance without scribe line;
[0039] Figure 8 This is a photograph of the anti-corrosion coatings prepared in Comparative Examples 1-9 of the present invention after being marked with salt spray resistance. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be clearly and completely described below in combination with the embodiments of the present application and the comparative examples. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0041] The raw materials used in this application can all be purchased on the market, and the hydroxyl-containing acrylate emulsion adopts CS-hydroxy acrylate emulsion produced by Cansen Chemical New Materials (Shenzhen) Co., Ltd.
[0042] Example 1
[0043] A marine anticorrosive coating based on waterborne graphene, comprising: component A and component B; wherein:
[0044] Component A includes: 0.5wt% konjac gum, 1.5wt% xanthan gum, 4wt% graphene, 3wt% sodium ethyl sulfate, 1wt% sodium benzoate (preservative), 0.5wt% potassium sorbate (preservative), and 89.5wt% water balance.
[0045] Component B includes: 73.4wt% waterborne epoxy modified polyurethane emulsion, 1.5wt% ethyl acetate, 0.5wt% ammonium sulfate, 0.1wt% silane coupling agent, 2wt% mica, 5wt% aluminum tripolyphosphate, 2wt% molybdenum modified zinc phosphate, 8wt% talc, 2wt% ethylene glycol butyl ether acetate (film-forming aid), 1wt% propylene carbonate (film-forming aid), 0.5wt% alcohol silane (anti-flash rust aid), 2wt% quaternary ammonium salt (anti-mildew agent), 0.5wt% BYK024 (defoaming agent), 0.5wt% Aerosil R960 (anti-settling agent), and 0.5wt% SER-ADFA379 (corrosion inhibitor).
[0046] The waterborne epoxy modified polyurethane emulsion comprises: 6wt% epoxy resin E51 and 94wt% waterborne polyurethane emulsion;
[0047] The waterborne polyurethane emulsion includes: 22wt% polycarbonate diol, 15wt% hydroxyl-containing acrylate emulsion, 8wt% polyoxypropylene glycol, 0.8wt% DMEA, 1wt% 1,4-butanediol, 23wt% IPDI, 14wt% HDI, 6wt% N,N-dimethylformamide, 1.5wt% triethylamine, 0.5wt% 4,4'-diaminodicyclohexylmethane, and 8.2wt% water.
[0048] Preparation method of component A:
[0049] S101: adding graphene, a stabilizer and a preservative into water and performing ultrasonic dispersion treatment for 3-4 hours to obtain a graphene aqueous solution;
[0050] S102: heating the graphene aqueous solution to 30-45° C., slowly adding the polysaccharide colloid during ultrasonic dispersion treatment, and continuing ultrasonic stirring for 1-2 hours, and obtaining a graphene colloid solution, i.e., component A, after cooling.
[0051] Preparation method of waterborne epoxy modified polyurethane emulsion:
[0052] S201: Add polycarbonate diol, hydroxyl-containing acrylic emulsion, and polyoxypropylene glycol into a reaction kettle, heat to 100-120° C., stir for 1-1.5 hours, vacuum to remove moisture, cool down, add IPDI, HDI, and DMEA; control the reaction temperature to 40-50° C., react for 0.5-1 hour to generate terminal isocyanate polyurethane prepolymer;
[0053] S202: Add epoxy resin to the prepolymer, slowly raise the temperature to 60-70°C, add 20% N,N-dimethylformamide in acetone solution, and react for 2-3h;
[0054] S203: maintaining the temperature at 60-70°C, adding 1,4-butanediol, and continuing the reaction for 1-1.5 hours to generate an epoxy-modified polyurethane prepolymer;
[0055] S204: lowering the temperature to 40°C, adding triethylamine to the epoxy-modified polyurethane prepolymer for neutralization for 20 minutes, adding deionized water for emulsification for 15-20 minutes under high-speed stirring, continuing to add 4,4'-diaminodicyclohexylmethane monomer for chain extension for 0.5-1h, and finally removing the remaining solvent acetone in the reaction system under reduced pressure to obtain a water-based epoxy-modified polyurethane emulsion.
