A quantum dot functional diffusion plate capable of changing white light spectrum and its preparation method and application
Through a three-layer structure perovskite quantum dot functional diffusion plate, the Rb/Cs mixed cation method is used to prepare perovskite quantum dots, which solves the problem of high blue light peak and weak red light in the LED white light spectrum, and achieves spectral stability and wavelength Control and optimize the white light effect.
Patent Information
- Application Number
- CN202410469981.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-18
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-04-18
AI Technical Summary
The existing LED lighting white light spectrum has the problem of high blue light peak and weak red light band, and spectral stability and wavelength control are difficult to achieve in the wavelength range between green light and blue light.
It adopts a three-layer structure of perovskite quantum dot functional diffusion plate. The middle layer contains perovskite quantum dots with a particle size of 1-10nm. It is prepared by the method of Rb/Cs mixed cations, avoiding the halogen in the traditional Cl/Br mixed system. Solve the problem of ion migration and achieve spectral stability and wavelength control.
It effectively regulates blue light emission, achieves spectrum conversion from 450±5nm to 630-680nm, improves spectral stability and light transmittance, avoids halogen phase separation problems, and optimizes the white light effect.
Smart Images

Figure CN118328333B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of optoelectronic display materials, and in particular to a quantum dot functional diffusion plate capable of changing the spectrum of white light, and a preparation method and application thereof. Background Art
[0002] LED semiconductor lighting has entered mass consumption with its advantages of low price, long life and low energy consumption. It can be said that most of the current indoor home and office lighting are semiconductor LED lighting, but its white light emitting principle is that LED blue light excites yellow phosphor to achieve luminescence. The white light spectrum has the disadvantages of high blue light peak and weak red light band (spectrum).
[0003] The most suitable lighting for humans is blackbody radiation (the principle of sunlight), which should also be the result of human biological evolution. The spectrum of blackbody radiation is very wide, from ultraviolet to infrared, and the visible light spectrum is rich. Before the application of LED, the spectrum of incandescent lamps was close to that of the sun.
[0004] The existing technology generally adopts a chlorine-bromine mixed system, and then introduces Cl atoms into the CsPbBr3 system to achieve band gap regulation and thus produce blue light emission. However, perovskite is a typical ionic crystal, and the mixed halogen system is prone to halogen ion migration under conditions such as light and electric field, resulting in the separation of chlorine-rich phase and bromine-rich phase, and the fluorescence spectrum is red-shifted, causing poor spectral stability of the system. In addition, in the existing technology, the standard red, green and blue emission bands are: red light ranges from 620-640nm, green light ranges from 520-540nm and blue light ranges from 450-480nm. There are no reports on methods that have good spectral stability and precise wavelength control in the emission wavelength range of 480-520n between green light and blue light, so it needs to be improved. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a quantum dot functional diffusion plate capable of changing the white light spectrum, wherein the diffusion plate comprises three layers, namely an upper diffusion plate, a middle diffusion plate, and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3;
[0006] The middle diffuser is a diffuser containing perovskite quantum dots; the particle size of the perovskite quantum dots is 1-10 nm;
[0007] The perovskite quantum dots are prepared by a mixed cation method.
[0008] As an embodiment of the present invention, the preparation method of the perovskite quantum dots is as follows:
[0009] Weigh a certain molar amount of rubidium bromide (RbBr), lead bromide (PbBr2), ABr, and LBr and dissolve them in a solvent. Stir them at a certain temperature for 6 hours and then filter them for later use.
[0010] The substrate is placed on a coating machine, and the perovskite precursor solution is dripped onto the surface of the substrate and spin-coated at a certain speed for a certain time. During the spin coating process, a certain amount of anti-solvent is dripped, and then the solvent is removed by annealing, and finally a Rb / Cs mixed cation perovskite film is formed on the surface of the substrate;
[0011] The perovskite film is freeze-dried and then ball-milled in a ball mill to obtain the perovskite quantum dots.
[0012] As an implementation mode of the present invention, the mass content of perovskite quantum dots in the middle diffusion plate is 0.1‰-1‰.
[0013] As an embodiment of the present invention, the raw materials for preparing the upper diffusion plate include resin 1, diffusing agent 1, and auxiliary agent 1; and the diffusing agent 1 is a core-shell structure.
[0014] As an embodiment of the present invention, the raw materials for preparing the lower diffusion plate include resin 2, diffusing agent 2, and auxiliary agent 2; and the diffusing agent 2 is an organic diffusing agent.
[0015] As an embodiment of the present invention, the preparation method of the diffusing agent 1 is as follows:
[0016] The surfactant and deionized water are mixed; styrene, 4-nitrostyrene and azobisisobutyronitrile are then mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then modified silica and methanol are added to obtain an oil phase; under stirring, the oil phase is added dropwise to the reactor to obtain a mixed reaction liquid; the mixed reaction liquid is cured in an oven to obtain the diffusant 1.
[0017] As an embodiment of the present invention, the diffusing agent 2 is an organic silicon light diffusing agent.
[0018] The second aspect of the present invention provides a method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum, the preparation method comprising the following steps:
[0019] After the three layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1, screw 2, and screw 3 at a thickness ratio of 3:4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffuser plate is then cooled and cut into shape.
[0020] The third aspect of the present invention provides a method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum, which is used in the field of LED semiconductor light emitting.
[0021] By adopting the above technical solution, the present invention has the following beneficial effects:
[0022] The band gap is regulated to achieve blue light emission in the form of Rb / Cs mixed cations, rather than the traditional Cl / Br mixed method to achieve blue light emission. Since the halogen ions in the lead halide perovskite are very prone to ion migration, the halogen phase separation causes the spectrum to shift. The present invention is a single halogen system, which can effectively avoid the halogen phase separation problem, thereby ensuring good spectral stability. Using quantum dot materials with special structures, the 630-680 range of this quantum dot spectrum is composed of one or more quantum dots. The characteristic of quantum dots is that they can convert blue light into materials of other spectra. Therefore, the technology of the present invention and the quantum dot material invented can convert blue light (450±5) to 630-680 spectra. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings in the following description are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0024] Figure 1 This is the light source spectrum test result of the plate in Example 1.
[0025] Figure 2 The plate is the same as that in Example 1 (but a common plate without the addition of perovskite material).
[0026] Figure 3 This is the light source spectrum test result of the plate in Example 2-2.
[0027] Figure 4 It is the same plate as Example 2-2 (but a normal plate without adding perovskite material). DETAILED DESCRIPTION
[0028] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] The present invention provides a quantum dot functional diffusion plate capable of changing the spectrum of white light, wherein the diffusion plate comprises three layers, namely, an upper diffusion plate, a middle diffusion plate, and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3. The middle diffusion plate is a diffusion plate containing perovskite quantum dots; the particle size of the perovskite quantum dots is 1-10 nm; and the perovskite quantum dots are prepared by a mixed cation method.
[0030] Upper diffuser plate
[0031] The raw materials for preparing the upper diffusion plate include resin 1, diffusing agent 1, and auxiliary agent 1, and the mass ratio is 1:0.001:0.005.
[0032] The resin 1 is polystyrene.
[0033] The preparation method of the diffusing agent 1 is as follows:
[0034] 1 part by weight of sodium dodecylbenzene sulfonate and 12.5 parts of deionized water are mixed; then 6.35 parts of styrene, 4.75 parts of 4-nitrostyrene, and 0.382 parts of azobisisobutyronitrile are mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then 0.3 parts of modified silicon dioxide and 2.2 parts of methanol are added to obtain an oil phase; under stirring at 800 r / min, the oil phase is added dropwise into the reactor to obtain a mixed emulsion; the mixed emulsion is placed in an oven at 65° C. for curing for 10 hours to obtain the diffusant 1.
[0035] The preparation method of the modified silicon dioxide is as follows: 1 part by weight of nano silicon dioxide powder and 50 parts by weight of solvent are mixed, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified silicon dioxide.
