Adhesive coated on film surface and preparation method thereof

By adding polymeric antioxidants and modified chloroether resins to epoxy resin adhesives, the problems of poor high-temperature oxidation resistance and high film brittleness of epoxy resin adhesives are solved, significantly improving their high-temperature resistance. Oxidation performance and bonding performance extend the service life of the film.

CN118325547BActive Publication Date: 2024-10-11KUNSHAN BYE MACROMOLECULE MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410751229.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-10-11
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

Epoxy resin adhesives have poor high-temperature oxidation resistance and the film is highly brittle, causing the film to easily oxidize and fall off in high-temperature environments.

Method used

Use 55-65 parts of epoxy resin, 1-2 parts of polymer antioxidant material, 5-7.5 parts of modified chloroether resin, 0.5-1 part of thixotropic agent, 10-20 parts of curing agent, 0.5-1.5 parts of curing The combination of accelerator and 0.5-1 parts of defoaming agent improves the high temperature oxidation resistance and bonding properties of epoxy resin through polymer antioxidant materials and modified chloroether resin.

Benefits of technology

It effectively improves the high-temperature oxidation resistance and bonding performance of the epoxy resin adhesive, prolongs the service life of the film, and avoids the risk of falling off due to the brittleness of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118325547B_ABST
    Figure CN118325547B_ABST
Patent Text Reader

Abstract

This invention relates to the field of adhesive technology, and discloses an adhesive for coating a thin film surface and its preparation method. This adhesive is made by mixing epoxy resin as a base material with polymeric antioxidants, modified chloroprene resin, and thixotropic agents as excipients. The polymeric antioxidants and modified chloroprene resin participate in the curing process of the epoxy resin, thereby forming an interwoven cross-linked structure with the epoxy resin molecular chains. The polymeric antioxidant structure contains a large number of high-bond-energy silicon-oxygen bonds and hindered phenolic antioxidant structures, achieving a significant improvement in the adhesive's high-temperature oxidation resistance with a relatively small addition amount. The large number of ether bonds in the modified chloroprene resin structure increases the number of hydrogen bonds that can form with the substrate in the adhesive, thereby enhancing the adhesive's bonding performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adhesives, and in particular to an adhesive coated on a film surface and a preparation method thereof. Background Art

[0002] With the rapid development of modern industry and technology, film materials are widely used in packaging, electronics, optics and other fields due to their light weight, transparency and strong plasticity. The coating technology on the film surface, especially the application of adhesives, plays a vital role in improving the functionality, durability and processing performance of the film. Especially at the moment when electronic equipment is becoming more and more popular, the protective films used on the surface of various electronic product displays need to be coated with adhesives to ensure that the film can be stably attached to the display surface. This requires the adhesive to have good bonding properties to ensure that multiple materials can be tightly bonded. In addition, since electronic products will generate higher temperatures during use, this requires the adhesive to have good high temperature oxidation resistance to avoid oxidation of the adhesive during use, which leads to the problem of film shedding.

[0003] The mainstream adhesives currently include epoxy resins, acrylates, and polyurethanes. Epoxy resin adhesives are relatively more adhesive, more chemically stable, and more transparent, so they can be used on film surfaces. However, epoxy resin adhesives have average antioxidant properties, and will turn yellow when exposed to high temperatures for a long time, which not only affects the appearance, but also creates the risk of film shedding. In addition, the film formed after epoxy resin is cured is very brittle, and the film may be damaged when subjected to external forces. These defects have a significant negative impact on the service life of the film.

[0004] Based on this, the present invention provides an adhesive having comprehensive properties such as good bonding properties, which can be used on the surface of a film to improve the durability of the film material. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies in the prior art, the present invention provides an adhesive coated on the surface of a film and a preparation method thereof, which solves the problems of poor high-temperature oxidation resistance of epoxy resin adhesives and greater film brittleness.