[0056] When used, spraying is performed through a two-component spraying device according to a mass ratio of component A to component B of 1:3, and the spraying temperature is 40-50°C.
[0057] Example 2
[0058] A marine anticorrosive coating based on waterborne graphene, comprising: component A and component B; wherein:
[0059] Component A includes: 0.2wt% konjac gum, 1.4wt% xanthan gum, 4wt% graphene, 3wt% sodium ethyl sulfate, 1wt% ethyl glycoside, 0.5wt% sodium benzoate (preservative), 0.5wt% potassium sorbate (preservative), and 89.4wt% water.
[0060] Component B includes: 80.9wt% waterborne epoxy modified polyurethane emulsion, 1.5wt% ethyl acetate, 0.5wt% ammonium sulfate, 0.1wt% silane coupling agent, 2wt% talc, 3wt% aluminum tripolyphosphate, 2wt% molybdenum modified zinc phosphate, 3wt% barium sulfate, 2wt% ethylene glycol butyl ether acetate (film-forming aid), 1wt% propylene carbonate (film-forming aid), 0.5wt% alcohol silane (anti-flash rust aid), 2wt% quaternary ammonium salt (anti-mildew agent), 0.5wt% BYK024 (defoaming agent), 0.5wt% Aerosil R960 (anti-settling agent), and 0.5wt% SER-AD FA379 (corrosion inhibitor).
[0061] The waterborne epoxy modified polyurethane emulsion comprises: 8wt% epoxy resin E51 and 92wt% waterborne polyurethane emulsion;
[0062] The waterborne polyurethane emulsion includes: 20wt% polycarbonate diol, 16wt% hydroxyl-containing acrylate emulsion, 9wt% polyoxypropylene diol, 0.5wt% DMEA, 0.6wt% 1,4-butanediol, 19wt% IPDI, 16wt% HDI, 7wt% N,N-dimethylformamide, 2wt% triethylamine, 0.8wt% 4,4'-diaminodicyclohexylmethane, and 9.1wt% water.
[0063] The preparation methods of component A and waterborne epoxy-modified polyurethane emulsion are the same as those in Example 1.
[0064] When used, spraying is performed through a two-component spraying device according to a mass ratio of component A to component B of 1:4, and the spraying temperature is 40-50°C.
[0065] Example 3
[0066] A marine anticorrosive coating based on waterborne graphene, comprising: component A and component B; wherein:
[0067] Component A includes: 0.5wt% konjac gum, 2wt% carrageenan, 6wt% graphene, 3wt% sodium ethyl sulfate, 2wt% ethyl glycoside, 1wt% sodium benzoate (preservative), 0.5wt% potassium sorbate (preservative), and 85wt% water.
[0068] Component B includes: 73wt% waterborne epoxy modified polyurethane emulsion, 0.5wt% n-hexane, 1.3wt% borax, 1wt% calcium chloride, 0.2wt% silane coupling agent, 2wt% barium sulfate, 3wt% aluminum tripolyphosphate, 3wt% molybdenum modified zinc phosphate, 5wt% mica, 1.5wt% ethylene glycol butyl ether acetate (film-forming aid), 3wt% propylene carbonate (film-forming aid), 1.5wt% alcohol silane (anti-flash rust aid), 3wt% quaternary ammonium salt (anti-mildew agent), 0.5wt% BYK024 (defoaming agent), 1wt% Aerosil R960 (anti-settling agent), and 0.5wt% SER-AD FA379 (corrosion inhibitor).