[0036] The nano silicon dioxide powder is a mixed powder of nano silicon dioxide with a particle size of about 10 nm and nano silicon dioxide with a particle size of about 50 nm in a mass ratio of 1:1.
[0037] The raw materials for preparing the additive 1 include: polystyrene, didodecanol ester, and mineral oil, and the mass ratio is 9:0.1:0.002. The preparation method is to extrude and granulate using a twin-screw extruder after mixing.
[0038] Middle diffuser plate
[0039] The raw materials for preparing the middle diffusion plate include: polystyrene and perovskite quantum dots.
[0040] The preparation method of the perovskite quantum dots is as follows:
[0041] S01 Weigh a certain molar amount of rubidium bromide, lead bromide, ABr, and LBr and dissolve them in a solvent. Stir them at a certain temperature for 6 hours and filter them for later use.
[0042] Wherein, the ABr is one or more of CsBr, MABr and FABr; preferably, ABr is CsBr.
[0043] The LBr is one of butylammonium bromide (BABr), octylammonium bromide (OABr), phenethylammonium bromide (PEABr) and phenbutylammonium bromide (PBABr); preferably, the LBr is OABr.
[0044] The concentration of the precursor solution is 0.1-0.4 mol / L, and the preferred concentration is 0.3 mol / L.
[0045] The precursor stirring temperature is 60°C.
[0046] The filter head used for the filtration is a 0.22-0.45 μm organic filter head.
[0047] The S02 substrate is placed on a coating machine, and the perovskite precursor solution is dripped onto the substrate surface and spin-coated at a certain speed for a certain time. During the spin coating process, a certain amount of anti-solvent is dripped, and then the solvent is removed by annealing, and finally a Rb / Cs mixed cation perovskite film is formed on the substrate surface;
[0048] The substrate was ultrasonically cleaned with acetone, deionized water and anhydrous ethanol for 15 minutes in sequence, and then dried with nitrogen. The dried substrate was cleaned in an oxygen plasma cleaner for 10 minutes.
[0049] The spin coating speed is 1500-4000 rpm, preferably 2000 rpm; the spin coating time is 90-180 seconds, preferably 120 seconds.
[0050] The ambient temperature during the spin coating process is 20-40°C, preferably 30-35°C.
[0051] The anti-solvent is one or more of toluene, chlorobenzene, ethyl acetate, dichloromethane, and chloroform; the amount of the anti-solvent added is 0-500 μL, preferably 200 μL. The annealing temperature is 80-150° C., and the annealing time is 5-30 min.
[0052] S03 freeze-drying the perovskite film and then ball-milling it in a ball mill to obtain the perovskite quantum dots.
[0053] Among them, the ball milling beads are zirconium oxide, with a size of 10mm; the ball-to-material ratio is between 30:1; the speed of the ball mill is controlled between 550 rpm, and the ball milling time is 15h.
[0054] In the present invention, before the middle-layer diffuser plate is prepared into a diffuser plate, the perovskite quantum dots need to be granulated, and the specific treatment method is as follows: after mixing 1 part by weight of perovskite quantum dots and 50 parts by weight of solvent, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50°C for 24 hours to obtain the modified perovskite quantum dots.
[0055] Lower diffuser plate
[0056] In the present invention, the raw materials for preparing the lower diffusion plate include resin 2, diffusing agent 2, and auxiliary agent 2, and the mass ratio is 1:0.001:0.002.
[0057] The resin 2 is polystyrene; the diffusing agent 2 is an organic silicon light diffusing agent, specifically HY-7000 spherical silicone resin micropowder produced by Hangzhou Yuheng Technology Co., Ltd. The auxiliary agent 2 is ethylene bis stearamide.
[0058] The second aspect of the present invention provides a method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum, the preparation method comprising the following steps:
[0059] After the three layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1, screw 2, and screw 3 at a thickness ratio of 3:4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffuser plate is then cooled and cut into shape.
[0060] The third aspect of the present invention provides a quantum dot functional diffusion plate capable of changing the white light spectrum, which is used in the field of LED semiconductor light emitting.
[0061] The present invention prepares perovskite film by using Rb / Cs mixed cations, introduces Rb atoms to replace some Cs atoms in CsPbBr3, and realizes band gap regulation by using mixed A-site cations, thus effectively avoiding the halogen phase separation problem of traditional mixed halogen ion system.
[0062] At the same time, when preparing the diffusing agent 1, the present invention selects nano-scale silica of various particle sizes and polystyrene to form a core-shell structure, and at the same time, the surface of the silica is hydrophobically modified, so that in the core-shell structure obtained, the polystyrene shell layer contains multiple silicas. At the same time, the surface of the internal silica is hydrophobically modified, so that there are certain pores between the silicas in the core layer, so that the prepared upper diffuser has excellent light transmittance and haze.
[0063] At the same time, the perovskite quantum dots prepared by the present invention can avoid the halogen phase separation problem of the traditional mixed halogen ion system, and have a certain ability to resist oxygen and moisture; in addition, if only the middle-layer diffuser is used, its light transmittance is not very good; after the perovskite quantum dots are modified, a diffuser with good light transmittance and excellent white light effect can be obtained.
[0064] The present invention is further explained below in conjunction with specific implementation modes.
[0065] Example 1
[0066] This embodiment provides a quantum dot functional diffusion plate capable of changing the spectrum of white light. The diffusion plate comprises three layers, namely an upper diffusion plate, a middle diffusion plate, and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3.
[0067] The raw materials for preparing the upper diffusion plate include polystyrene, diffusing agent 1, and auxiliary agent 1, and the mass ratio is 1:0.001:0.005.
[0068] The preparation method of the diffusing agent 1 is as follows:
[0069] 1 part by weight of sodium dodecylbenzene sulfonate and 12.5 parts of deionized water are mixed; then 6.35 parts of styrene, 4.75 parts of 4-nitrostyrene, and 0.382 parts of azobisisobutyronitrile are mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then 0.3 parts of modified silicon dioxide and 2.2 parts of methanol are added to obtain an oil phase; under stirring at 800 r / min, the oil phase is added dropwise into the reactor to obtain a mixed emulsion; the mixed emulsion is placed in an oven at 65° C. for curing for 10 hours to obtain the diffusant 1.
[0070] The preparation method of the modified silicon dioxide is as follows: 1 part by weight of nano silicon dioxide powder and 50 parts by weight of solvent are mixed, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified silicon dioxide.
[0071] The nano silicon dioxide powder is a mixed powder of nano silicon dioxide with a particle size of about 10 nm and nano silicon dioxide with a particle size of about 50 nm in a mass ratio of 1:1.
[0072] The raw materials for preparing the additive 1 include: polystyrene, didodecanol ester, and mineral oil, and the mass ratio is 9:0.1:0.002. The preparation method is to extrude and granulate using a twin-screw extruder after mixing.
[0073] The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001.
[0074] The preparation method of the perovskite quantum dots is as follows:
[0075] 0.3mmol of lead bromide (PbBr2), 0.09mmol of cesium bromide (CsBr), 0.21mmol of rubidium bromide (RbBr) and 0.03mmol of octylammonium bromide (OABr) were dissolved in 1mL of dimethyl sulfoxide (DMSO), stirred at 60℃ for 6 hours to obtain a perovskite precursor solution, and the obtained solution was filtered for use. The quartz glass substrate was ultrasonically cleaned in acetone, deionized water and anhydrous ethanol for 15min in turn, and then dried under nitrogen for use. The quartz substrate was placed on a coater, 50μL of the perovskite precursor solution was dripped on the quartz substrate, and spin-coated at 2000 rpm for 2min. After the coater was completed, it was placed on a hot plate and annealed at 130℃ for 10min to obtain a Rb / Cs mixed cation perovskite film.
[0076] The perovskite film is freeze-dried and then ball-milled in a ball mill to obtain the perovskite quantum dots.
