A preparation process of high-strength composite fiber
Through the esterification and polycondensation of terephthalic acid, 1,4-butanediol and allylmalonic acid and the modification of 2-mercaptopyrimidine, combined with PET for composite spinning, the problem of insufficient strength and stability of composite fibers was solved. , achieving improved high strength and antibacterial effect.
Patent Information
- Application Number
- CN202410444101.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-15
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-04-15
AI Technical Summary
Existing composite fibers have poor strength and dimensional stability, making it difficult to meet the needs of highly differentiated and functional fibers.
Terephthalic acid, 1,4-butanediol and allylmalonic acid are used for esterification and polycondensation reaction, 2-mercaptopyrimidine is added for modification, and combined with PET for composite spinning to form high-strength composite fibers.
It improves the strength and dimensional stability of the composite fiber and gives it an antibacterial effect, which is significantly better than traditional PBT/PET composite fiber.
Abstract
Description
Technical Field
[0001] The invention relates to the field of fibers, and in particular to a preparation process of high-strength composite fibers. Background Art
[0002] Polyethylene terephthalate (PET) is often called polyester. At present, PET fiber is mainly produced by direct esterification of terephthalic acid (PTA) and ethylene glycol (EG) or transesterification of dimethyl terephthalate (DMT) and ethylene glycol (EG). There are benzene rings in the PET molecule, so it needs to be stretched after traditional melt spinning to make it crystallize quickly, so that the orientation and crystallinity of the produced fiber are higher, and the PET fiber produced has better performance. The disadvantages of PET are mainly due to the close arrangement of molecules and the lack of hydrophilic groups, so the hygroscopicity and antistatic properties are poor, and the product is easy to burn.
[0003] Polybutylene terephthalate (PBT) is a polycondensation product of dimethyl terephthalate (DMT) or terephthalic acid (PTA) and butanediol (BDO). Due to the excellent resilience, mildew and moth resistance, good curl elasticity, antistatic and dyeability of PBT fiber, PBT fiber is widely used in elastic clothing such as swimsuits, sportswear, ski suits, jumpsuits, dance tights, etc. The elasticity of PBT fiber is second only to spandex and better than nylon. At the same time, spandex is more expensive and has poor light resistance and is prone to yellowing. Therefore, it can completely replace spandex in some fabrics. For example, in stretch jeans, spandex is usually used as stretch yarn, but spandex has low strength and is easy to break after long-term wear and friction. Using PBT fiber instead of spandex as stretch yarn can effectively improve this situation. Because PBT fiber has a wool-like feel, it can be interwoven with cotton, linen, etc. in the wool spinning industry as autumn and winter clothing. It is also an ideal imitation down and filling material.
[0004] With the progress of society and the improvement of people's living standards, the demand for fiber differentiation and functionalization is getting higher and higher. In recent years, existing textile fibers have gradually developed towards lightness and softness, and fiber thinning is a major trend. At present, fibers with a single filament fineness of less than 1.0 dtex are generally defined as ultrafine fibers, and the acquisition of ultrafine composite fibers has become the key. However, due to the defects of the fiber material itself, most of the composite fibers produced on the market currently have poor performance in strength and dimensional stability. Summary of the invention
[0005] In view of the problems existing in the prior art, the object of the present invention is to provide a preparation process of high-strength composite fibers.
[0006] The purpose of the present invention is achieved by the following technical solutions:
[0007] A preparation process of a high-strength composite fiber comprises the following steps:
[0008] Step 1, preparing the PBT primary product:
[0009] Using terephthalic acid, 1,4-butanediol and allylmalonic acid as raw materials, esterification reaction and polycondensation reaction are carried out in sequence under the action of a first catalyst to obtain a PBT primary product;
[0010] Step 2, preparing modified PBT product:
[0011] The PBT initial product is dissolved in an organic solvent, nitrogen is used as a protective gas, 2-mercaptopyrimidine is added, and after sufficient stirring, the second catalyst is added, and the reaction is stirred for 1-3 hours under ultraviolet light, and the solvent is removed under reduced pressure to obtain a modified PBT product;
[0012] Step 3, preparing the melt:
[0013] After the PET slices are subjected to a melting treatment, a PET melt is obtained; after the modified PBT product is subjected to a melting treatment, a modified PBT melt is obtained;
[0014] Step 4, preparing composite fibers:
[0015] The modified PBT melt and the PET melt are subjected to composite spinning to obtain high-strength composite fibers.