[0069] The waterborne epoxy modified polyurethane emulsion comprises: 9wt% epoxy resin E51 and 91wt% waterborne polyurethane emulsion;
[0070] The waterborne polyurethane emulsion includes: 23wt% polycarbonate diol, 13wt% hydroxyl-containing acrylate emulsion, 12wt% polyoxypropylene diol, 1wt% DMEA, 0.9wt% 1,4-butanediol, 20wt% IPDI, 15wt% HDI, 5wt% N,N-dimethylformamide, 2wt% triethylamine, 0.6wt% 4,4'-diaminodicyclohexylmethane, and 7.5wt% water.
[0071] The preparation methods of component A and waterborne epoxy-modified polyurethane emulsion are the same as those in Example 1.
[0072] When used, spraying is performed through a two-component spraying device according to a mass ratio of component A to component B of 1:5, and the spraying temperature is 40-50°C.
[0073] Example 4
[0074] A marine anticorrosive coating based on waterborne graphene, comprising: component A and component B; wherein:
[0075] Component A includes: 0.5wt% konjac gum, 1.5wt% carrageenan, 5wt% graphene, 1wt% sodium ethyl sulfate, 3wt% ethyl glycoside, 1wt% sodium benzoate (preservative), 0.5wt% potassium sorbate (preservative), and 87.5wt% water.
[0076] Component B includes: 70.8wt% waterborne epoxy modified polyurethane emulsion, 1wt% ethyl acetate, 0.5wt% ammonium sulfate, 0.5wt% ammonium acetate, 1wt% borax, 0.5wt% calcium chloride, 0.2wt% silane coupling agent, 2wt% mica, 2wt% aluminum tripolyphosphate, 3wt% molybdenum modified zinc phosphate, 6wt% talc, 5wt% propylene carbonate (film-forming aid), 2wt% alcohol silane (anti-flash rust aid), 3wt% quaternary ammonium salt (anti-mildew agent), 0.8wt% BYK024 (defoaming agent), 1.2wt% Aerosil R960 (anti-settling agent), and 0.5wt% SER-AD FA379 (corrosion inhibitor).
[0077] The waterborne epoxy modified polyurethane emulsion comprises: 8wt% epoxy resin E51 and 92wt% waterborne polyurethane emulsion;
[0078] The water-based polyurethane emulsion includes: 18wt% polycarbonate diol, 20wt% hydroxyl-containing acrylate emulsion, 9wt% polyoxypropylene glycol, 0.8wt% DMEA, 0.8wt% 1,4-butanediol, 18wt% IPDI, 16wt% HDI, 7wt% N,N-dimethylformamide, 1.5wt% triethylamine, 0.8wt% 4,4'-diaminodicyclohexylmethane, and 8.1wt% water.
[0079] The preparation methods of component A and waterborne epoxy-modified polyurethane emulsion are the same as those in Example 1.
[0080] When used, spraying is performed through a two-component spraying device according to a mass ratio of component A to component B of 1:4, and the spraying temperature is 40-50°C.
[0081] Example 5
[0082] A marine anticorrosive coating based on waterborne graphene, comprising: component A and component B; wherein:
[0083] Component A includes: 0.5wt% konjac gum, 1.5wt% carrageenan, 6wt% graphene, 2wt% sodium ethyl sulfate, 3wt% ethyl glycoside, 0.5wt% sodium benzoate (preservative), 1wt% potassium sorbate (preservative), and 85.5wt% water.
[0084] Component B includes: 77.8wt% waterborne epoxy modified polyurethane emulsion, 0.5wt% ammonium acetate, 1.5wt% acetic acid, 0.5wt% borax, 0.2wt% silane coupling agent, 4wt% aluminum tripolyphosphate, 2wt% molybdenum modified zinc phosphate, 4wt% talc, 3wt% ethylene glycol butyl ether acetate (film-forming aid), 1.5wt% alcohol silane (anti-flash rust aid), 3wt% quaternary ammonium salt (anti-mildew agent), 0.5wt% BYK024 (defoaming agent), 1wt% Aerosil R960 (anti-settling agent), and 0.5wt% SER-AD FA379 (corrosion inhibitor).
