A method for measuring the bandgap width of semiconductor thin film materials

By combining ultraviolet photoelectron spectroscopy and reflective electron spectroscopy technology in ultra-high vacuum environment, the bandwidth gap width of semiconductor thin film materials is solved, and the measurement difficulties and signal distortion problems in the prior art are improved, and the accuracy of the test results is improved. Accuracy.

CN118329952BActive Publication Date: 2024-11-29BEIJING INST OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410748369.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2024-11-29
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

It is difficult for the prior art to directly measure the band gap width of semiconductor thin film materials, and the 'relaxation process' during the excitation process leads to signal distortion, affecting the accuracy of the test results.

Method used

In ultra-high vacuum environment, the semiconductor thin film material is calculated by measuring the positions of the top and bottom of the valence band or the highest occupying molecular orbitals and the lowest not occupying molecular orbitals. Band-disabled width.

Benefits of technology

The accuracy and accuracy of the test signal are improved, and the bandwidth gap information of the semiconductor thin film material is directly obtained, avoiding the problem of signal distortion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118329952B_ABST
    Figure CN118329952B_ABST
Patent Text Reader

Abstract

The present invention discloses a method for measuring the bandgap width of semiconductor thin film materials, including: a calibration step, a test step and a calculation step. By combining ultraviolet photoelectron spectroscopy technology with reflected photoelectron spectroscopy technology, the method can not only directly obtain the position of the top of the valence band and the bottom of the conduction band of the semiconductor thin film material, or directly obtain the position of the highest occupied molecular orbital and the lowest unoccupied molecular orbital of the semiconductor thin film material, but also obtain the bandgap width of the semiconductor thin film material by calculation, and the test result is more realistic. The ultraviolet photoelectron spectroscopy unit and the reflected photoelectron spectroscopy unit are placed in the same ultra-high vacuum environment, and the concentration of gas molecules in the ultra-high vacuum environment is extremely low, resulting in an improvement in the accuracy of the collected test signal. In addition, since the excitation source energy is low and the core energy level excitation is not included in the excitation process, the signal distortion caused by the "relaxation process" accompanying the core energy level excitation can be avoided, and the accuracy of the test result is greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to ultraviolet photoelectron spectroscopy technology and reflected photoelectron spectroscopy technology, belonging to the field of surface and interface analysis, and in particular to a method for measuring the bandgap width of semiconductor thin film materials. Background Art

[0002] Photoelectron spectroscopy and reflected photoelectron spectroscopy are mainly used for surface and interface analysis. X-rays, ultraviolet light, and electron beams with a certain energy emitted by the excitation source act on the sample surface. The basic principle of ultraviolet photoelectron spectroscopy technology is based on Einstein's law of photoelectric effect. Ultraviolet photoelectron spectroscopy measures the energy distribution of valence electrons and obtains various information about the valence electron structure, including the valence band spectrum, work function, and state density distribution of the material. The basic physical process of reflected photoelectron spectroscopy is opposite to that of the photoelectric effect. It is used to detect the electron empty state density and the band structure of the empty state above the Fermi level on the solid surface. Theoretically, it can detect all unoccupied energy levels between the Fermi level and the vacuum level, and can be directly used to measure the electronic structure of the material conduction band.

[0003] The bandgap width is the energy difference between the lowest point of the conduction band and the highest point of the valence band. Semiconductor thin film materials are an important part of materials science, and regulating the conduction band and valence band positions of the bandgap plays an important role in studying new, modulatable semiconductor thin film materials and studying the lattice structure, phase transition, optical and electrical properties of thin film materials.