[0007] (II) Technical solution

[0008] An adhesive coated on the surface of a film is made of the following components in parts by weight:

[0009] 55-65 parts of epoxy resin, 1-2 parts of polymer antioxidant, 5-7.5 parts of modified chloroether resin, 0.5-1 parts of thixotropic agent, 10-20 parts of curing agent, 0.5-1.5 parts of curing accelerator, 0.5-1 parts of defoaming agent;

[0010] The modified chloroether resin is prepared by taking chloroether resin and alcoholamine monomer as raw materials.

[0011] A method for preparing an adhesive coated on a film surface comprises the following steps:

[0012] Step A, weigh each component raw material according to weight and set aside;

[0013] Step B, mixing epoxy resin, polymer antioxidant, modified chloroether resin and thixotropic agent, stirring and mixing at a speed of 1000-2000r / min, reducing the speed to 200-300r / min, adding defoamer, standing for 30-60min after adding, degassing, and preparing a mixed material;

[0014] Step C: Add curing agent and curing accelerator to the mixed material, increase the speed to 800-1000r / min after adding, stir and mix evenly to obtain an adhesive.

[0015] Preferably, the preparation method of the polymer antioxidant material comprises the following steps:

[0016] Step S1, castor oil and tetrahydrofuran are mixed and stirred to form a uniform liquid material, nitrogen is introduced as a protective gas, and dichloromethylsilane is added to the liquid material. After the addition, the temperature is raised to 40-50° C. and maintained for 2-4 hours under stirring conditions, and then an acidifying agent is added to the liquid material, and the temperature is maintained for 4-6 hours. The nitrogen is removed and the material is discharged to obtain a branched castor oil polymer;

[0017] Step S2, mixing the branched castor oil polymer and toluene, mechanically stirring, then adding 2-(2-hydroxy-3-tert-butyl-5-methylbenzyl)-4-methyl-6-tert-butylphenyl acrylate and a catalyst, stirring and mixing to form a uniform solution, turning on the heating, stirring and keeping warm at 70-80° C. for 3-6 hours, discharging the material, and obtaining a polymer antioxidant material.

[0018] Preferably, in step S1, the molar ratio of castor oil to dichloromethylsilane is 1:1-1.5.

[0019] Preferably, in step S1, the acidifying agent is selected from pyridine or triethylamine.

[0020] Preferably, in step S2, the catalyst is chloroplatinic acid, and the amount of the catalyst used is 0.02-0.03% of the total mass of the branched castor oil polymer and 2-(2-hydroxy-3-tert-butyl-5-methylbenzyl)-4-methyl-6-tert-butylphenyl acrylate.

[0021] Specifically, the structure of the polymer antioxidant contains a large number of silicon-oxygen bonds and hindered phenol antioxidant structures. Therefore, adding a small amount of the polymer antioxidant can effectively improve the high-temperature oxidation resistance of the epoxy resin. In addition, by controlling the amount of castor oil and dichloromethylsilane, the polymer antioxidant structure can also contain active hydroxyl groups that do not participate in the reaction, which can participate in the curing process of the epoxy resin, thereby introducing flexible castor oil segments into the film molecular chain, which is beneficial to improving the toughness of the film formed by the curing of the epoxy resin adhesive.

[0022] Preferably, the specific preparation method of the modified chloroether resin is as follows:

[0023] Dissolve the chloroether resin in xylene and stir to form a mixed liquid. Then add the alcohol amine monomer to the mixed liquid and stir to form a uniform reaction liquid. Turn on the heating and control the heating rate to 1-2°C / min. Raise the temperature to 50-55°C and maintain it at this temperature for 2-3h. Discharge the material to obtain the modified chloroether resin.

[0024] Preferably, the chlorine content of the chloroether resin is 44%.

[0025] Preferably, the alcoholamine monomer is selected from ethanolamine or diethanolamine.