[0085] The waterborne epoxy modified polyurethane emulsion comprises: 6wt% epoxy resin E51 and 94wt% waterborne polyurethane emulsion;
[0086] The waterborne polyurethane emulsion includes: 23wt% polycarbonate diol, 12wt% hydroxyl-containing acrylate emulsion, 8wt% polyoxypropylene glycol, 0.8wt% DMEA, 0.7wt% 1,4-butanediol, 20wt% IPDI, 16wt% HDI, 7wt% N,N-dimethylformamide, 1.5wt% triethylamine, 0.7wt% 4,4'-diaminodicyclohexylmethane, and 10.3wt% water.
[0087] The preparation methods of component A and waterborne epoxy-modified polyurethane emulsion are the same as those in Example 1.
[0088] When used, spraying is performed through a two-component spraying device according to a mass ratio of component A to component B of 1:5, and the spraying temperature is 40-50°C.
[0089] The compositions of component A and component B are shown in Table 1-Table 3:
[0090] Table 1 Composition of component A in Examples 1-5
[0091]
[0092] Table 2 Composition of component B in Examples 1-5
[0093]
[0094] Table 3 Composition of waterborne epoxy modified polyurethane emulsion in component B of Examples 1-5
[0095]
[0096] Comparative Example 1
[0097] The difference from Example 1 is that the modified graphene prepared by the preparation method of Example 3 of a graphene anti-corrosion coating disclosed in publication number CN117363148B is used instead of the graphene in Example 1, and no polysaccharide colloid is used.
[0098] The preparation method of modified graphene is as follows:
[0099] 1.1. Take diethanolamine and acetone and stir them to dissolve them. Install a calcium oxide alkaline drying tube in the reflux vessel, heat to 48°C for reflux, apply mechanical stirring at 240rpm, slowly add allyl chloride within 50min, continue the constant temperature reflux reaction after complete addition, and control the addition reaction time to be 2h. In the reaction, the amount ratio of diethanolamine, allyl chloride and acetone is 0.1mol:0.12mol:70mL. After the reaction is completed, remove the low-boiling substances mainly composed of acetone and excess allyl chloride by rotary evaporation to obtain an intermediate.
[0100] 1.2. Take γ-mercaptopropyltriethoxysilane, intermediate, dimethylphenylphosphine and dimethyl sulfoxide, mix them under nitrogen protection, heat to 80°C, apply mechanical stirring at 120 rpm, and 600 W / m 2 The mixture was irradiated with ultraviolet light and stirred at a constant temperature for 2.5 hours. During the reaction, the amount ratio of γ-mercaptopropyltriethoxysilane, intermediate, dimethylphenylphosphine and dimethyl sulfoxide was 0.1 mol: 0.1 mol: 0.12 g: 90 mL. After the reaction, the dimethyl sulfoxide was removed by vacuum rotary evaporation to obtain a modifier.
[0101] 1.3. Prepare a 40% ethanol solution by mass, mix the modifier, ethanol solution and dimethylacetamide, add acetic acid to adjust the pH value to 4, stir and hydrolyze for 1.2 hours, then add graphene oxide, stir and mix at 2000rpm for 10 minutes, then control the stirring rate to 150rpm, add ammonia water at a uniform rate to adjust to neutrality, and stand at room temperature for 24 hours. During the reaction, the amount ratio of graphene oxide, modifier, ethanol solution and dimethylacetamide is 100g:25mmol:280mL:70mL. After the reaction is completed, centrifuge to take the bottom precipitate, add water for ultrasonic dispersion to form a dispersion with a solid content of 50%, spray dry to obtain modified graphene.
[0102] Comparative Example 2
[0103] The difference from Example 1 is that graphene oxide is used instead of the graphene in Example 1, and no polysaccharide colloid is used.
[0104] Comparative Example 3
[0105] The difference from Example 1 is that component A is not used.