[0004] The light absorption coefficient method, photoconductivity method, photovoltaic effect method, photoluminescence spectroscopy method, etc. can all measure the bandgap width of materials, but none of the above methods can directly obtain the conduction band and valence band information that make up the bandgap width; and the excitation process of the above methods will be affected by the "relaxation process" accompanied by the core energy level excitation process. This has brought great difficulties to the research of semiconductor materials and the regulation of energy band structure, so a method for measuring the bandgap width of semiconductor thin film materials is urgently needed. Summary of the invention

[0005] The purpose of the present invention is to provide a method for measuring the bandgap width of semiconductor thin film materials, and to provide a method for measuring the bandgap width of the valence band top, the conduction band bottom position in the bandgap width of the thin film material, or the position of the highest occupied molecular orbital and the lowest unoccupied molecular orbital of the semiconductor thin film material to obtain the bandgap width; the ultraviolet photoelectron energy spectrum unit and the reflected photoelectron energy spectrum unit are placed in the same ultra-high vacuum environment, and the concentration of gas molecules in the ultra-high vacuum environment is extremely low, so that the accuracy of the collected test signal is improved. In addition, since the excitation source energy is low, the excitation process does not include core energy level excitation, so the signal distortion caused by the "relaxation process" accompanying the core energy level excitation can be avoided, and the accuracy of the test result is greatly improved.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] The present invention provides a method for measuring the bandgap width of a semiconductor thin film material, comprising the following steps:

[0008] Calibration steps:

[0009] Test the reflected photoelectron energy spectrum of the standard sample, determine the Fermi level position in the reflected photoelectron energy spectrum, and calibrate the Fermi level zero point E F ; Test the ultraviolet photoelectron spectrum of the standard sample, determine the Fermi level position in the ultraviolet photoelectron spectrum, and calibrate the Fermi level zero point E F ;

[0010] Test steps:

[0011] According to the calibration of the Fermi level zero point E in the reflected electron energy spectrum F And the calibration of the Fermi level zero point E of the ultraviolet photoelectron spectrum F , to test the semiconductor thin film material to be tested;

[0012] Test the ultraviolet photoelectron spectrum of the semiconductor thin film material to obtain the valence band top position E VBM Or get the highest occupied molecular orbital position E HOMO ;

[0013] Test the reflected electron energy spectrum of the semiconductor thin film material to obtain the conduction band bottom position E CBM Or get the lowest unoccupied molecular orbital position E LUMO ;

[0014] Calculation steps: Calculate the bandgap width of the semiconductor thin film material to be tested, expressed as E g =|E CBM -E VBM | or E g =|E LUMO -E HOMO |.

[0015] Furthermore, the standard sample in the calibration step is single substance silver.

[0016] It is worth noting that the standard sample silver element in the calibration step needs to be confirmed to have no contamination layer on the surface before the calibration begins. If there is a contamination layer on the surface, it needs to be cleaned. The cleaning method is to sputter with an argon ion sputtering source until there is no contamination layer on the surface, exposing a pure silver element layer.

[0017] Furthermore, in the calibration step:

[0018] Determining the Fermi level position in the reflected electron energy spectrum and calibrating the Fermi level zero point E F, using the 50% height method; including: on the reflected electron energy spectrum, make two tangent lines ab and cd and the extended line of the Fermi edge intersecting at points b and c, make a rectangle with points b and c as diagonal angles, take the midpoints of the opposite sides of the rectangle to get the straight line ef, and the intersection point with the Fermi edge is g, and the energy mark corresponding to g is the zero point of the Fermi level E F .

[0019] Furthermore, in the calibration step:

[0020] The determination of the Fermi level position in the ultraviolet photoelectron energy spectrum and the calibration of the Fermi level zero point E F , using the 50% height method; including: making two tangent lines ab and cd on the ultraviolet photoelectron energy spectrum and the extension line of the Fermi edge intersecting at points b and c, making a rectangle with points b and c as diagonal angles, taking the straight line ef connecting the midpoints of the opposite sides of the rectangle, and the intersection point with the Fermi edge is g, and the energy mark corresponding to g is the zero point of the Fermi level E F .

[0021] Furthermore, the calibration step and the test step are performed in the same photoelectron spectrometer, which is equipped with an ultraviolet photoelectron spectrometer unit and a reflective photoelectron spectrometer unit, and the vacuum degree is better than 5*10 -6 Pa.

