A repair factor composite bone support material and preparation method thereof

By loading polylactic acid and KGN composite fibers, activated mesoporous silica and modified silk fibroin on the surface of titanium alloys, combined with the technology of oxidizing icariin, the mechanical and biocompatibility issues of titanium alloy orthopedic implant materials have been solved. and insufficient antibacterial properties, it achieves bone cell adhesion and growth, enhances anti-inflammatory properties, and achieves slow and stable release of repair factors.

CN118340936BActive Publication Date: 2024-10-11SHANGHAI AIDU MEDICAL EQUIP TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410764880.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-11
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

Existing titanium alloy orthopedic implant materials have deficiencies in mechanical properties, biocompatibility, anti-inflammatory and antibacterial properties, resulting in poor bone repair effects and uneven release of repair factors.

Method used

Polylactic acid and KGN composite fibers are loaded on the surface of titanium alloy through electrospinning technology, and mesoporous silica is activated through plasma immersion ion implantation technology, combined with methacrylate-modified silk fibroin and oxidized icariin, Forming a hydrophilic three-dimensional network structure, stably coating the titanium alloy, improving its mechanical and biocompatibility, and achieving sustained release of repair factors.

Benefits of technology

It significantly improves the mechanical properties and biocompatibility of titanium alloys, promotes the adhesion and growth of bone cells, enhances anti-inflammatory and antibacterial properties, achieves slow and stable release of repair factors, and improves the effect of bone repair.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118340936B_ABST
    Figure CN118340936B_ABST
Patent Text Reader

Abstract

The invention discloses a repair factor composite bone support material and a preparation method thereof, and belongs to the technical field of biomedical materials; the invention proposes that polylactic acid and KGN composite fibers are loaded on the surface of an alkali-heat-activated titanium alloy by electrostatic spinning to achieve drug loading and sustained release; mesoporous silica obtained by surface activation treatment using plasma immersion ion implantation technology is added to provide biologically active sites to promote the adsorption and proliferation of bone cells; zinc ions are introduced to improve antibacterial properties; silk fibroin obtained by methyl acrylate modification is added and immersed in an oxidized icariin solution, and a Schiff base reaction occurs between the amino group of the silk fibroin and the aldehyde group of the oxidized icariin, thereby forming a hydrophilic three-dimensional network structure gel structure, stably coating the titanium alloy, improving the corrosion resistance, antibacterial and anti-inflammatory properties, thereby improving the mechanical properties and biocompatibility of the titanium alloy in vivo, and achieving the technical effect of sustained release of the repair factor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biomedical materials, and specifically refers to a repair factor composite bone support material and a preparation method thereof. Background Art

[0002] With the aging of the population, the incidence of orthopedic defects or fractures caused by rheumatoid arthritis, osteoporosis, limb trauma or congenital deformities is increasing rapidly, so artificial implants are needed to repair, replace or reconstruct bone structure; orthopedic implant materials play a vital role in orthopedic surgical treatment. Orthopedic implant materials are implanted into the human body to promote fracture healing and bone cell growth. Ideal orthopedic implant materials should usually have suitable mechanical properties, interconnected porous structure, good hydrophilicity, appropriate anti-degradation ability and excellent bone conductivity, as well as good antibacterial ability.

[0003] Common orthopedic implant materials include metal alloys, bioceramics, natural polymer materials, artificial polymer materials, bioactive glass, etc. Metal alloys have good mechanical properties and can be used as the preferred option for orthopedic support materials. Metal alloys include titanium, magnesium, zinc and their alloys. Among them, titanium and its alloys are widely used as implantable support materials for orthopedic, plastic surgery and dental applications due to their excellent mechanical properties, corrosion resistance and biocompatibility. In order to further improve the biological properties of orthopedic support materials, repair growth factors, as important participants in the bone formation process, are also often introduced into orthopedic implant materials to improve the effect of bone repair, such as the commonly used vascular endothelial growth factor (VEGF) and bone morphogenetic protein-2 (BMP-2), which can induce angiogenesis, activate osteogenesis-related signaling pathways, and ultimately promote bone regeneration. However, these growth factors are expensive and unstable. Icariin is the main bioactive component of the traditional Chinese medicine Epimedium, which has significant pro-angiogenic and anti-inflammatory effects and can be added to bone support materials as a repair growth factor.

[0004] However, the original titanium alloy surface is bioinert and cannot fully induce or stimulate specific cell behaviors, which is not conducive to the adhesion and growth of bone cells. The lack of osteogenesis, vascularization and anti-inflammatory properties will reduce the ability of new bone tissue to grow, thereby increasing the risk of bone repair failure, and ultimately leading to poor integration with surrounding bone tissue and hindering new bone formation or slow bone integration rate, seriously affecting the success rate of orthopedic implant surgery; therefore, how to provide a titanium alloy-based orthopedic support material with good mechanical properties and biocompatibility, anti-wear, anti-inflammatory, antibacterial properties, promoting osteogenesis, and sustained release of repair factors is a problem that technical personnel in this field urgently need to solve. Summary of the invention