[0077] Among them, the ball milling beads are zirconium oxide, with a size of 10mm; the ball-to-material ratio is between 30:1; the speed of the ball mill is controlled between 550 rpm, and the ball milling time is 15h.
[0078] Before the middle-layer diffuser plate is prepared into a diffuser plate, the perovskite quantum dots need to be granulated, and the specific treatment method is as follows: after mixing 1 part by weight of perovskite quantum dots and 50 parts by weight of solvent, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50°C for 24 hours to obtain modified perovskite quantum dots.
[0079] The raw materials for preparing the lower diffuser plate include polystyrene, diffuser 2, and ethylene bis stearamide, and the mass ratio is 1:0.001:0.002. The diffuser 2 is an organic silicon light diffuser, specifically HY-7000 spherical silicone resin micropowder from Hangzhou Yuheng Technology Co., Ltd.
[0080] The method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum comprises the following steps:
[0081] After the three layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1, screw 2, and screw 3 at a thickness ratio of 3:4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffuser plate is then cooled and cut into shape.
[0082] Example 2-1
[0083] This embodiment provides a quantum dot functional diffusion plate capable of changing the spectrum of white light. The diffusion plate comprises three layers, namely an upper diffusion plate, a middle diffusion plate, and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3.
[0084] The raw materials for preparing the upper diffusion plate include polystyrene, diffusing agent 1, and auxiliary agent 1, and the mass ratio is 1:0.001:0.005.
[0085] The diffusing agent 1 is modified silicon dioxide.
[0086] The preparation method of the modified silicon dioxide is as follows: 1 part by weight of nano silicon dioxide powder and 50 parts by weight of solvent are mixed, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified silicon dioxide.
[0087] The nano silicon dioxide powder is a mixed powder of nano silicon dioxide with a particle size of about 10 nm and nano silicon dioxide with a particle size of about 50 nm in a mass ratio of 1:1.
[0088] The raw materials for preparing the additive 1 include: polystyrene, didodecanol ester, and mineral oil, and the mass ratio is 9:0.1:0.002. The preparation method is to extrude and granulate using a twin-screw extruder after mixing.
[0089] The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001.
[0090] The preparation method of the perovskite quantum dots is as follows:
[0091] 0.3mmol of lead bromide (PbBr2), 0.09mmol of cesium bromide (CsBr), 0.21mmol of rubidium bromide (RbBr) and 0.03mmol of octylammonium bromide (OABr) were dissolved in 1mL of dimethyl sulfoxide (DMSO), stirred at 60℃ for 6 hours to obtain a perovskite precursor solution, and the obtained solution was filtered for use. The quartz glass substrate was ultrasonically cleaned in acetone, deionized water and anhydrous ethanol for 15min in turn, and then dried under nitrogen for use. The quartz substrate was placed on a coater, 50μL of the perovskite precursor solution was dripped on the quartz substrate, and spin-coated at 2000 rpm for 2min. After the coater was completed, it was placed on a hot plate and annealed at 130℃ for 10min to obtain a Rb / Cs mixed cation perovskite film.
[0092] The perovskite film is freeze-dried and then ball-milled in a ball mill to obtain the perovskite quantum dots.
[0093] Among them, the ball milling beads are zirconium oxide, with a size of 10mm; the ball-to-material ratio is between 30:1; the speed of the ball mill is controlled between 550 rpm, and the ball milling time is 15h.
[0094] Before the middle-layer diffuser plate is prepared into a diffuser plate, the perovskite quantum dots need to be granulated, and the specific treatment method is as follows: after mixing 1 part by weight of perovskite quantum dots and 50 parts by weight of solvent, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50°C for 24 hours to obtain modified perovskite quantum dots.
[0095] The raw materials for preparing the lower diffuser plate include polystyrene, diffuser 2, and ethylene bis stearamide, and the mass ratio is 1:0.001:0.002. The diffuser 2 is an organic silicon light diffuser, specifically HY-7000 spherical silicone resin micropowder from Hangzhou Yuheng Technology Co., Ltd.
[0096] The method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum comprises the following steps:
[0097] After the three layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1, screw 2, and screw 3 at a thickness ratio of 3:4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffuser plate is then cooled and cut into shape.
[0098] Example 2-2
[0099] This embodiment provides a quantum dot functional diffusion plate capable of changing the spectrum of white light. The diffusion plate comprises three layers, namely an upper diffusion plate, a middle diffusion plate, and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3.
[0100] The raw materials for preparing the upper diffusion plate include polystyrene, diffusing agent 1, and auxiliary agent 1, and the mass ratio is 1:0.001:0.005.
[0101] The preparation method of the diffusing agent 1 is as follows:
[0102] 1 part by weight of sodium dodecylbenzene sulfonate and 12.5 parts of deionized water are mixed; then 6.35 parts of styrene, 4.75 parts of 4-nitrostyrene, and 0.382 parts of azobisisobutyronitrile are mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then 0.3 parts of modified silicon dioxide and 2.2 parts of methanol are added to obtain an oil phase; under stirring at 800 r / min, the oil phase is added dropwise into the reactor to obtain a mixed emulsion; the mixed emulsion is placed in an oven at 65° C. for curing for 10 hours to obtain the diffusant 1.
[0103] The preparation method of the modified silicon dioxide is as follows: 1 part by weight of nano silicon dioxide powder and 50 parts by weight of solvent are mixed, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified silicon dioxide.
[0104] The nano silicon dioxide powder is nano silicon dioxide with a particle size of about 10 nm.
[0105] The raw materials for preparing the additive 1 include: polystyrene, didodecanol ester, and mineral oil, and the mass ratio is 9:0.1:0.002. The preparation method is to extrude and granulate using a twin-screw extruder after mixing.
[0106] The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001.
[0107] The preparation method of the perovskite quantum dots is as follows:
[0108] 0.3mmol of lead bromide (PbBr2), 0.09mmol of cesium bromide (CsBr), 0.21mmol of rubidium bromide (RbBr) and 0.03mmol of octylammonium bromide (OABr) were dissolved in 1mL of dimethyl sulfoxide (DMSO), stirred at 60℃ for 6 hours to obtain a perovskite precursor solution, and the obtained solution was filtered for use. The quartz glass substrate was ultrasonically cleaned in acetone, deionized water and anhydrous ethanol for 15min in turn, and then dried under nitrogen for use. The quartz substrate was placed on a coater, 50μL of the perovskite precursor solution was dripped on the quartz substrate, and spin-coated at 2000 rpm for 2min. After the coater was completed, it was placed on a hot plate and annealed at 130℃ for 10min to obtain a Rb / Cs mixed cation perovskite film.
[0109] The perovskite film is freeze-dried and then ball-milled in a ball mill to obtain the perovskite quantum dots.
[0110] Among them, the ball milling beads are zirconium oxide, with a size of 10mm; the ball-to-material ratio is between 30:1; the speed of the ball mill is controlled between 550 rpm, and the ball milling time is 15h.
[0111] Before the middle-layer diffuser plate is prepared into a diffuser plate, the perovskite quantum dots need to be granulated, and the specific treatment method is as follows: after mixing 1 part by weight of perovskite quantum dots and 50 parts by weight of solvent, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50°C for 24 hours to obtain modified perovskite quantum dots.
[0112] The raw materials for preparing the lower diffuser plate include polystyrene, diffuser 2, and ethylene bis stearamide, and the mass ratio is 1:0.001:0.002. The diffuser 2 is an organic silicon light diffuser, specifically HY-7000 spherical silicone resin micropowder from Hangzhou Yuheng Technology Co., Ltd.
[0113] The method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum comprises the following steps:
[0114] After the three layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1, screw 2, and screw 3 at a thickness ratio of 3:4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffuser plate is then cooled and cut into shape.
[0115] Example 2-3
[0116] This embodiment provides a quantum dot functional diffusion plate capable of changing the spectrum of white light. The diffusion plate comprises three layers, namely an upper diffusion plate, a middle diffusion plate, and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3.