[0022] It is worth noting that photon, electron, and photoelectron signals are easily affected by the scattering of nearby gas molecules. In an ultra-high vacuum environment, the concentration of gas molecules is kept at a very low level, and photons, electrons, and photoelectrons can obtain a sufficiently long mean free path, so the accuracy of the test signal can be improved. Surface analysis technology has strict requirements on the cleanliness of the material surface. In an ultra-high vacuum, the material surface can be "atomic clean", so the test results are more consistent with the material itself. The ultraviolet light energy used in the ultraviolet photoelectron energy spectrum unit is helium I, and the photon energy is 21.22 eV; the electron gun emission energy used in the reflected photoelectron energy spectrum unit is less than 50 eV. Both have low energy, and the excitation process does not include core energy level excitation, so the signal distortion caused by the "relaxation process" accompanying the core energy level excitation can be avoided, and the accuracy of the test results is greatly improved.

[0023] Furthermore, in the calibration step, the reflected photoelectron spectrum of the test standard sample is collected on a reflected photoelectron spectrum unit;

[0024] In the testing step, the reflected photoelectron spectrum of the semiconductor thin film material to be tested is collected on a reflected photoelectron spectrum unit.

[0025] Further, the ultraviolet photoelectron spectrum of the standard sample tested in the calibration step is collected on an ultraviolet photoelectron spectrum unit;

[0026] In the testing step, the ultraviolet photoelectron spectrum of the semiconductor thin film material to be tested is collected on an ultraviolet photoelectron spectrum unit.

[0027] Furthermore, the top of the valence band or the highest occupied molecular orbital in the testing step corresponds to the position where the outermost electron has the lowest binding energy close to the Fermi level;

[0028] The method to determine the valence band top or the highest occupied molecular orbital position is to linearly extrapolate the steep rising part along the starting edge of the ultraviolet photoelectron energy spectrum band, and take its intersection with the background noise baseline as the valence band top position E VBM Or the highest occupied molecular orbital position E HOMO .

[0029] Furthermore, in the test step, the bottom of the conduction band or the lowest unoccupied molecular orbital corresponds to a position with the highest binding energy of the electron empty state density near the Fermi level;

[0030] The method to determine the bottom of the conduction band or the position of the lowest unoccupied molecular orbital is to linearly extrapolate the steep rise along the starting edge of the reflected electron energy spectrum band, and take its intersection with the background noise baseline as the conduction band bottom position E CBM Or the lowest unoccupied molecular orbital position E LUMO .

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] The purpose of the present invention is to combine the ultraviolet photoelectron spectroscopy technology and the reflected photoelectron spectroscopy technology in an ultra-high vacuum, so as to not only directly obtain the position of the top of the valence band and the bottom of the conduction band of the semiconductor thin film material, or directly obtain the position of the highest occupied molecular orbital and the lowest unoccupied molecular orbital of the semiconductor thin film material, but also obtain the bandgap width of the semiconductor thin film material by calculation, and the test result is more realistic. The ultraviolet photoelectron spectroscopy and the reflected photoelectron spectroscopy units are placed in the same ultra-high vacuum environment, and the concentration of gas molecules in the ultra-high vacuum environment is extremely low, so that the accuracy of the collected test signal is improved. In addition, since the excitation source energy is low and the core energy level excitation is not included in the excitation process, the signal distortion caused by the "relaxation process" accompanying the core energy level excitation can be avoided, and the accuracy of the test result is greatly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 An Ag reflected photoelectron energy spectrum diagram for determining the Fermi level position and calibrating the Fermi level to zero provided in an embodiment of the present invention;

[0034] Figure 2 The reflected electron energy spectrum of Ag with a Fermi level of zero provided in an embodiment of the present invention;

[0035] Figure 3The ultraviolet photoelectron spectrum of Ag with a Fermi level of zero provided in an embodiment of the present invention;

[0036] Figure 4 The ultraviolet photoelectron spectrum of the PbI2 film provided in the embodiment of the present invention;

[0037] Figure 5 The reflected electron spectrum of the PbI2 film provided in the embodiment of the present invention;

[0038] Figure 6 The ultraviolet photoelectron spectrum of the Meo-2PACz film provided in the embodiment of the present invention;