[0026] Specifically, by modifying the chloroether resin, a large number of active substituted hydroxyl groups are generated in the chloroether resin structure. In the subsequent curing process of the epoxy resin adhesive, the molecular chains of the modified chloroether resin can be cross-linked and entangled with the epoxy resin molecular chains. On the one hand, the cross-linking degree of the molecular chains can be improved, showing higher cohesive energy. On the other hand, the large number of ether bonds in the chloroether resin can be utilized to increase the number of hydrogen bonds with the surface of the adhered substrate. Therefore, the bonding performance of the epoxy resin adhesive can be improved from these two inventions.

[0027] Preferably, the thixotropic agent is selected from fumed silica; the curing agent is selected from anhydride curing agents; the curing accelerator is selected from imidazole curing accelerators; and the defoaming agent is selected from BYK-A530 or BYK-A515.

[0028] 3. Beneficial technical effects

[0029] (1) The present invention first prepares a polymer antioxidant, which contains abundant silicon-oxygen bonds with high bond energy, and can improve the high temperature resistance of epoxy resin adhesives. The large amount of hindered phenol antioxidant structures contained in the polymer antioxidant structure can improve the antioxidant performance of epoxy resins, thereby producing a synergistic effect, and achieving a small amount of addition to effectively improve the high temperature oxidation resistance of epoxy resin adhesives. In addition, since the polymer antioxidant participates in the curing process, it can be stably present in the adhesive, and there will be no problem of volatilization migration leading to the inability to ensure antioxidant performance.

[0030] (2) The present invention prepares a modified chloroether resin and mixes it with an epoxy resin. On the one hand, the large number of ether bonds in the chloroether resin structure can be used to increase the number of hydrogen bonds that can be generated between the adhesive and the adhered substrate. On the other hand, the cohesive force of the epoxy resin adhesive can be increased by participating in the curing, thereby further improving the bonding performance of the adhesive. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0032] Figure 1 This is the infrared test image of polymer antioxidant material. DETAILED DESCRIPTION

[0033] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. Preferred embodiments of the present invention are given below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0034] Example 1

[0035] Preparation of polymer antioxidants

[0036] Step S1, 2.4 g of castor oil and tetrahydrofuran are mixed and stirred to form a uniform liquid material, nitrogen is introduced as a protective gas, and then 0.3 g of dichloromethylsilane is added to the liquid material. After the addition, the temperature is raised to 45° C. and maintained for 3 hours under stirring conditions. Then, 0.1 g of triethylamine is added to the liquid material, and the temperature is maintained for 6 hours. The nitrogen is removed and the material is discharged to obtain a branched castor oil polymer;

[0037] Step S2, 1.6 g of branched castor oil polymer and toluene are mixed, mechanically stirred, and then 0.5 g of 2-(2-hydroxy-3-tert-butyl-5-methylbenzyl)-4-methyl-6-tert-butylphenyl acrylate and 5 mg of chloroplatinic acid are added, and after stirring and mixing into a uniform solution, heating is turned on, and the mixture is kept stirred at 75° C. for 4 hours, and the material is discharged to obtain a polymer antioxidant material.

[0038] Figure 1 This is the infrared test image of the polymer antioxidant material, where 3398cm -1 The absorption peak at 3065cm is the characteristic absorption peak of hydroxyl group. -1 and 30998cm -1 The absorption peak at 2800-3000cm is the characteristic absorption peak of CH on the benzene ring. -1 The absorption peaks at 1052 cm are the characteristic absorption peaks of CH in methyl, methylene and methine. -1 The absorption peak at is the Si-O characteristic absorption peak, and Figure 1 It can be observed that 2150cm -1 There is no characteristic absorption peak of Si-H.

[0039] Example 2

[0040] Preparation of modified chloroether resin

[0041] 1.5 g of chloroether resin with a chlorine content of 44% was dissolved in xylene and stirred to form a mixed liquid. Then 0.2 g of diethanolamine was added to the mixed liquid and stirred to form a uniform reaction liquid. The heating was turned on and the heating rate was controlled to be 2°C / min. The temperature was raised to 55°C and maintained at this temperature for 3 hours. The material was discharged to obtain a modified chloroether resin.