[0016] Preferably, in step 1, the mass ratio of terephthalic acid, 1,4-butanediol and allylmalonic acid is 1.7-2.5:1.2-1.8:0.28-0.56.
[0017] Preferably, in step 1, the first catalyst is one of antimony trioxide, tetrabutyl titanate, dibutyltin dilaurate, p-toluenesulfonic acid, and stannous octoate.
[0018] Preferably, in step 1, the amount of the first catalyst used is 4%-8% of the mass of terephthalic acid.
[0019] Preferably, in step 1, the temperature of the esterification reaction is 242-252° C., the pressure is 220-380 kPa, and the reaction time is 2-4 h.
[0020] Preferably, in step 1, the polycondensation reaction includes a first polycondensation reaction and a second polycondensation reaction. The first polycondensation reaction is a pre-polycondensation reaction, and the product of the esterification reaction is maintained at a temperature of 250-260°C and a pressure of 100-150 kPa for 0.5-1 h; the temperature of the second polycondensation reaction is 260-270°C, the pressure is within 100 Pa, and the reaction time is 3-5 h.
[0021] Preferably, in step 2, the mass ratio of the PBT primary product, 2-mercaptopyrimidine and the organic solvent is 1:0.2-0.4:10-20.
[0022] Preferably, in step 2, the wavelength of the ultraviolet lamp is 200-400 nm, and the preferred wavelength is 365 nm.
[0023] Preferably, in step 2, the organic solvent is N,N-dimethylformamide or N-methylpyrrolidone.
[0024] Preferably, in step 2, the second catalyst is a benzophenone photoinitiator, including one of benzophenone, 4-methylbenzophenone and 4-phenylbenzophenone.
[0025] Preferably, in step 2, the amount of the second catalyst used is 4%-8% of the total mass of 2-mercaptopyrimidine.
[0026] Preferably, in step 3, the PET chips and the modified PBT product need to be dried before the melt treatment, and the drying temperature is 110-120° C. and the treatment time is 4-8 hours.
[0027] Preferably, in step 3, the melting temperature of the PET chips is 260-270°C, and the melting temperature of the modified PBT product is 280-290°C.
[0028] Preferably, in step 4, the mass ratio of the modified PBT melt to the PET melt is 1.2-1.5:1.
[0029] Preferably, in step 4, the composite spinning process includes the following steps: composite spinning, cooling, oiling, pre-network treatment, hot roller treatment, main network treatment, winding and testing and packaging.
[0030] Preferably, in the composite spinning process, the spinning temperature of the modified PBT melt is 282-288°C, and the spinning temperature of the PET melt is 285-295°C.
[0031] More preferably, the cooling process is side-blowing cooling, the side-blowing temperature is 20-25° C., and the wind speed is 0.5-1 m / s.
[0032] More preferably, the pressure during the pre-networking process is 0.3-0.8 MPa.
[0033] More preferably, the hot roller treatment includes a first hot roller (GR1) and a second hot roller (GR2), the speed of the first hot roller is 1550-1750 m / min and the temperature is 80-90°C; the speed of the second hot roller is 3350-3850 m / min and the temperature is 115-135°C.
[0034] More preferably, the pressure during the main network treatment process is 0.2-0.6 MPa.
[0035] More preferably, the winding speed is 3000-4000 m / min.