[0117] The raw materials for preparing the upper diffusion plate include polystyrene, diffusing agent 1, and auxiliary agent 1, and the mass ratio is 1:0.001:0.005.
[0118] The preparation method of the diffusing agent 1 is as follows:
[0119] 1 part by weight of sodium dodecylbenzene sulfonate and 12.5 parts of deionized water are mixed; then 6.35 parts of styrene, 4.75 parts of 4-nitrostyrene, and 0.382 parts of azobisisobutyronitrile are mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then 0.3 parts of silicon dioxide and 2.2 parts of methanol are added to obtain an oil phase; under stirring at 800 r / min, the oil phase is added dropwise into the reactor to obtain a mixed emulsion; the mixed emulsion is placed in an oven at 65° C. for curing for 10 hours to obtain the diffusant 1.
[0120] The silicon dioxide is a mixed powder of nano silicon dioxide with a particle size of about 10 nm and nano silicon dioxide with a particle size of about 50 nm in a mass ratio of 1:1.
[0121] The raw materials for preparing the additive 1 include: polystyrene, didodecanol ester, and mineral oil, and the mass ratio is 9:0.1:0.002. The preparation method is to extrude and granulate using a twin-screw extruder after mixing.
[0122] The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001.
[0123] The preparation method of the perovskite quantum dots is as follows:
[0124] 0.3mmol of lead bromide (PbBr2), 0.09mmol of cesium bromide (CsBr), 0.21mmol of rubidium bromide (RbBr) and 0.03mmol of octylammonium bromide (OABr) were dissolved in 1mL of dimethyl sulfoxide (DMSO), stirred at 60℃ for 6 hours to obtain a perovskite precursor solution, and the obtained solution was filtered for use. The quartz glass substrate was ultrasonically cleaned in acetone, deionized water and anhydrous ethanol for 15min in turn, and then dried under nitrogen for use. The quartz substrate was placed on a coater, 50μL of the perovskite precursor solution was dripped on the quartz substrate, and spin-coated at 2000 rpm for 2min. After the coater was completed, it was placed on a hot plate and annealed at 130℃ for 10min to obtain a Rb / Cs mixed cation perovskite film.
[0125] The perovskite film is freeze-dried and then ball-milled in a ball mill to obtain the perovskite quantum dots.
[0126] Among them, the ball milling beads are zirconium oxide, with a size of 10mm; the ball-to-material ratio is between 30:1; the speed of the ball mill is controlled between 550 rpm, and the ball milling time is 15h.
[0127] Before the middle-layer diffuser plate is prepared into a diffuser plate, the perovskite quantum dots need to be granulated, and the specific treatment method is as follows: after mixing 1 part by weight of perovskite quantum dots and 50 parts by weight of solvent, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50°C for 24 hours to obtain modified perovskite quantum dots.
[0128] The raw materials for preparing the lower diffuser plate include polystyrene, diffuser 2, and ethylene bis stearamide, and the mass ratio is 1:0.001:0.002. The diffuser 2 is an organic silicon light diffuser, specifically HY-7000 spherical silicone resin micropowder from Hangzhou Yuheng Technology Co., Ltd.
[0129] The method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum comprises the following steps:
[0130] After the three layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1, screw 2, and screw 3 at a thickness ratio of 3:4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffuser plate is then cooled and cut into shape.
[0131] Embodiment 2-4
[0132] This embodiment provides a quantum dot functional diffusion plate capable of changing the spectrum of white light. The diffusion plate comprises three layers, namely an upper diffusion plate, a middle diffusion plate, and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3.
[0133] The raw materials for preparing the upper diffusion plate include polystyrene, diffusing agent 1, and auxiliary agent 1, and the mass ratio is 1:0.001:0.005.
[0134] The preparation method of the diffusing agent 1 is as follows:
[0135] 1 part by weight of sodium dodecylbenzene sulfonate and 12.5 parts of deionized water are mixed; then 6.35 parts of styrene, 4.75 parts of divinylbenzene, and 0.382 parts of azobisisobutyronitrile are mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then 0.3 parts of modified silicon dioxide and 2.2 parts of methanol are added to obtain an oil phase; under stirring at 800 r / min, the oil phase is added dropwise into the reactor to obtain a mixed emulsion; the mixed emulsion is placed in an oven at 65° C. for curing for 10 hours to obtain the diffusant 1.
[0136] The preparation method of the modified silicon dioxide is as follows: 1 part by weight of nano silicon dioxide powder and 50 parts by weight of solvent are mixed, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified silicon dioxide.
[0137] The nano silicon dioxide powder is a mixed powder of nano silicon dioxide with a particle size of about 10 nm and nano silicon dioxide with a particle size of about 50 nm in a mass ratio of 1:1.
[0138] The raw materials for preparing the additive 1 include: polystyrene, didodecanol ester, and mineral oil, and the mass ratio is 9:0.1:0.002. The preparation method is to extrude and granulate using a twin-screw extruder after mixing.
[0139] The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001.
[0140] The preparation method of the perovskite quantum dots is as follows:
[0141] 0.3mmol of lead bromide (PbBr2), 0.09mmol of cesium bromide (CsBr), 0.21mmol of rubidium bromide (RbBr) and 0.03mmol of octylammonium bromide (OABr) were dissolved in 1mL of dimethyl sulfoxide (DMSO), stirred at 60℃ for 6 hours to obtain a perovskite precursor solution, and the obtained solution was filtered for use. The quartz glass substrate was ultrasonically cleaned in acetone, deionized water and anhydrous ethanol for 15min in turn, and then dried under nitrogen for use. The quartz substrate was placed on a coater, 50μL of the perovskite precursor solution was dripped on the quartz substrate, and spin-coated at 2000 rpm for 2min. After the coater was completed, it was placed on a hot plate and annealed at 130℃ for 10min to obtain a Rb / Cs mixed cation perovskite film.
[0142] The perovskite film is freeze-dried and then ball-milled in a ball mill to obtain the perovskite quantum dots.
[0143] Among them, the ball milling beads are zirconium oxide, with a size of 10mm; the ball-to-material ratio is between 30:1; the speed of the ball mill is controlled between 550 rpm, and the ball milling time is 15h.
[0144] Before the middle-layer diffuser plate is prepared into a diffuser plate, the perovskite quantum dots need to be granulated, and the specific treatment method is as follows: after mixing 1 part by weight of perovskite quantum dots and 50 parts by weight of solvent, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50°C for 24 hours to obtain modified perovskite quantum dots.
[0145] The raw materials for preparing the lower diffuser plate include polystyrene, diffuser 2, and ethylene bis stearamide, and the mass ratio is 1:0.001:0.002. The diffuser 2 is an organic silicon light diffuser, specifically HY-7000 spherical silicone resin micropowder from Hangzhou Yuheng Technology Co., Ltd.
[0146] The method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum comprises the following steps:
[0147] After the three layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1, screw 2, and screw 3 at a thickness ratio of 3:4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffuser plate is then cooled and cut into shape.
[0148] Example 3-1
[0149] This embodiment provides a quantum dot functional diffusion plate capable of changing the spectrum of white light. The diffusion plate comprises three layers, namely an upper diffusion plate, a middle diffusion plate, and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3.
[0150] The raw materials for preparing the upper diffusion plate include polystyrene, diffusing agent 1, and auxiliary agent 1, and the mass ratio is 1:0.001:0.005.
[0151] The preparation method of the diffusing agent 1 is as follows:
[0152] 1 part by weight of sodium dodecylbenzene sulfonate and 12.5 parts of deionized water are mixed; then 6.35 parts of styrene, 4.75 parts of 4-nitrostyrene, and 0.382 parts of azobisisobutyronitrile are mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then 0.3 parts of modified silicon dioxide and 2.2 parts of methanol are added to obtain an oil phase; under stirring at 800 r / min, the oil phase is added dropwise into the reactor to obtain a mixed emulsion; the mixed emulsion is placed in an oven at 65° C. for curing for 10 hours to obtain the diffusant 1.