[0039] Figure 7 This is a photoreflective electron spectrum diagram of the Meo-2PACz film provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0040] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0041] In the description of the present invention, it should be noted that the terms "upper", "lower", "inner", "outer", "front end", "rear end", "two ends", "one end", "the other end" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0042] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "provided with", "connected", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0043] The present invention provides a method for measuring the bandgap width of a semiconductor thin film material, comprising the following steps:

[0044] Calibration steps:

[0045] Test the reflected photoelectron energy spectrum of the standard sample, determine the Fermi level position in the reflected photoelectron energy spectrum, and calibrate the Fermi level zero point E F; Test the ultraviolet photoelectron spectrum of the standard sample, determine the Fermi level position in the ultraviolet photoelectron spectrum, and calibrate the Fermi level zero point E F ;

[0046] Test steps:

[0047] According to the calibration of the Fermi level zero point E in the reflected electron energy spectrum F And the calibration of the Fermi level zero point E of the ultraviolet photoelectron spectrum F , to test the semiconductor thin film material to be tested;

[0048] Test the ultraviolet photoelectron spectrum of the semiconductor thin film material to obtain the valence band top position E VBM Or get the highest occupied molecular orbital position E HOMO ;

[0049] Test the reflected electron energy spectrum of the semiconductor thin film material to obtain the conduction band bottom position E CBM ; or obtain the lowest unoccupied molecular orbital position E LUMO ; Among them, the highest occupied molecular orbital in organic semiconductors and quantum dots corresponds to the top of the valence band in inorganic semiconductors, while the lowest unoccupied molecular orbital corresponds to the bottom of the conduction band.

[0050] Calculation steps: Calculate the bandgap width of the semiconductor thin film material to be tested, expressed as E g =|E CBM -E VBM | or E g =|E LUMO -E HOMO |.

[0051] This method combines ultraviolet photoelectron spectroscopy technology with reflected photoelectron spectroscopy technology. It can not only directly obtain the position of the valence band top and conduction band bottom in inorganic semiconductors (or directly obtain the highest occupied molecular orbital position and the lowest unoccupied molecular orbital position in organic semiconductors and quantum dots), but also obtain the bandgap width of semiconductor thin film materials through calculation. The ultraviolet photoelectron spectroscopy and reflected photoelectron spectroscopy units are placed in the same ultra-high vacuum environment. The concentration of gas molecules in the ultra-high vacuum environment is extremely low, which improves the accuracy of the collected test signals. In addition, since the excitation source is ultraviolet light and electrons, their energy is relatively low, and the excitation process does not include core energy level excitation, it can avoid signal distortion caused by the "relaxation process" accompanying core energy level excitation, and the accuracy of the test results is greatly improved.

[0052] The calibration step includes the following steps (1) and (2):

[0053] Step (1) Test the reflected electron energy spectrum of the standard sample, determine the Fermi level position, and calibrate the Fermi level zero point, expressed as EF .

[0054] Step (2) Test the UV photoelectron spectrum of the standard sample, determine the Fermi level position, and calibrate the Fermi level zero point, expressed as E F .

[0055] The above-mentioned standard samples are single element silver with a purity of 99.999%, which is conducive to accurately calibrating the zero point of the Fermi level.

[0056] The test procedure includes the following steps (3) and (4):

[0057] Step (3) Test the ultraviolet photoelectron spectrum of the semiconductor thin film material to obtain the valence band top position E VBM Or get the highest occupied molecular orbital position E HOMO .

[0058] In inorganic semiconductors, the valence band top corresponds to the position where the outermost electron has the lowest binding energy near the Fermi level. The method to determine the position of the valence band top is to linearly extrapolate the steep rising part along the starting edge of the ultraviolet photoelectron energy spectrum band, and take its intersection with the background noise baseline as the valence band top position E. VBM .

[0059] In addition, in organic semiconductors and quantum dot semiconductors, the highest occupied molecular orbital corresponds to the position where the outermost electron has the lowest binding energy near the Fermi level; the method for determining the position of the highest occupied molecular orbital is to linearly extrapolate the steeply rising part along the starting edge of the ultraviolet photoelectron energy spectrum band, and take its intersection with the background noise baseline as the highest occupied molecular orbital position E HOMO .