[0042] The XKCHN-700 organic element analyzer was used to analyze the percentage of each element in the modified chloroether resin. The test results showed that the percentage of carbon element was 43.81% and the content of nitrogen element was 2.48%. The chloroether resin itself does not contain nitrogen element, so it can be obviously inferred that the nitrogen element comes from diethanolamine.

[0043] Example 3

[0044] An adhesive coated on the surface of a film is made of the following components in parts by weight:

[0045] 55 parts of epoxy resin, 1 part of polymer antioxidant, 5 parts of modified chloroether resin, 0.5 parts of fumed silica, 10 parts of curing agent hexahydrophthalic anhydride, 0.5 parts of curing accelerator 2-methylimidazole, 0.5 parts of defoaming agent BYK-A530;

[0046] The preparation method of the adhesive comprises the following steps:

[0047] Step A, weigh each component raw material according to weight and set aside;

[0048] Step B, mixing epoxy resin, polymer antioxidant, modified chloroether resin and fumed silica, stirring and mixing at a speed of 1000 r / min, reducing the speed to 200 r / min, adding defoamer BYK-A530, and after adding, standing for 30 minutes to degas to prepare a mixed material;

[0049] Step C: adding a curing agent hexahydrophthalic anhydride and a curing accelerator 2-methylimidazole to the mixed material, and after adding, increasing the speed to 800 r / min, stirring and mixing evenly to obtain an adhesive.

[0050] Example 4

[0051] An adhesive coated on the surface of a film is made of the following components in parts by weight:

[0052] 60 parts of epoxy resin, 1.5 parts of polymer antioxidant, 7 parts of modified chloroether resin, 0.6 parts of fumed silica, 18 parts of curing agent hexahydrophthalic anhydride, 1 part of curing accelerator 2-methylimidazole, 0.8 parts of defoaming agent BYK-A515;

[0053] The preparation method of the adhesive comprises the following steps:

[0054] Step A, weigh each component raw material according to weight and set aside;

[0055] Step B, mixing epoxy resin, polymer antioxidant, modified chloroether resin and fumed silica, stirring and mixing at a speed of 1500 r / min, reducing the speed to 300 r / min, adding defoamer BYK-A515, and after adding, standing for 40 minutes to degas to prepare a mixed material;

[0056] Step C: adding a curing agent hexahydrophthalic anhydride and a curing accelerator 2-methylimidazole to the mixed material, and after adding, increasing the speed to 1000 r / min, stirring and mixing evenly to obtain an adhesive.

[0057] Example 5

[0058] An adhesive coated on the surface of a film is made of the following components in parts by weight:

[0059] 65 parts of epoxy resin, 2 parts of polymer antioxidant, 7.5 parts of modified chloroether resin, 1 part of fumed silica, 20 parts of curing agent hexahydrophthalic anhydride, 1.5 parts of curing accelerator 2-methylimidazole, 1 part of defoaming agent BYK-A515;

[0060] The preparation method of the adhesive comprises the following steps:

[0061] Step A, weigh each component raw material according to weight and set aside;

[0062] Step B, mixing epoxy resin, polymer antioxidant, modified chloroether resin and fumed silica, stirring and mixing at a speed of 2000 r / min, reducing the speed to 300 r / min, adding defoamer BYK-A515, and after adding, standing for 60 minutes to degas to prepare a mixed material;

[0063] Step C: adding a curing agent hexahydrophthalic anhydride and a curing accelerator 2-methylimidazole to the mixed material, and after adding, increasing the speed to 1000 r / min, stirring and mixing evenly to obtain an adhesive.