[0106] Comparative Example 4
[0107] The difference from Example 1 is that konjac gum is not used, and an equal amount of xanthan gum is used instead.
[0108] Comparative Example 5
[0109] The difference from Example 4 is that konjac gum is not used, but an equal amount of carrageenan is used instead.
[0110] Comparative Example 6
[0111] The difference from Example 1 is that no colloid dehydrating agent is used, and an equal amount of water is used instead.
[0112] Comparative Example 7
[0113] The difference from Example 1 is that no stabilizer is used, and an equal amount of water is used instead.
[0114] Comparative Example 8
[0115] The difference from Example 1 is that, during application, the mass mixing ratio of component A to component B is 1:2.
[0116] Comparative Example 9
[0117] The difference from Example 1 is that, during application, the mass mixing ratio of component A to component B is 1:6.
[0118] Test methods and results
[0119] 1. Dispersibility of graphene: The prepared graphene dispersion was placed in a transparent plastic bottle, left to stand for 30 days, the situation in the bottle was observed, and then its dispersibility was observed using an ultra-depth of field microscope;
[0120] 2. Salt spray resistance test: 3.5 wt% NaCl solution is used to simulate the seawater environment, and the spray test is carried out according to the ASTM B117 standard to evaluate the corrosion resistance of the coating in the simulated marine atmospheric environment. In the experimental setting, the coating samples are placed in a dedicated salt spray test chamber and continuously exposed to high salinity conditions. The test time reaches 1000h to simulate the impact of long-term marine climate. The coating samples include those with and without surface scratches;
[0121] 3. Acid and alkali resistance test: The coating samples were exposed to solutions with different pH values, and pH 3 sulfuric acid solution and pH 11 sodium hydroxide solution were selected for testing. The test time was 168 hours. After the test, the acid and alkali resistance of the coating was evaluated by comparing the mass change and the surface morphology;
[0122] 4. Solvent resistance test: The coating samples are immersed in acetone and toluene for 24 hours. The solvent resistance is evaluated by observing whether the coating surface has blistering, cracking or shedding. The corrosion ability of the solvent on the coating is often a direct and effective indicator for testing the chemical corrosion resistance of the coating material;
[0123] 5. Adhesion test: Grind the galvanized sheet with 800-grit sandpaper to remove the surface material, and then wipe it repeatedly with alcohol to remove the oil on the surface. Spray the coating evenly on the galvanized sheet. After drying for 7 days, use a thickness gauge to measure the film thickness of about 120μm. Seal the edges with paraffin wax, and use a knife to draw a series of parallel horizontal and vertical lines. The horizontal and vertical lines intersect to form small squares. Use tape to stick to the scratches, slowly tear off and observe whether the film has peeling to judge its adhesion. Use GB / T9286-1998 standard to analyze the adhesion level;
[0124] 6. Water resistance test: According to the provisions of 9.1 of GB / T1733-1993, immerse the test panel in grade 3 water that meets the requirements of GB / T6682-2008 for 30 days.
[0125] 7. Impact resistance test: carried out in accordance with the provisions of GB / T1732-1993;
[0126] 8. Pencil hardness test: Conduct in accordance with the provisions of GB / T6739-2006.
[0127] The test results are shown in Tables 4-7 and Figure 1-8 ,Since graphene in comparative example 6 is insoluble in water, its dispersibility cannot be effectively tested by observing it using an ultra-depth-of-field microscope.
[0128] Table 4: Test results of Examples 1-5
[0129]
[0130] Table 5: Test results of Example 1 and Comparative Examples 1-4
[0131]
[0132] Table 6: Test results of Example 4 and Comparative Example 5
[0133]
[0134] Table 7: Test results of Example 1 and Comparative Examples 6-9
[0135]
[0136] From the above examples 1-5 and comparative examples 1-9, Tables 4-7, Figure 1-8 It can be seen that the graphene solution of this embodiment has good stability and dispersibility, and is applied to marine anti-corrosion coatings to improve the stability and corrosion resistance of the coatings.