[0036] The beneficial effects of the present invention are:
[0037] 1. The present invention prepares a high-strength composite fiber, which is prepared by composite spinning of modified PBT and PET. Different from the conventional PBT / PET composite fiber, the present invention modifies the PBT material and then composite spins it with PET. The obtained composite fiber has excellent strength and dimensional stability even in a relatively thin case, and also has a certain antibacterial effect.
[0038] 2. The modified PBT prepared by the present invention uses terephthalic acid and 1,4-butanediol as main raw materials, and allylmalonic acid containing double bonds as a modified raw material to prepare a PBT primary product containing unsaturated double bonds, and then uses 2-mercaptopyrimidine containing thiol and pyrimidine groups to combine with the unsaturated PBT primary product, and the thiol and double bonds undergo click chemistry reaction to generate thioether bonds, and finally obtain a modified PBT containing thioether groups and pyrimidine groups.
[0039] 3. After testing, the modified PBT / PET composite fiber prepared by the present invention has higher strength, stability and antibacterial properties than traditional PBT / PET composite fibers. The possible reason is the sulfide group and pyrimidine group present in the modified PBT structure. These two groups have good stability and antibacterial properties, which greatly improve the performance of the composite fiber. DETAILED DESCRIPTION
[0040] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.
[0041] In order to better understand the above technical scheme, the exemplary embodiments of the present invention are described in more detail below. Although exemplary embodiments of the present invention are shown, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0042] The PET chips used in the embodiments of the present invention are Sinopec polyester PET chips, model BG85, melting point of 248° C., terminal carboxyl value of 21 mol / L, crystallinity of 54%, and viscosity of 0.879 dl / g.
[0043] The present invention will be further described below in conjunction with the following examples. Example 1
[0044] A preparation process of a high-strength composite fiber comprises the following steps:
[0045] Step 1, preparing the PBT primary product:
[0046] Terephthalic acid, 1,4-butanediol and allylmalonic acid are sequentially mixed in a reactor, the mass ratio of terephthalic acid, 1,4-butanediol and allylmalonic acid is 2.1:1.5:0.42, tetrabutyl titanate is added as a catalyst, the amount of tetrabutyl titanate is 6% of the mass of terephthalic acid, then the temperature in the reactor is raised to 247°C, while the pressure is maintained at 280 kPa, after reacting for 3 hours, the esterification is completed; then the reactor is further heated to 255°C, the pressure is reduced to 100 kPa, and the temperature is maintained for 0.5 hours to complete the pre-condensation; then the temperature is further raised to 270°C, the pressure is reduced to less than 100 Pa, the temperature is maintained for 4 hours, the reaction is completed, that is, the condensation process is completed, and finally the PBT primary product is prepared;
[0047] Step 2, preparing modified PBT product:
[0048] The PBT initial product is dissolved in N,N-dimethylformamide, nitrogen is used as a protective gas, 2-mercaptopyrimidine is added, the mass ratio of the PBT initial product, 2-mercaptopyrimidine and N,N-dimethylformamide is 1:0.3:15, after sufficient stirring, 4-methylbenzophenone is added, the amount of 4-methylbenzophenone used is 6% of the total mass of 2-mercaptopyrimidine, and the reaction is stirred for 2 hours under the irradiation of an ultraviolet lamp with a wavelength of 365nm, and the solvent is removed under reduced pressure to obtain a modified PBT product;
[0049] Step 3, preparing the melt:
[0050] The PET slices were dried at 110°C for 6 hours and then melted at 265°C to obtain a PET melt; the modified PBT product was dried at 115°C for 6 hours and then melted at 285°C to obtain a modified PBT melt;
[0051] Step 4, preparing composite fibers:
[0052] The modified PBT melt and the PET melt are respectively transported to the spinning equipment for composite spinning through metering pumps, the spinning temperature of the modified PBT melt is 286°C, the spinning temperature of the PET melt is 290°C, and the modified PBT melt and the PET melt are compositely spun at a mass ratio of 1.3:1 to form a composite filament bundle, which is then cooled by side blowing, the temperature of the side blowing is 20°C, and the wind speed is 0.5m / s, followed by oiling and 0.5MPa pre-network treatment to form a pre-network product;