[0153] The preparation method of the modified silicon dioxide is as follows: 1 part by weight of nano silicon dioxide powder and 50 parts by weight of solvent are mixed, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified silicon dioxide.
[0154] The nano silicon dioxide powder is a mixed powder of nano silicon dioxide with a particle size of about 10 nm and nano silicon dioxide with a particle size of about 50 nm in a mass ratio of 1:1.
[0155] The raw materials for preparing the additive 1 include: polystyrene, didodecanol ester, and mineral oil, and the mass ratio is 9:0.1:0.002. The preparation method is to extrude and granulate using a twin-screw extruder after mixing.
[0156] The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001.
[0157] The preparation method of the perovskite quantum dots is as follows:
[0158] 0.3mmol of lead bromide (PbBr2), 0.09mmol of cesium bromide (CsBr), 0.21mmol of rubidium bromide (RbBr) and 0.03mmol of octylammonium bromide (OABr) were dissolved in 1mL of dimethyl sulfoxide (DMSO), stirred at 60°C for 6 hours to obtain a perovskite precursor solution, and the obtained solution was filtered for use. The quartz glass substrate was ultrasonically cleaned in acetone, deionized water and anhydrous ethanol for 15 minutes in turn, and then dried under nitrogen for use. The quartz substrate was placed on a sizing machine, 50μL of the perovskite precursor solution was dripped on the quartz substrate, and spin-coated at 2000 rpm for 2 minutes. After the sizing was completed, it was placed on a heating plate and annealed at 130°C for 10 minutes to obtain a Rb / Cs mixed cation perovskite film. After the prepared perovskite film was freeze-dried, the perovskite quantum dots were obtained.
[0159] Before the middle-layer diffuser plate is prepared into a diffuser plate, the perovskite quantum dots need to be granulated, and the specific treatment method is as follows: after mixing 1 part by weight of perovskite quantum dots and 50 parts by weight of solvent, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50°C for 24 hours to obtain modified perovskite quantum dots.
[0160] The raw materials for preparing the lower diffuser plate include polystyrene, diffuser 2, and ethylene bis stearamide, and the mass ratio is 1:0.001:0.002. The diffuser 2 is an organic silicon light diffuser, specifically HY-7000 spherical silicone resin micropowder from Hangzhou Yuheng Technology Co., Ltd.
[0161] The method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum comprises the following steps:
[0162] After the three layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1, screw 2, and screw 3 at a thickness ratio of 3:4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffuser plate is then cooled and cut into shape.
[0163] Example 3-2
[0164] This embodiment provides a quantum dot functional diffusion plate capable of changing the spectrum of white light. The diffusion plate comprises three layers, namely an upper diffusion plate, a middle diffusion plate, and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3.
[0165] The raw materials for preparing the upper diffusion plate include polystyrene, diffusing agent 1, and auxiliary agent 1, and the mass ratio is 1:0.001:0.005.
[0166] The preparation method of the diffusing agent 1 is as follows:
[0167] 1 part by weight of sodium dodecylbenzene sulfonate and 12.5 parts of deionized water are mixed; then 6.35 parts of styrene, 4.75 parts of 4-nitrostyrene, and 0.382 parts of azobisisobutyronitrile are mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then 0.3 parts of modified silicon dioxide and 2.2 parts of methanol are added to obtain an oil phase; under stirring at 800 r / min, the oil phase is added dropwise into the reactor to obtain a mixed emulsion; the mixed emulsion is placed in an oven at 65° C. for curing for 10 hours to obtain the diffusant 1.
[0168] The preparation method of the modified silicon dioxide is as follows: 1 part by weight of nano silicon dioxide powder and 50 parts by weight of solvent are mixed, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified silicon dioxide.
[0169] The nano silicon dioxide powder is a mixed powder of nano silicon dioxide with a particle size of about 10 nm and nano silicon dioxide with a particle size of about 50 nm in a mass ratio of 1:1.
[0170] The raw materials for preparing the additive 1 include: polystyrene, didodecanol ester, and mineral oil, and the mass ratio is 9:0.1:0.002. The preparation method is to extrude and granulate using a twin-screw extruder after mixing.
[0171] The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001.
[0172] The preparation method of the perovskite quantum dots is as follows:
[0173] 0.3 mmol of lead bromide (PbBr2), 0.09 mmol of cesium bromide (CsBr), 0.21 mmol of rubidium bromide (RbBr) and 0.03 mmol of octylammonium bromide (OABr) were dissolved in 1 mL of dimethyl sulfoxide (DMSO), stirred at 60 ° C for 6 hours to obtain a perovskite precursor solution, and the obtained solution was filtered and placed in a polytetrafluoroethylene reactor, and calcined at 130 ° C for 30 min to obtain Rb / Cs mixed cation perovskite quantum dots.
[0174] Before the middle-layer diffuser plate is prepared into a diffuser plate, the perovskite quantum dots need to be granulated, and the specific treatment method is as follows: after mixing 1 part by weight of perovskite quantum dots and 50 parts by weight of solvent, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50°C for 24 hours to obtain modified perovskite quantum dots.
[0175] The raw materials for preparing the lower diffuser plate include polystyrene, diffuser 2, and ethylene bis stearamide, and the mass ratio is 1:0.001:0.002. The diffuser 2 is an organic silicon light diffuser, specifically HY-7000 spherical silicone resin micropowder from Hangzhou Yuheng Technology Co., Ltd.
[0176] The method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum comprises the following steps:
[0177] After the three layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1, screw 2, and screw 3 at a thickness ratio of 3:4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffuser plate is then cooled and cut into shape.
[0178] Example 3-3
[0179] This embodiment provides a quantum dot functional diffusion plate capable of changing the spectrum of white light. The diffusion plate comprises three layers, namely an upper diffusion plate, a middle diffusion plate, and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3.
[0180] The raw materials for preparing the upper diffusion plate include polystyrene, diffusing agent 1, and auxiliary agent 1, and the mass ratio is 1:0.001:0.005.
[0181] The preparation method of the diffusing agent 1 is as follows:
[0182] 1 part by weight of sodium dodecylbenzene sulfonate and 12.5 parts of deionized water are mixed; then 6.35 parts of styrene, 4.75 parts of 4-nitrostyrene, and 0.382 parts of azobisisobutyronitrile are mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then 0.3 parts of modified silicon dioxide and 2.2 parts of methanol are added to obtain an oil phase; under stirring at 800 r / min, the oil phase is added dropwise into the reactor to obtain a mixed emulsion; the mixed emulsion is placed in an oven at 65° C. for curing for 10 hours to obtain the diffusant 1.
[0183] The preparation method of the modified silicon dioxide is as follows: 1 part by weight of nano silicon dioxide powder and 50 parts by weight of solvent are mixed, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified silicon dioxide.
[0184] The nano silicon dioxide powder is a mixed powder of nano silicon dioxide with a particle size of about 10 nm and nano silicon dioxide with a particle size of about 50 nm in a mass ratio of 1:1.
[0185] The raw materials for preparing the additive 1 include: polystyrene, didodecanol ester, and mineral oil, and the mass ratio is 9:0.1:0.002. The preparation method is to extrude and granulate using a twin-screw extruder after mixing.
[0186] The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001.
[0187] The preparation method of the perovskite quantum dots refers to the preparation method of Example 1 in patent CN116904184A.
[0188] Before the middle-layer diffuser plate is prepared into a diffuser plate, the perovskite quantum dots need to be granulated, and the specific treatment method is as follows: after mixing 1 part by weight of perovskite quantum dots and 50 parts by weight of solvent, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50°C for 24 hours to obtain modified perovskite quantum dots.