[0064] Comparative Example 1

[0065] An adhesive coated on the surface of a film is made of the following components in parts by weight:

[0066] 60 parts of epoxy resin, 1.5 parts of polymer antioxidant, 7 parts of chloroether resin, 0.6 parts of fumed silica, 18 parts of curing agent hexahydrophthalic anhydride, 1 part of curing accelerator 2-methylimidazole, 0.8 parts of defoaming agent BYK-A515;

[0067] The preparation method of the adhesive comprises the following steps:

[0068] Step A, weigh each component raw material according to weight and set aside;

[0069] Step B, mixing epoxy resin, polymer antioxidant, chloroether resin and fumed silica, stirring and mixing at a speed of 1500 r / min, reducing the speed to 300 r / min, adding defoamer BYK-A515, and after adding, standing for 40 minutes to degas to prepare a mixed material;

[0070] Step C: adding a curing agent hexahydrophthalic anhydride and a curing accelerator 2-methylimidazole to the mixed material, and after adding, increasing the speed to 1000 r / min, stirring and mixing evenly to obtain an adhesive.

[0071] Comparative Example 2

[0072] An adhesive coated on the surface of a film is made of the following components in parts by weight:

[0073] 60 parts of epoxy resin, 1.5 parts of polymer antioxidant, 0.6 parts of fumed silica, 18 parts of curing agent hexahydrophthalic anhydride, 1 part of curing accelerator 2-methylimidazole, 0.8 parts of defoaming agent BYK-A515;

[0074] The preparation method of the adhesive comprises the following steps:

[0075] Step A, weigh each component raw material according to weight and set aside;

[0076] Step B, mixing epoxy resin, polymer antioxidant and fumed silica, stirring and mixing at a speed of 1500 r / min, reducing the speed to 300 r / min, adding defoamer BYK-A515, and after adding, standing for 40 minutes to degas to prepare a mixed material;

[0077] Step C: adding a curing agent hexahydrophthalic anhydride and a curing accelerator 2-methylimidazole to the mixed material, and after adding, increasing the speed to 1000 r / min, stirring and mixing evenly to obtain an adhesive.

[0078] Comparative Example 3

[0079] An adhesive coated on the surface of a film is made of the following components in parts by weight:

[0080] 60 parts of epoxy resin, 1.5 parts of 2-(2-hydroxy-3-tert-butyl-5-methylbenzyl)-4-methyl-6-tert-butylphenyl acrylate, 7 parts of modified chloroether resin, 0.6 parts of fumed silica, 18 parts of curing agent hexahydrophthalic anhydride, 1 part of curing accelerator 2-methylimidazole, 0.8 parts of defoaming agent BYK-A515;

[0081] The preparation method of the adhesive comprises the following steps:

[0082] Step A, weigh each component raw material according to weight and set aside;

[0083] Step B, epoxy resin, 2-(2-hydroxy-3-tert-butyl-5-methylbenzyl)-4-methyl-6-tert-butylphenyl acrylate, modified chloroether resin and fumed silica are mixed, stirred and mixed at a speed of 1500 r / min, the speed is reduced to 300 r / min, and then a defoamer BYK-A515 is added. After the addition is completed, the mixture is allowed to stand for 40 minutes for degassing to prepare a mixed material;

[0084] Step C: adding a curing agent hexahydrophthalic anhydride and a curing accelerator 2-methylimidazole to the mixed material, and after adding, increasing the speed to 1000 r / min, stirring and mixing evenly to obtain an adhesive.