[0053] Then the pre-network product is processed by the first hot roller (GR1) and the second hot roller (GR2) in sequence, the speed of the first hot roller is 1650m / min and the temperature is 85℃; the speed of the second hot roller is 3560m / min and the temperature is 125℃;
[0054] After the hot roller treatment, the main network treatment of 0.4MPa is carried out, and then it is wound and formed at a speed of 3500m / min. After inspection and packaging, high-strength composite fibers are obtained. Example 2
[0055] A preparation process of a high-strength composite fiber comprises the following steps:
[0056] Step 1, preparing the PBT primary product:
[0057] Terephthalic acid, 1,4-butanediol and allylmalonic acid are sequentially mixed in a reactor, the mass ratio of terephthalic acid, 1,4-butanediol and allylmalonic acid is 1.7:1.2:0.28, tetrabutyl titanate is added, the amount of tetrabutyl titanate is 4% of the mass of terephthalic acid, and then the temperature in the reactor is raised to 242°C, while the pressure is maintained at 220 kPa, and after reacting for 2 hours, esterification is completed; then the reactor is further heated to 250°C, the pressure is reduced to 100 kPa, and the temperature is maintained for 0.5 hours to complete the pre-condensation; then the temperature is further raised to 260°C, the pressure is reduced to less than 100 Pa, and the temperature is maintained for 3 hours, the reaction is completed, that is, the condensation process is completed, and finally the PBT primary product is prepared;
[0058] Step 2, preparing modified PBT product:
[0059] The PBT initial product is dissolved in N,N-dimethylformamide, nitrogen is used as a protective gas, 2-mercaptopyrimidine is added, the mass ratio of the PBT initial product, 2-mercaptopyrimidine and N,N-dimethylformamide is 1:0.2:10, after sufficient stirring, benzophenone is added, the amount of benzophenone used is 4% of the total mass of 2-mercaptopyrimidine, and the reaction is stirred for 1-3 hours under the irradiation of an ultraviolet lamp with a wavelength of 365nm, and the solvent is removed under reduced pressure to obtain a modified PBT product;
[0060] Step 3, preparing the melt:
[0061] The PET slices were dried at 110°C for 4 hours and then melted at 260°C to obtain a PET melt; the modified PBT product was dried at 110°C for 4 hours and then melted at 280°C to obtain a modified PBT melt;
[0062] Step 4, preparing composite fibers:
[0063] The modified PBT melt and the PET melt are respectively transported to the spinning equipment for composite spinning through metering pumps, the spinning temperature of the modified PBT melt is 282°C, the spinning temperature of the PET melt is 285°C, and the modified PBT melt and the PET melt are compositely spun at a mass ratio of 1.2:1 to form a composite filament bundle, which is then cooled by side blowing, the temperature of the side blowing is 20°C, and the wind speed is 0.5m / s, followed by oiling and 0.3MPa pre-network treatment to form a pre-network product;
[0064] Then the pre-network product is sequentially processed by the first hot roller (GR1) and the second hot roller (GR2), the speed of the first hot roller is 1550m / min and the temperature is 80℃; the speed of the second hot roller is 3350m / min and the temperature is 115℃;
[0065] After the hot roller treatment, the main network treatment is carried out at 0.2MPa, and then it is wound and formed at a speed of 3000m / min. After inspection and packaging, high-strength composite fibers are obtained. Example 3
[0066] A preparation process of a high-strength composite fiber comprises the following steps:
[0067] Step 1, preparing the PBT primary product:
[0068] Terephthalic acid, 1,4-butanediol and allylmalonic acid are sequentially mixed in a reactor, the mass ratio of terephthalic acid, 1,4-butanediol and allylmalonic acid is 2.5:1.8:0.56, p-toluenesulfonic acid is added, the amount of p-toluenesulfonic acid is 8% of the mass of terephthalic acid, and then the temperature in the reactor is raised to 252°C, while the pressure is maintained at 380 kPa, and after reacting for 4 hours, esterification is completed; then the reactor is further heated to 260°C, the pressure is reduced to 150 kPa, and the temperature is maintained for 1 hour to complete the pre-condensation; then the temperature is further raised to 270°C, the pressure is reduced to less than 100 Pa, and the temperature is maintained for 5 hours, the reaction is completed, that is, the condensation process is completed, and finally the PBT primary product is prepared;