[0189] The raw materials for preparing the lower diffuser plate include polystyrene, diffuser 2, and ethylene bis stearamide, and the mass ratio is 1:0.001:0.002. The diffuser 2 is an organic silicon light diffuser, specifically HY-7000 spherical silicone resin micropowder from Hangzhou Yuheng Technology Co., Ltd.
[0190] The method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum comprises the following steps:
[0191] After the three layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1, screw 2, and screw 3 at a thickness ratio of 3:4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffuser plate is then cooled and cut into shape.
[0192] Embodiment 3-4
[0193] This embodiment provides a quantum dot functional diffusion plate capable of changing the spectrum of white light. The diffusion plate comprises three layers, namely an upper diffusion plate, a middle diffusion plate, and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3.
[0194] The raw materials for preparing the upper diffusion plate include polystyrene, diffusing agent 1, and auxiliary agent 1, and the mass ratio is 1:0.001:0.005.
[0195] The preparation method of the diffusing agent 1 is as follows:
[0196] 1 part by weight of sodium dodecylbenzene sulfonate and 12.5 parts of deionized water are mixed; then 6.35 parts of styrene, 4.75 parts of 4-nitrostyrene, and 0.382 parts of azobisisobutyronitrile are mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then 0.3 parts of modified silicon dioxide and 2.2 parts of methanol are added to obtain an oil phase; under stirring at 800 r / min, the oil phase is added dropwise into the reactor to obtain a mixed emulsion; the mixed emulsion is placed in an oven at 65° C. for curing for 10 hours to obtain the diffusant 1.
[0197] The preparation method of the modified silicon dioxide is as follows: 1 part by weight of nano silicon dioxide powder and 50 parts by weight of solvent are mixed, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified silicon dioxide.
[0198] The nano silicon dioxide powder is a mixed powder of nano silicon dioxide with a particle size of about 10 nm and nano silicon dioxide with a particle size of about 50 nm in a mass ratio of 1:1.
[0199] The raw materials for preparing the additive 1 include: polystyrene, didodecanol ester, and mineral oil, and the mass ratio is 9:0.1:0.002. The preparation method is to extrude and granulate using a twin-screw extruder after mixing.
[0200] The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001.
[0201] The preparation method of the perovskite quantum dots is as follows:
[0202] 0.3mmol of lead bromide (PbBr2), 0.09mmol of cesium bromide (CsBr), 0.21mmol of rubidium bromide (RbBr) and 0.03mmol of octylammonium bromide (OABr) were dissolved in 1mL of dimethyl sulfoxide (DMSO), stirred at 60℃ for 6 hours to obtain a perovskite precursor solution, and the obtained solution was filtered for use. The quartz glass substrate was ultrasonically cleaned in acetone, deionized water and anhydrous ethanol for 15min in turn, and then dried under nitrogen for use. The quartz substrate was placed on a coater, 50μL of the perovskite precursor solution was dripped on the quartz substrate, and spin-coated at 2000 rpm for 2min. After the coater was completed, it was placed on a hot plate and annealed at 130℃ for 10min to obtain a Rb / Cs mixed cation perovskite film.
[0203] The perovskite film is freeze-dried and then ball-milled in a ball mill to obtain the perovskite quantum dots.
[0204] Among them, the ball milling beads are zirconium oxide, with a size of 10mm; the ball-to-material ratio is between 30:1; the speed of the ball mill is controlled between 550 rpm, and the ball milling time is 15h.
[0205] The raw materials for preparing the lower diffuser plate include polystyrene, diffuser 2, and ethylene bis stearamide, and the mass ratio is 1:0.001:0.002. The diffuser 2 is an organic silicon light diffuser, specifically HY-7000 spherical silicone resin micropowder from Hangzhou Yuheng Technology Co., Ltd.
[0206] The method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum comprises the following steps:
[0207] After the three layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1, screw 2, and screw 3 at a thickness ratio of 3:4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffuser plate is then cooled and cut into shape.
[0208] Example 4-1
[0209] This embodiment provides a quantum dot functional diffusion plate capable of changing the spectrum of white light. The diffusion plate comprises three layers, namely an upper diffusion plate, a middle diffusion plate, and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3.
[0210] The raw materials for preparing the lower diffusion plate include polystyrene, diffusing agent 1, and auxiliary agent 1, and the mass ratio is 1:0.001:0.005.
[0211] The preparation method of the diffusing agent 1 is as follows:
[0212] 1 part by weight of sodium dodecylbenzene sulfonate and 12.5 parts of deionized water are mixed; then 6.35 parts of styrene, 4.75 parts of 4-nitrostyrene, and 0.382 parts of azobisisobutyronitrile are mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then 0.3 parts of modified silicon dioxide and 2.2 parts of methanol are added to obtain an oil phase; under stirring at 800 r / min, the oil phase is added dropwise into the reactor to obtain a mixed emulsion; the mixed emulsion is placed in an oven at 65° C. for curing for 10 hours to obtain the diffusant 1.
[0213] The preparation method of the modified silicon dioxide is as follows: 1 part by weight of nano silicon dioxide powder and 50 parts by weight of solvent are mixed, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified silicon dioxide.
[0214] The nano silicon dioxide powder is a mixed powder of nano silicon dioxide with a particle size of about 10 nm and nano silicon dioxide with a particle size of about 50 nm in a mass ratio of 1:1.
[0215] The raw materials for preparing the additive 1 include: polystyrene, didodecanol ester, and mineral oil, and the mass ratio is 9:0.1:0.002. The preparation method is to extrude and granulate using a twin-screw extruder after mixing.
[0216] The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001.
[0217] The preparation method of the perovskite quantum dots is as follows:
[0218] 0.3mmol of lead bromide (PbBr2), 0.09mmol of cesium bromide (CsBr), 0.21mmol of rubidium bromide (RbBr) and 0.03mmol of octylammonium bromide (OABr) were dissolved in 1mL of dimethyl sulfoxide (DMSO), stirred at 60℃ for 6 hours to obtain a perovskite precursor solution, and the obtained solution was filtered for use. The quartz glass substrate was ultrasonically cleaned in acetone, deionized water and anhydrous ethanol for 15min in turn, and then dried under nitrogen for use. The quartz substrate was placed on a coater, 50μL of the perovskite precursor solution was dripped on the quartz substrate, and spin-coated at 2000 rpm for 2min. After the coater was completed, it was placed on a hot plate and annealed at 130℃ for 10min to obtain a Rb / Cs mixed cation perovskite film.
[0219] The perovskite film is freeze-dried and then ball-milled in a ball mill to obtain the perovskite quantum dots.
[0220] Among them, the ball milling beads are zirconium oxide, with a size of 10mm; the ball-to-material ratio is between 30:1; the speed of the ball mill is controlled between 550 rpm, and the ball milling time is 15h.
[0221] Before the middle-layer diffuser plate is prepared into a diffuser plate, the perovskite quantum dots need to be granulated, and the specific treatment method is as follows: after mixing 1 part by weight of perovskite quantum dots and 50 parts by weight of solvent, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50°C for 24 hours to obtain modified perovskite quantum dots.
[0222] The raw materials for preparing the upper diffusion plate include polystyrene, diffusing agent 2, and ethylene bis stearamide, and the mass ratio is 1:0.001:0.002. The diffusing agent 2 is an organic silicon light diffusing agent, specifically HY-7000 spherical silicone resin micropowder of Hangzhou Yuheng Technology Co., Ltd.
[0223] The method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum comprises the following steps:
[0224] After the three layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1, screw 2, and screw 3 at a thickness ratio of 3:4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffuser plate is then cooled and cut into shape.
[0225] Example 4-2
[0226] This embodiment provides a quantum dot functional diffusion plate capable of changing the spectrum of white light. The diffusion plate comprises two layers, namely a middle diffusion plate and a lower diffusion plate; and the thickness ratio of the two layers is 4:3.
[0227] The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001.