[0060] The calculation steps can be completed on a computer to calculate the bandgap width value, expressed as:

[0061] The conduction band bottom position E CBM E VBM The absolute difference of E g =|E CBM -E VBM |;

[0062] Or expressed as:

[0063] The lowest unoccupied molecular orbital position E LUMO With the highest occupied molecular orbital position E HOMO The absolute difference of E g =|E LUMO -E HOMO |.

[0064] In the above steps (1) and (2), the method for determining the Fermi level position and calibrating the Fermi level zero point is the 50% height method. Figure 1 As shown, the horizontal axis is the electron gun energy, in units of ev; the vertical axis is: the intensity of the reflected electron energy spectrum signal, in units of c / s (coulomb per second). Taking Ag as a standard sample, two tangent lines ab and cd are made on the reflected electron energy spectrum diagram, and the extension line of the Fermi edge intersects at points b and c. A rectangle is made with points b and c as diagonal angles. The ef straight line is connected to the midpoints of the opposite sides of the rectangle, and the intersection with the Fermi edge is g. The energy mark corresponding to g is the zero point of the Fermi level. In this embodiment, the method for calibrating the Fermi level belongs to single-point calibration, which is convenient, simple and fast.

[0065] The above steps (1), (2), (3) and (4) are carried out in the same photoelectron spectrometer, which is equipped with an ultraviolet photoelectron spectrometer unit and a reflective photoelectron spectrometer unit, and the vacuum degree is better than 10 -6 Pa. Wherein, steps (1) and (4) are collected on a reflective electron spectrum unit; steps (2) and (3) are collected on an ultraviolet photoelectron spectrum unit.

[0066] In the embodiments of the present invention, the ultraviolet photoelectron spectroscopy technology and the reflected photoelectron spectroscopy technology are combined, which can not only directly obtain the position of the valence band top and the conduction band bottom in inorganic semiconductors, or directly obtain the highest occupied molecular orbital and the lowest unoccupied molecular orbital in organic semiconductors and quantum dot semiconductors, but also obtain the bandgap width of semiconductor thin film materials through calculation. The ultraviolet photoelectron spectroscopy and reflected photoelectron spectroscopy information collection process does not include core energy level excitation, so the signal distortion caused by the "relaxation process" accompanying the core energy level excitation can be avoided, and the accuracy of the test results is greatly improved. Since the vacuum degree of the ultraviolet photoelectron spectroscopy and reflected photoelectron spectroscopy units is better than 5*10 -6 Pa, so the measured data can more truly reflect the actual state of the semiconductor film, and the test results are closer to the actual situation.

[0067] The measurement method of the present invention is further explained below by two examples;

[0068] Embodiment 1:

[0069] The method for implementing the bandgap width of the PbI2 film according to the present invention comprises the following steps:

[0070] (1) Test the reflected electron spectrum of the standard sample Ag, such as Figure 2 As shown, the Fermi level position is determined and the Fermi level zero point is calibrated.

[0071] (2) Test the UV photoelectron spectrum of the standard sample Ag, such as Figure 3 As shown, the Fermi level position is determined and the Fermi level zero point is calibrated.

[0072] (3) Test the UV photoelectron spectrum of PbI2 thin film materials, such as Figure 4As shown in the figure, the valence band top corresponds to the position where the outermost electron has the lowest binding energy near the Fermi level; the method to determine the position of the valence band top is to linearly extrapolate the steep rising part along the starting edge of the ultraviolet photoelectron energy spectrum band, and take its intersection with the background noise baseline as the valence band top position E VBM , expressed as E VBM =1.08 eV;

[0073] (4) Test the reflected electron spectrum of PbI2 thin film materials, such as Figure 5 As shown in the figure, the bottom of the conduction band corresponds to the position where the electron empty state density has the highest binding energy near the Fermi level; the method to determine the position of the bottom of the conduction band is to linearly extrapolate the steep rising part along the starting edge of the reflected electron energy spectrum band, and take its intersection with the background noise baseline as the conduction band position E CBM ; Get the conduction band bottom position, expressed as E CBM = -1.53 ​​eV;

[0074] (5) E g =|E CBM -E VBM |=2.61 eV, as the bandgap width value of PbI2.