[0069] Step 2, preparing modified PBT product:
[0070] The PBT initial product is dissolved in N,N-dimethylformamide, nitrogen is used as a protective gas, 2-mercaptopyrimidine is added, the mass ratio of the PBT initial product, 2-mercaptopyrimidine and N,N-dimethylformamide is 1:0.4:20, after sufficient stirring, 4-phenylbenzophenone is added, the amount of 4-phenylbenzophenone used is 8% of the total mass of 2-mercaptopyrimidine, and the reaction is stirred for 3 hours under the irradiation of an ultraviolet lamp with a wavelength of 365nm, and the solvent is removed under reduced pressure to obtain a modified PBT product;
[0071] Step 3, preparing the melt:
[0072] The PET slices were dried at 120°C for 8 hours and then melted at 270°C to obtain a PET melt; the modified PBT product was dried at 120°C for 8 hours and then melted at 290°C to obtain a modified PBT melt;
[0073] Step 4, preparing composite fibers:
[0074] The modified PBT melt and the PET melt are respectively transported to the spinning equipment for composite spinning through metering pumps, the spinning temperature of the modified PBT melt is 288°C, the spinning temperature of the PET melt is 295°C, and the modified PBT melt and the PET melt are compositely spun at a mass ratio of 1.5:1 to form a composite filament bundle, which is then cooled by side blowing, the temperature of the side blowing is 25°C, and the wind speed is 1m / s, followed by oiling and 0.8MPa pre-network treatment to form a pre-network product;
[0075] Then the pre-network product is processed by the first hot roller (GR1) and the second hot roller (GR2) in sequence, the speed of the first hot roller is 1750m / min and the temperature is 90℃; the speed of the second hot roller is 3350-3850m / min and the temperature is 135℃;
[0076] After the hot roller treatment, the main network treatment is carried out at 0.6MPa, and then it is wound and formed at a speed of 4000m / min. After inspection and packaging, high-strength composite fibers are obtained.
[0077] Comparative Example 1
[0078] A preparation process of a composite fiber is the same as the steps of Example 1, except that the modified PBT product prepared in step 1-2 is replaced by a conventional PBT product. The preparation method of the conventional PBT product includes:
[0079] Terephthalic acid and 1,4-butanediol are mixed in a reactor in sequence, with a mass ratio of terephthalic acid to 1,4-butanediol of 2.1:1.5. Tetrabutyl titanate is added, with the amount of tetrabutyl titanate being 6% of the mass of terephthalic acid. The temperature in the reactor is then raised to 247°C while maintaining the pressure at 280 kPa. After reacting for 3 hours, esterification is completed. The reactor is then heated to 255°C, the pressure is reduced to 100 kPa, and the temperature and pressure are maintained for 0.5 hours to complete pre-condensation. The temperature is then raised to 270°C, the pressure is reduced to less than 100 Pa, the temperature and pressure are maintained for 4 hours, the reaction is completed, and the condensation process is completed, and finally a PBT product is prepared.
[0080] Comparative Example 2
[0081] A preparation process of a composite fiber is the same as the steps of Example 1, except that the preparation method of the modified PBT product is different (2-mercaptopyrimidine is not added). The preparation method of the modified PBT product in this comparative example includes:
[0082] Terephthalic acid, 1,4-butanediol and allylmalonic acid are mixed in a reactor in sequence, the mass ratio of terephthalic acid, 1,4-butanediol and allylmalonic acid is 2.1:1.5:0.42, tetrabutyl titanate is added as a catalyst, the amount of tetrabutyl titanate is 4%-8% of the mass of terephthalic acid, and then the temperature in the reactor is raised to 247°C, while maintaining the pressure at 280 kPa. After the reaction for 3 hours, the esterification is completed; then the reactor is further heated to 255°C, the pressure is reduced to 100 kPa, and the temperature is maintained for 0.5 hours to complete the pre-condensation; then the temperature is continued to be raised to 270°C, the pressure is reduced to less than 100 Pa, and the temperature is maintained for 4 hours. The reaction is completed, that is, the condensation process is completed, and finally a modified PBT product is prepared.