[0228] The preparation method of the perovskite quantum dots is as follows:
[0229] 0.3mmol of lead bromide (PbBr2), 0.09mmol of cesium bromide (CsBr), 0.21mmol of rubidium bromide (RbBr) and 0.03mmol of octylammonium bromide (OABr) were dissolved in 1mL of dimethyl sulfoxide (DMSO), stirred at 60℃ for 6 hours to obtain a perovskite precursor solution, and the obtained solution was filtered for use. The quartz glass substrate was ultrasonically cleaned in acetone, deionized water and anhydrous ethanol for 15min in turn, and then dried under nitrogen for use. The quartz substrate was placed on a coater, 50μL of the perovskite precursor solution was dripped on the quartz substrate, and spin-coated at 2000 rpm for 2min. After the coater was completed, it was placed on a hot plate and annealed at 130℃ for 10min to obtain a Rb / Cs mixed cation perovskite film.
[0230] The perovskite film is freeze-dried and then ball-milled in a ball mill to obtain the perovskite quantum dots.
[0231] Among them, the ball milling beads are zirconium oxide, with a size of 10mm; the ball-to-material ratio is between 30:1; the speed of the ball mill is controlled between 550 rpm, and the ball milling time is 15h.
[0232] Before the middle-layer diffuser plate is prepared into a diffuser plate, the perovskite quantum dots need to be granulated, and the specific treatment method is as follows: after mixing 1 part by weight of perovskite quantum dots and 50 parts by weight of solvent, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50°C for 24 hours to obtain modified perovskite quantum dots.
[0233] The raw materials for preparing the lower diffuser plate include polystyrene, diffuser 2, and ethylene bis stearamide, and the mass ratio is 1:0.001:0.002. The diffuser 2 is an organic silicon light diffuser, specifically HY-7000 spherical silicone resin micropowder from Hangzhou Yuheng Technology Co., Ltd.
[0234] The method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum comprises the following steps:
[0235] After the two layers of raw materials are mixed and dispersed evenly, they are extruded through screw 2 and screw 3 at a thickness ratio of 4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffusion plate is then cooled and cut into shape.
[0236] Example 4-3
[0237] This embodiment provides a quantum dot functional diffusion plate capable of changing the spectrum of white light. The diffusion plate comprises two layers, namely an upper diffusion plate and a middle diffusion plate; and the thickness ratio of the two layers is 3:4.
[0238] The raw materials for preparing the upper diffusion plate include polystyrene, diffusing agent 1, and auxiliary agent 1, and the mass ratio is 1:0.001:0.005.
[0239] The preparation method of the diffusing agent 1 is as follows:
[0240] 1 part by weight of sodium dodecylbenzene sulfonate and 12.5 parts of deionized water are mixed; then 6.35 parts of styrene, 4.75 parts of 4-nitrostyrene, and 0.382 parts of azobisisobutyronitrile are mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then 0.3 parts of modified silicon dioxide and 2.2 parts of methanol are added to obtain an oil phase; under stirring at 800 r / min, the oil phase is added dropwise into the reactor to obtain a mixed emulsion; the mixed emulsion is placed in an oven at 65° C. for curing for 10 hours to obtain the diffusant 1.
[0241] The preparation method of the modified silicon dioxide is as follows: 1 part by weight of nano silicon dioxide powder and 50 parts by weight of solvent are mixed, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified silicon dioxide.
[0242] The nano silicon dioxide powder is a mixed powder of nano silicon dioxide with a particle size of about 10 nm and nano silicon dioxide with a particle size of about 50 nm in a mass ratio of 1:1.
[0243] The raw materials for preparing the additive 1 include: polystyrene, didodecanol ester, and mineral oil, and the mass ratio is 9:0.1:0.002. The preparation method is to extrude and granulate using a twin-screw extruder after mixing.
[0244] The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001.
[0245] The preparation method of the perovskite quantum dots is as follows:
[0246] 0.3mmol of lead bromide (PbBr2), 0.09mmol of cesium bromide (CsBr), 0.21mmol of rubidium bromide (RbBr) and 0.03mmol of octylammonium bromide (OABr) were dissolved in 1mL of dimethyl sulfoxide (DMSO), stirred at 60℃ for 6 hours to obtain a perovskite precursor solution, and the obtained solution was filtered for use. The quartz glass substrate was ultrasonically cleaned in acetone, deionized water and anhydrous ethanol for 15min in turn, and then dried under nitrogen for use. The quartz substrate was placed on a coater, 50μL of the perovskite precursor solution was dripped on the quartz substrate, and spin-coated at 2000 rpm for 2min. After the coater was completed, it was placed on a hot plate and annealed at 130℃ for 10min to obtain a Rb / Cs mixed cation perovskite film.
[0247] The perovskite film is freeze-dried and then ball-milled in a ball mill to obtain the perovskite quantum dots.
[0248] Among them, the ball milling beads are zirconium oxide, with a size of 10mm; the ball-to-material ratio is between 30:1; the speed of the ball mill is controlled between 550 rpm, and the ball milling time is 15h.
[0249] Before the middle-layer diffuser plate is prepared into a diffuser plate, the perovskite quantum dots need to be granulated, and the specific treatment method is as follows: after mixing 1 part by weight of perovskite quantum dots and 50 parts by weight of solvent, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50°C for 24 hours to obtain modified perovskite quantum dots.
[0250] The method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum comprises the following steps:
[0251] After the two layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1 and screw 2 at a thickness ratio of 3:4, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffusion plate is then cooled and cut into shape.
[0252] Example 4-4
[0253] This embodiment provides a quantum dot functional diffusion plate capable of changing the spectrum of white light. The diffusion plate comprises three layers, namely an upper diffusion plate, a middle diffusion plate, and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3.
[0254] The raw materials for preparing the upper diffusion plate include polystyrene, diffusing agent 1, and auxiliary agent 1, and the mass ratio is 1:0.001:0.005.
[0255] The preparation method of the diffusing agent 1 is as follows:
[0256] 1 part by weight of sodium dodecylbenzene sulfonate and 12.5 parts of deionized water are mixed; then 6.35 parts of styrene, 4.75 parts of 4-nitrostyrene, and 0.382 parts of azobisisobutyronitrile are mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then 0.3 parts of modified silicon dioxide and 2.2 parts of methanol are added to obtain an oil phase; under stirring at 800 r / min, the oil phase is added dropwise into the reactor to obtain a mixed emulsion; the mixed emulsion is placed in an oven at 65° C. for curing for 10 hours to obtain the diffusant 1.
[0257] The preparation method of the modified silicon dioxide is as follows: 1 part by weight of nano silicon dioxide powder and 50 parts by weight of solvent are mixed, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified silicon dioxide.
[0258] The nano silicon dioxide powder is a mixed powder of nano silicon dioxide with a particle size of about 10 nm and nano silicon dioxide with a particle size of about 50 nm in a mass ratio of 1:1.
[0259] The raw materials for preparing the additive 1 include: polystyrene, didodecanol ester, and mineral oil, and the mass ratio is 9:0.1:0.002. The preparation method is to extrude and granulate using a twin-screw extruder after mixing.
[0260] The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001.
[0261] The preparation method of the perovskite quantum dots is as follows:
[0262] 0.3mmol of lead bromide (PbBr2), 0.09mmol of cesium bromide (CsBr), 0.21mmol of rubidium bromide (RbBr) and 0.03mmol of octylammonium bromide (OABr) were dissolved in 1mL of dimethyl sulfoxide (DMSO), stirred at 60℃ for 6 hours to obtain a perovskite precursor solution, and the obtained solution was filtered for use. The quartz glass substrate was ultrasonically cleaned in acetone, deionized water and anhydrous ethanol for 15min in turn, and then dried under nitrogen for use. The quartz substrate was placed on a coater, 50μL of the perovskite precursor solution was dripped on the quartz substrate, and spin-coated at 2000 rpm for 2min. After the coater was completed, it was placed on a hot plate and annealed at 130℃ for 10min to obtain a Rb / Cs mixed cation perovskite film.