[0085] Test example

[0086] The adhesives in Examples 3 to 5 and Comparative Examples 1 to 3 were applied to the surface of the polyimide film, the dry adhesive thickness was controlled to be 50 μm, and a release layer was covered on the coated surface of the adhesive to prepare a test sample;

[0087] According to GB / T 2792-1998, the 180° peel strength of the test sample was tested;

[0088] After the test samples were placed at room temperature for 60 days, they were transferred to an accelerated aging test chamber and the aging temperature was set to (120±5)℃ and the humidity was set to (85±5)%. After 500 hours, the 180° peel strength of the test samples was tested. At the same time, the test samples were observed for bubbles, delamination, glue overflow, yellowing and other undesirable phenomena. The light transmittance was tested to evaluate the high temperature oxidation resistance of the adhesive. The results are recorded in the following table:

[0089]

[0090] Analysis of the test results presented in the above table shows that the addition of modified chloroether resin and polymer antioxidants has a very obvious effect on improving the bonding performance and high temperature aging resistance of epoxy resin adhesives.

[0091] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. An adhesive applied to a film surface, characterized in that: It is made of the following components in parts by weight: 55-65 parts of epoxy resin, 1-2 parts of polymer antioxidant, 5-7.5 parts of modified chloroether resin, 0.5-1 parts of thixotropic agent, 10-20 parts of curing agent, 0.5-1.5 parts of curing accelerator, 0.5-1 parts of defoaming agent; The preparation method of the polymer antioxidant material comprises the following steps: Step S1, castor oil and tetrahydrofuran are mixed and stirred to form a uniform liquid material, nitrogen is introduced as a protective gas, and dichloromethylsilane is added to the liquid material. After the addition, the temperature is raised to 40-50° C. and maintained for 2-4 hours under stirring conditions, and then an acidifying agent is added to the liquid material, and the temperature is maintained for 4-6 hours. The nitrogen is removed and the material is discharged to obtain a branched castor oil polymer; Step S2, mixing the branched castor oil polymer material and toluene, mechanically stirring, then adding 2-(2-hydroxy-3-tert-butyl-5-methylbenzyl)-4-methyl-6-tert-butylphenyl acrylate and a catalyst, stirring and mixing to form a uniform solution, turning on the heating, keeping the temperature at 70-80° C. and stirring for 3-6 hours, discharging the material, and obtaining a polymer antioxidant material; The modified chloroether resin is prepared by using chloroether resin and alcoholamine monomer as raw materials; In the step S1, the acidifying agent is selected from pyridine or triethylamine; In the step S2, the catalyst is chloroplatinic acid, and the amount of the catalyst is 0.02-0.03% of the total mass of the branched castor oil polymer and 2-(2-hydroxy-3-tert-butyl-5-methylbenzyl)-4-methyl-6-tert-butylphenyl acrylate; The specific preparation method of the modified chloroether resin is as follows: Dissolve the chloroether resin in xylene and stir to form a mixed liquid, then add the alcohol amine monomer to the mixed liquid, stir to form a uniform reaction liquid, turn on the heating, control the heating rate to be 1-2°C / min, raise the temperature to 50-55°C, and maintain it at this temperature for 2-3h, discharge the material, and obtain the modified chloroether resin; The alcoholamine monomer is selected from ethanolamine or diethanolamine; The thixotropic agent is selected from fumed silica; the curing agent is selected from anhydride curing agents; the curing accelerator is selected from imidazole curing accelerators; and the defoaming agent is selected from BYK-A530 or BYK-A515.

2. The adhesive applied to the surface of a film according to claim 1, characterized in that: In the step S1, the molar ratio of castor oil to dichloromethylsilane is 1:1-1.

5.

3. The adhesive applied to the surface of a film according to claim 1, characterized in that: The chlorine content of the chloroether resin is 44%.

4. A method for preparing an adhesive coated on a film surface as claimed in claim 1, characterized in that: The following steps are involved: Step A, weigh each component raw material according to weight and set aside; Step B, mixing epoxy resin, polymer antioxidant, modified chloroether resin and thixotropic agent, stirring and mixing at a speed of 1000-2000r / min, reducing the speed to 200-300r / min, adding defoamer, standing for 30-60min after adding, degassing, and preparing a mixed material; Step C: Add curing agent and curing accelerator to the mixed material, increase the speed to 800-1000r / min after adding, stir and mix evenly to obtain an adhesive.