[0083] Comparative Example 3
[0084] A preparation process of a composite fiber is the same as the steps of Example 1, except that the preparation method of the modified PBT product is different (allylmalonic acid is not added). The preparation method of the modified PBT product in this comparative example includes:
[0085] Step 1, preparing the PBT primary product:
[0086] Terephthalic acid and 1,4-butanediol are sequentially mixed in a reactor, the mass ratio of terephthalic acid to 1,4-butanediol is 2.1:1.5, tetrabutyl titanate is added as a catalyst, the amount of tetrabutyl titanate is 6% of the mass of terephthalic acid, and then the temperature in the reactor is raised to 247°C, while the pressure is maintained at 280 kPa, and after the reaction for 3 hours, the esterification is completed; then the reactor is further heated to 255°C, the pressure is reduced to 100 kPa, and the temperature and pressure are maintained for 0.5 hours to complete the pre-condensation; then the temperature is further raised to 270°C, the pressure is reduced to less than 100 Pa, and the temperature and pressure are maintained for 4 hours, the reaction is completed, that is, the condensation process is completed, and finally the PBT primary product is prepared;
[0087] Step 2, preparing modified PBT product:
[0088] The PBT initial product is dissolved in N,N-dimethylformamide, nitrogen is used as a protective gas, 2-mercaptopyrimidine is added, the mass ratio of the PBT initial product, 2-mercaptopyrimidine and N,N-dimethylformamide is 1:0.2:10, after sufficient stirring, benzophenone is added, the amount of benzophenone used is 4% of the total mass of 2-mercaptopyrimidine, and the reaction is stirred for 1-3 hours under the irradiation of an ultraviolet lamp with a wavelength of 365nm, and the solvent is removed under reduced pressure to obtain a modified PBT product.
[0089] In order to more intuitively demonstrate the performance of the product prepared by the present invention, the performance of the composite fibers prepared by Examples 1-3 and the comparative example was tested, and the tests included:
[0090] The fiber breaking strength and 50% elongation (after elongation of 50% of the original length) recovery rate are tested using an XQ-1A fiber strength and elongation tester. The average value is taken after three tests, referring to GB / T 14344-2022 "Test method for tensile properties of chemical fiber filaments".
[0091] For the detection of fiber antibacterial rate, please refer to Appendix D of FZ / T 73023-2006 "Antibacterial Knitwear".
[0092] The test results are shown in Table 1 below.
[0093] Table 1 Performance test results of different composite fibers
[0094] Single yarn fineness (dtex) Breaking strength (cN / dtex) 50% elongation recovery rate (%) Escherichia coli inhibition rate (%) Staphylococcus aureus inhibition rate (%) Example 1 0.50 8.34 95.8 95.8 97.2 Comparative Example 1 0.50 6.25 86.1 67.3 70.2 Comparative Example 2 0.51 7.33 91.7 68.5 71.5 Comparative Example 3 0.50 6.21 85.3 72.6 75.9
[0095] It can be seen from the test in Table 1 that the composite fiber prepared in Example 1 has higher breaking strength and 50% elongation recovery rate than those of Comparative Examples 1-3 under the premise of a single fiber fineness of about 0.50 dtex, indicating that the composite fiber prepared in Example 1 has better strength and dimensional stability; in addition, the antibacterial rate of the composite fiber prepared in Example 1 against Escherichia coli and Staphylococcus aureus can reach 95%, indicating that it has excellent antibacterial effect, while Comparative Examples 1-2 do not have antibacterial groups, so the antibacterial effect is poor, and Comparative Example 3 may have a small amount of thiol or pyrimidine groups remaining on the surface, resulting in an antibacterial effect slightly higher than that of Comparative Examples 1-3, but it is still far weaker than that of Example 1.