[0263] Before the middle diffuser plate is prepared into a diffuser plate, the perovskite quantum dot film needs to be granulated, and the specific treatment method is as follows: after mixing 1 weight part of the perovskite quantum dot film and 50 weight parts of the solvent, 0.5 weight parts of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 weight parts of ammonia water are added, and the mixture is reacted at 50°C for 24 hours to obtain the modified perovskite quantum dot film.
[0264] The raw materials for preparing the lower diffuser plate include polystyrene, diffuser 2, and ethylene bis stearamide, and the mass ratio is 1:0.001:0.002. The diffuser 2 is an organic silicon light diffuser, specifically HY-7000 spherical silicone resin micropowder from Hangzhou Yuheng Technology Co., Ltd.
[0265] The method for preparing a quantum dot functional diffusion plate capable of changing the white light spectrum comprises the following steps:
[0266] After the three layers of raw materials are mixed and dispersed evenly, they are extruded through screw 1, screw 2, and screw 3 at a thickness ratio of 3:4:3, and the temperatures are set to 225°C, 235°C, 240°C, 242°C, 245°C, and 238°C. The diffuser plate is then cooled and cut into shape.
[0267] Performance test: Performance test is carried out in accordance with enterprise standard Q / GODM 2-2020.
[0268] Total light transmittance
[0269] In the process of the incident light flux leaving from the illuminated surface or the medium incident surface to the other side, the ratio of the radiant energy projected and passed through the object to the total radiant energy projected onto the object is called the transmittance of the object. The average value of the light transmittance of 380nm~750mm is the total light transmittance, represented by T.
[0270] Haze
[0271] A beam of parallel light from a standard "c" light source is vertically irradiated onto a transparent or translucent film, sheet, or plate. Due to scattering inside and on the surface of the material, part of the parallel light deviates from the incident direction by more than 2.5°. d The percentage of the luminous flux T2 transmitted through the material.
[0272] Test method: total light transmittance, haze, blue light removal rate test
[0273] The instruments and equipment are as follows: Spectrophotometer or similar equipment, which is required to be able to test the transmittance, haze and other parameters of the sample at a wavelength of 380nm ~ 750nm, and be able to test samples of specified thickness.
[0274] Sample preparation
[0275] The sample surface should not have defects such as bubbles, scratches, impurities, etc., and proceed as follows:
[0276] The sampling position should be at least 50 mm away from the edge of the original plate; the sample length is 50 mm~100 mm, and the width is 50 mm~100 mm; remove the sample protective film, if the surface is dirty, clean the surface with anhydrous ethanol or other suitable solvents, and dry it naturally for use.
[0277] The test steps are as follows:
[0278] Start the instrument and connect it to the computer, open the test software, and initialize the instrument first; after initialization, perform a blank test without installing the sample, then place the test sample in the instrument, start the test, and obtain the light transmittance curve, data and haze results;
[0279] Take the average light transmittance of 380 nm ~ 420 nm samples as the blue light removal rate, %;
[0280] Take the average light transmittance of samples >380 nm ~ 750 nm as the total light transmittance, %;
[0281] In the present invention, the haze requirement is 90% as the critical point, more than 90% is qualified, 85-90% is fair, and less than 85% is unqualified.
[0282] Brightness uniformity was determined by arranging four cold cathode tubes at intervals of 2 cm, fixing a light diffusion plate sample parallel to the plate at 10 mm, and visually observing the image. Uniform brightness was indicated by ○, and uneven brightness was indicated by ×.
[0283] Table 1 Test results of test 1 and test 2
[0284]
[0285] in, Figure 1 The light source spectrum test results of the plate in Example 1 are as follows: Figure 2 The plate is the same as that in Example 1 (but a common plate without adding perovskite material). It can be seen that the plate in Example 1 can reduce blue light. Figure 3 This is the light source spectrum test result of the plate in Example 2-2. Figure 4 It is the same plate as Example 2-2 (but a normal plate without adding perovskite material).
[0286] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A quantum dot functional diffusion plate that can change the white light spectrum. It is characterized in that The diffusion plate comprises three layers, namely an upper diffusion plate, a middle diffusion plate and a lower diffusion plate; and the thickness ratio of the three layers is 3:4:3; The raw materials for preparing the upper diffusion plate include polystyrene, diffusing agent 1, and auxiliary agent 1; and the mass ratio is 1:0.001:0.005; The preparation method of the diffusing agent 1 is as follows: 1 part by weight of sodium dodecylbenzene sulfonate and 12.5 parts by weight of deionized water are mixed; then 6.35 parts of styrene, 4.75 parts of 4-nitrostyrene and 0.382 parts of azobisisobutyronitrile are mixed and ultrasonicated until the azobisisobutyronitrile is completely dissolved, and then 0.3 parts of modified silicon dioxide and 2.2 parts of methanol are added to obtain an oil phase; under stirring at 800 r / min, the oil phase is added dropwise into a reactor to obtain a mixed emulsion; the mixed emulsion is placed in an oven at 65° C. and cured for 10 hours to obtain the diffusing agent 1; The preparation method of the modified silicon dioxide is as follows: 1 part by weight of nano silicon dioxide powder and 50 parts by weight of solvent are mixed, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified silicon dioxide; The nano silicon dioxide powder is a mixed powder of nano silicon dioxide with a particle size of 10 nm and nano silicon dioxide with a particle size of 50 nm in a mass ratio of 1:1; The raw materials for preparing the additive 1 include: polystyrene, didodecyl alcohol ester, and mineral oil, and the mass ratio is 9:0.1:0.
002. The preparation method is to extrude and granulate them using a twin-screw extruder after mixing; The raw materials for preparing the middle diffuser plate include: polystyrene and perovskite quantum dots; the mass ratio is 1:0.0001; The preparation method of the perovskite quantum dots is as follows: 0.3 mmol of lead bromide, 0.09 mmol of cesium bromide, 0.21 mmol of rubidium bromide and 0.03 mmol of octylammonium bromide are dissolved in 1 mL of dimethyl sulfoxide, stirred at 60° C. for 6 hours to obtain a perovskite precursor solution, and the obtained solution is filtered and set aside; a quartz glass substrate is ultrasonically cleaned in acetone, deionized water and anhydrous ethanol in sequence for 15 minutes, and then blown dry under nitrogen for use; a quartz substrate is placed on a coater, 50 μL of the perovskite precursor solution is dripped on the quartz substrate, and spin-coated at 2000 rpm for 2 minutes. After the coater is completed, it is placed on a heating plate and annealed at 130° C. for 10 minutes to obtain a Rb / Cs mixed cation perovskite film; the perovskite film is freeze-dried and then ball-milled in a ball mill to obtain the perovskite quantum dots; The ball milling beads are zirconium oxide, with a size of 10 mm; the ball-to-material ratio is between 30:1; the speed of the ball mill is controlled between 550 rpm, and the ball milling time is 15 h; Before the middle diffuser plate is prepared into a diffuser plate, the perovskite quantum dots need to be granulated, and the specific processing method is as follows: after mixing 1 part by weight of the perovskite quantum dots and 50 parts by weight of the solvent, 0.5 parts by weight of 1,1,3,5,5-pentamethyl-3-phenyl-1,5-divinyltrisiloxane and 0.4 parts by weight of ammonia water are added, and the mixture is reacted at 50° C. for 24 hours to obtain the modified perovskite quantum dots; The raw materials for preparing the lower diffusion plate include polystyrene, a diffusion agent 2, and ethylene bisstearamide, and the mass ratio is 1:0.001:0.002; the diffusion agent 2 is an organic silicon light diffuser.
2. A quantum dot functional diffusion plate capable of changing the white light spectrum according to claim 1, It is characterized in that Used in LED semiconductor light-emitting field.