[0075] This method mainly uses the principle of photoelectric effect of ultraviolet photoelectron energy spectrum to measure the change of valence layer substructure caused by photogenerated charge generated by ultraviolet light entering the surface of the sample to be tested, and obtains ultraviolet photoelectron energy spectrum to detect the valence band information of semiconductor thin film; using the principle opposite to the photoelectric effect of reflected photoelectron energy spectrum, measure the information of photons excited by electrons entering the non-occupied state of the sample to obtain reflected photoelectron energy spectrum, and detect the information of conduction band of semiconductor thin film material. The complete information of bandgap width is obtained through the conduction band information and valence band information.

[0076] Embodiment 2:

[0077] The method for implementing the bandgap width of the Meo-2PACz thin film material according to the present invention comprises the following steps:

[0078] 1) Test the reflected electron energy spectrum of the standard sample Ag, determine the Fermi level position, and calibrate the Fermi level zero point.

[0079] 2) Test the UV photoelectron spectrum of the standard sample Ag, determine the Fermi level position, and calibrate the Fermi level zero point.

[0080] 3) Test the UV photoelectron spectrum of Meo-2PACz thin film materials, such as Figure 6 As shown in the figure, the highest occupied molecular orbital position corresponds to the position where the outermost electron has the lowest binding energy near the Fermi level; the method to determine the highest occupied molecular orbital position is to linearly extrapolate the steep rising part along the starting edge of the ultraviolet photoelectron energy spectrum band, and take its intersection with the background noise baseline as the highest occupied molecular orbital position EHOMO ; expressed as E HOMO = 0.73 eV;

[0081] 4) Test the reflected electron spectrum of Meo-2PACz thin film materials, such as Figure 7 As shown in the figure, the lowest unoccupied molecular orbital position corresponds to the position with the highest binding energy of the electron empty state density near the Fermi level; the method to determine the lowest unoccupied molecular orbital position is to linearly extrapolate the steep rising part along the starting edge of the reflected electron energy spectrum band, and take its intersection with the background noise baseline as the lowest unoccupied molecular orbital position E LUMO ; expressed as E LUMO = -2.59 eV;

[0082] 5) E g =|E LUMO -E HOMO |=3.32 eV, as the bandgap value of Meo-2PACz.

[0083] This method mainly uses the principle of photoelectric effect of ultraviolet photoelectron energy spectrum to measure the changes in the occupied state electronic structure caused by the photogenerated charge generated by ultraviolet light entering the surface of the sample to be tested, and obtains the ultraviolet photoelectron energy spectrum to detect the position information of the highest occupied molecular orbital of the semiconductor film; using the principle opposite to the photoelectric effect of the reflected photoelectron energy spectrum, the information of photons excited by electrons entering the non-occupied state of the sample to obtain the reflected photoelectron energy spectrum, and detect the information of the lowest unoccupied molecular orbital of the semiconductor film material. The complete information of the bandgap width is obtained through the information of the highest occupied molecular orbital position and the lowest unoccupied molecular orbital.

[0084] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. A method for measuring the bandgap width of a semiconductor thin film material, characterized in that: The following steps are involved: Calibration steps: Test the reflected photoelectron energy spectrum of the standard sample, determine the Fermi level position in the reflected photoelectron energy spectrum, and calibrate the Fermi level zero point E F ; Test the ultraviolet photoelectron spectrum of the standard sample, determine the Fermi level position in the ultraviolet photoelectron spectrum, and calibrate the Fermi level zero point E F ; Test steps: According to the calibration of the Fermi level zero point E in the reflected electron energy spectrum F And the calibration of the Fermi level zero point E of the ultraviolet photoelectron spectrum F , to test the semiconductor thin film material to be tested; Test the ultraviolet photoelectron spectrum of the semiconductor thin film material to obtain the valence band top position E VBM Or get the highest occupied molecular orbital position E HOMO ; Test the reflected electron energy spectrum of the semiconductor thin film material to obtain the conduction band bottom position E CBM Or get the lowest unoccupied molecular orbital position E LUMO ; Calculation steps: Calculate the bandgap width of the semiconductor thin film material to be tested, expressed as E g =|E CBM -E VBM | or E g =|E LUMO -E HOMO |.