[0137] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the protection scope of the technical solutions of the embodiments of the present application.
Claims
1. A marine anticorrosion coating based on waterborne graphene, characterized in that: include: Component A and component B; The component A comprises: 1.5-2.5wt% polysaccharide colloid, 4-6wt% graphene, 3-5wt% stabilizer, 1-1.5wt% preservative, and the balance is water; The component B comprises: 73-81wt% of waterborne epoxy modified polyurethane emulsion, 2-4wt% of colloidal dehydrating agent, 0.1-0.2wt% of wetting agent, 10-15wt% of anti-rust pigment, 3-5wt% of film-forming aid, 0.5-2wt% of anti-flash rust aid and 3-6wt% of other additives; The mass mixing ratio of component A and component B when used is 1:(3-5); The polysaccharide colloid is one of konjac gum, xanthan gum and carrageenan; The waterborne epoxy-modified polyurethane emulsion comprises: 6-9wt% epoxy resin and 91-94wt% waterborne polyurethane emulsion, wherein the waterborne polyurethane emulsion comprises: 20-23wt% polycarbonate diol, 10-20wt% hydroxyl-containing acrylate emulsion, 8-12wt% polyoxypropylene diol, 0.5-1wt% DMEA, 0.5-1wt% 1,4-butanediol, 18-23wt% IPDI, 14-16wt% HDI, 5-7wt% N,N-dimethylformamide, 1-2wt% triethylamine, 0.5-1wt% 4,4'-diaminodicyclohexylmethane, and the balance water; The colloidal dehydrating agent is at least one of ethyl acetate, n-hexane, ammonium acetate, ammonium sulfate, acetic acid, borax, and calcium chloride; The preparation of component A comprises the following steps: S101: adding graphene, a stabilizer and a preservative into water and performing ultrasonic dispersion treatment for 3-4 hours to obtain a graphene aqueous solution; S102: heating the graphene aqueous solution to 30-45° C., slowly adding the polysaccharide colloid during ultrasonic dispersion treatment, and continuing ultrasonic stirring for 1-2 hours, and cooling to obtain a graphene colloid solution, i.e., component A; The preparation of the aqueous epoxy-modified polyurethane emulsion comprises the following steps: S201: After vacuuming polycarbonate diol, hydroxyl-containing acrylic emulsion, and polyoxypropylene diol to remove moisture, IPDI, HDI, and DMEA are added to react to generate a prepolymer; S202: Add epoxy resin to the prepolymer, slowly raise the temperature to 60-70°C, add N,N-dimethylformamide acetone solution, and react for 2-3h; S203: maintaining the temperature at 60-70°C, adding 1,4-butanediol, and continuing the reaction for 1-1.5 hours to generate an epoxy-modified polyurethane prepolymer; S204: lowering the temperature to 40°C, adding triethylamine to the epoxy-modified polyurethane prepolymer for neutralization for 20 minutes, adding deionized water for emulsification for 15-20 minutes under high-speed stirring, continuing to add 4,4'-diaminodicyclohexylmethane monomer for chain extension, and finally removing the remaining solvent acetone in the reaction system under reduced pressure to obtain a water-based epoxy-modified polyurethane emulsion.
2. The marine anticorrosion coating based on water-based graphene according to claim 1, characterized in that: The stabilizer is at least one of sodium ethyl sulfate and ethyl glycoside.
3. The marine anticorrosion coating based on water-based graphene according to claim 1, characterized in that: The wetting agent is a silicone surfactant; The anti-rust pigment is at least one of barium sulfate, mica, talcum powder, aluminum tripolyphosphate, and molybdenum-modified zinc phosphate.
4. The use of the marine anticorrosion coating based on waterborne graphene according to any one of claims 1 to 3, characterized in that: The spraying is performed by a two-component spraying device according to a mass ratio of component A to component B of 1: (3-5) and a spraying temperature of 40-50°C.