[0096] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms should not be understood as necessarily being directed to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine different embodiments or examples described in this specification.
[0097] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A process for preparing high-strength composite fibers, characterized in that: The following steps are involved: Step 1, preparing the PBT primary product: Using terephthalic acid, 1,4-butanediol and allylmalonic acid as raw materials, esterification reaction and polycondensation reaction are carried out in sequence under the action of a first catalyst to obtain a PBT primary product; Step 2, preparing modified PBT product: The PBT initial product is dissolved in an organic solvent, nitrogen is used as a protective gas, 2-mercaptopyrimidine is added, and after sufficient stirring, the second catalyst is added, and the reaction is stirred for 1-3 hours under ultraviolet light, and the solvent is removed under reduced pressure to obtain a modified PBT product; Step 3, preparing the melt: After the PET slices are subjected to a melting treatment, a PET melt is obtained; after the modified PBT product is subjected to a melting treatment, a modified PBT melt is obtained; Step 4, preparing composite fibers: The modified PBT melt and the PET melt are subjected to composite spinning to obtain high-strength composite fibers; In the step 1, the mass ratio of terephthalic acid, 1,4-butanediol and allylmalonic acid is 1.7-2.5:1.2-1.8:0.28-0.56; In the step 2, the mass ratio of the PBT primary product, 2-mercaptopyrimidine and the organic solvent is 1:0.2-0.4:10-20; In the step 4, the mass ratio of the modified PBT melt to the PET melt is 1.2-1.5:
1.
2. The process for preparing a high-strength composite fiber according to claim 1, characterized in that: In the step 1, the first catalyst is one of antimony trioxide, tetrabutyl titanate, dibutyltin dilaurate, p-toluenesulfonic acid, and stannous octoate; and the amount of the first catalyst used is 4%-8% of the mass of terephthalic acid.
3. The process for preparing a high-strength composite fiber according to claim 1, characterized in that: In the step 1, the temperature of the esterification reaction is 242-252° C., the pressure is 220-380 kPa, and the reaction time is 2-4 h.
4. The process for preparing a high-strength composite fiber according to claim 1, characterized in that: In the step 1, the polycondensation reaction includes a first polycondensation reaction and a second polycondensation reaction. The first polycondensation reaction is a pre-polycondensation reaction, and the product of the esterification reaction is maintained at a temperature of 250-260° C. and a pressure of 100-150 kPa for 0.5-1 h; the temperature of the second polycondensation reaction is 260-270° C., the pressure is within 100 Pa, and the reaction time is 3-5 h.
5. The process for preparing a high-strength composite fiber according to claim 1, characterized in that: In step 2, the wavelength of the ultraviolet lamp is 200-400 nm; the organic solvent is N,N-dimethylformamide or N-methylpyrrolidone.
6. The process for preparing a high-strength composite fiber according to claim 1, characterized in that: In the step 2, the second catalyst is a benzophenone photoinitiator, including one of benzophenone, 4-methylbenzophenone, and 4-phenylbenzophenone; the amount of the second catalyst used is 4%-8% of the total mass of 2-mercaptopyrimidine.
7. The process for preparing a high-strength composite fiber according to claim 1, characterized in that: In the step 3, the PET slices and the modified PBT product need to be dried before the melting treatment, the drying temperature is 110-120°C, and the treatment time is 4-8h; the melting temperature of the PET slices is 260-270°C, and the melting temperature of the modified PBT product is 280-290°C.
Citation Information
Patent Citations
Molded article, insulating material comprising same, and method for improving electrical-insulating property of polyester resin composition
CN105229079A
Novel polyester sulfhydrylation and modification method
CN107652421A