2. The method for measuring the bandgap width of semiconductor thin film materials according to claim 1, characterized in that: The standard sample in the calibration step is single substance silver.

3. The method for measuring the bandgap width of semiconductor thin film materials according to claim 1, characterized in that: In the calibration step: Determining the Fermi level position in the reflected electron energy spectrum and calibrating the Fermi level zero point E F , using the 50% height method; including: on the reflected electron energy spectrum, make two tangent lines ab and cd and the extended line of the Fermi edge intersecting at points b and c, make a rectangle with points b and c as diagonal angles, take the midpoints of the opposite sides of the rectangle to get the straight line ef, and the intersection point with the Fermi edge is g, and the energy mark corresponding to g is the zero point of the Fermi level E F .

4. The method for measuring the bandgap width of semiconductor thin film materials according to claim 1, characterized in that: In the calibration step: The determination of the Fermi level position in the ultraviolet photoelectron energy spectrum and the calibration of the Fermi level zero point E F , using the 50% height method; including: making two tangent lines ab and cd on the ultraviolet photoelectron energy spectrum and the extension line of the Fermi edge intersecting at points b and c, making a rectangle with points b and c as diagonal angles, taking the straight line ef connecting the midpoints of the opposite sides of the rectangle, and the intersection point with the Fermi edge is g, and the energy mark corresponding to g is the zero point of the Fermi level E F .

5. The method for measuring the bandgap width of semiconductor thin film materials according to claim 1, characterized in that: The calibration step and the test step are performed in the same photoelectron spectrometer, which is equipped with an ultraviolet photoelectron spectrometer unit and a reflective photoelectron spectrometer unit, and the vacuum degree is better than 5*10 -6 Pa.

6. The method for measuring the bandgap width of semiconductor thin film materials according to claim 5, characterized in that: In the calibration step, the reflected photoelectron spectrum of the test standard sample is collected on the reflected photoelectron spectrum unit; In the testing step, the reflected photoelectron spectrum of the semiconductor thin film material to be tested is collected on a reflected photoelectron spectrum unit.

7. The method for measuring the bandgap width of semiconductor thin film materials according to claim 5, characterized in that: The ultraviolet photoelectron spectrum of the standard sample tested in the calibration step is collected on an ultraviolet photoelectron spectrum unit; In the testing step, the ultraviolet photoelectron spectrum of the semiconductor thin film material to be tested is collected on an ultraviolet photoelectron spectrum unit.

8. The method for measuring the bandgap width of semiconductor thin film materials according to claim 1, characterized in that: The top of the valence band or the highest occupied molecular orbital in the test step corresponds to the position where the outermost electron has the lowest binding energy close to the Fermi level; The method to determine the valence band top or the highest occupied molecular orbital position is to linearly extrapolate the steep rising part along the starting edge of the ultraviolet photoelectron energy spectrum band, and take its intersection with the background noise baseline as the valence band top position E VBM Or the highest occupied molecular orbital position E HOMO .

9. The method for measuring the bandgap width of semiconductor thin film materials according to claim 1, characterized in that: The bottom of the conduction band or the lowest unoccupied molecular orbital in the test step corresponds to a position with the highest binding energy of the electron empty state density near the Fermi level; The method to determine the bottom of the conduction band or the position of the lowest unoccupied molecular orbital is to linearly extrapolate the steep rise along the starting edge of the reflected electron energy spectrum band, and take its intersection with the background noise baseline as the conduction band bottom position E CBM or the lowest unoccupied molecular orbital E LUMO .

Citation Information

Patent Citations

  • Method and apparatus for measuring bending of energy band by employing photoelectron energy spectrums

    CN110161070A

  • Method for measuring photoelectron spectroscopy of polymer sublayer by utilizing plasma etching

    CN111537539A