[0005] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a repair factor composite bone support material and a preparation method thereof. In order to solve the problems of poor mechanical compatibility of titanium alloy, surface inertness that is not conducive to the adhesion of osteoblasts, poor anti-inflammatory and antibacterial properties, susceptibility to wear, and rapid and large-scale release of repair factors, the present invention proposes to load polylactic acid and KGN composite fibers on the surface of titanium alloy after alkali heat activation by electrospinning, so as to provide more surface area for the adhesion of bone cells and realize drug loading and sustained release; add mesoporous silica obtained by surface activation treatment using plasma immersion ion implantation technology to provide biologically active sites, which is beneficial to promote the adsorption and proliferation of bone cells; after adding silk fibroin modified with methyl acrylate, it is immersed in an oxidized icariin solution, and a Schiff base reaction occurs between the amino group of the silk fibroin and the aldehyde group of the oxidized icariin, thereby forming a hydrophilic three-dimensional network structure gel structure, stably coating the titanium alloy, and improving the wear resistance, antibacterial and anti-inflammatory properties, thereby achieving the technical effect of improving the mechanical properties and biocompatibility of the titanium alloy in the body and sustained release of the repair factor.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows: The present invention proposes a repair factor composite bone support material and a preparation method thereof, and the preparation method of the repair factor composite bone support material specifically comprises the following steps:

[0007] S1. Select a medical titanium alloy, extrude it into a titanium plate or rod, grind and polish the sample with 800 mesh, 1000 mesh, 1500 mesh and 2000 mesh silicon sandpaper, soak it in 1.0-1.8 mol / L sodium hydroxide solution at 50-60°C for 20-24h, clean it with ethanol, acetone and deionized water ultrasonically for 30-40min, dry it and set it aside;

[0008] S2, dissolving KGN in acetone to obtain a KGN solution; dissolving polylactic acid in a mixed solvent of acetone and N,N-dimethylformamide in a volume ratio of 6:1 to obtain a polylactic acid solution; mixing the KGN solution and the polylactic acid solution to obtain a spinning solution for standby use;

[0009] S3, applying an external voltage to the spinning solution obtained in S2 through an electrostatic spinning process, so that a jet is formed under the action of an external electric field, and the jet is received by the titanium alloy treated by S1, so that the jet is finally solidified into nanofibers on the surface of the titanium alloy, thereby obtaining a titanium alloy loaded with polylactic acid and KGN composite fibers for standby use;

[0010] S4, adding natural silk cocoons to a sodium carbonate aqueous solution with a concentration of 0.05 mol / L, boiling at 100°C for 20-30 min, then rinsing with cold water, repeating the same treatment 2-3 times, drying to obtain degummed silk, adding a lithium bromide aqueous solution with a concentration of 9.2 mol / L, dissolving at 65-75°C for 1-2 h, dialyzing for 12 h, obtaining a silk fibroin solution, adding glycidyl methacrylate, stirring for 3-5 h, dialyzing for 24 h, obtaining a methacrylate-modified silk fibroin solution, and setting aside;

[0011] S5, mixing the titanium alloy treated by S3 with the modified mesoporous silica, adding a 0.5 mol / L zinc nitrate hexahydrate solution for immersion treatment, placing at room temperature for 24 hours, freeze-drying, adding the methacrylate modified silk fibroin solution obtained by S4, stirring evenly at 4°C, freeze-drying at -2°C, obtaining a pretreated bone support material for standby use;

[0012] S6. Dissolve oxidized icariin in an ethanol aqueous solution with a mass fraction of 50-60% to obtain an oxidized icariin solution with a concentration of 0.5-3 mg / mL, soak the pretreated bone support material obtained in S5 in the oxidized icariin solution, react at 4°C for 20-24 hours, wash with deionized water, and freeze-dry to obtain a repair factor composite bone support material.

[0013] Preferably, in S2, the amount of KGN added to acetone is 0.01-0.02 g / mL;

[0014] Preferably, in S2, the amount of the polylactic acid added to the mixed solvent of acetone and N,N-dimethylformamide is 0.2-0.3 g / mL;

[0015] Preferably, in S2, the volume ratio of the KGN solution to the polylactic acid solution is 1-2:10;

[0016] Preferably, in S3, the conditions of the electrospinning process are: the external voltage is 10-20 kV, the propulsion rate is 1.2-1.6 mL / h, the distance between the syringe nozzle and the titanium alloy is 15 cm, the drum speed is 1000-3000 rpm, and the time is 4-6 min;

[0017] Preferably, in S3, the total weight of the polylactic acid and KGN composite fibers accounts for 1-2% of the total dry weight of the bone support material;

[0018] Preferably, in S4, the amount of the natural silkworm cocoons added to the sodium carbonate aqueous solution is 20-24 g / L;

[0019] Preferably, in S4, the amount of the degummed silk added to the lithium bromide aqueous solution is 0.2-0.24 g / mL;

[0020] Preferably, in S4, the mass volume ratio of the degummed silk and glycidyl methacrylate is 20-24 g:5-7 mL;

[0021] Silk fibroin has excellent biocompatibility. Stem cells, osteoblasts, and macrophages can all adhere to and grow on silk fibroin materials. It also has low immunogenicity and natural anti-inflammatory properties, making it suitable for the regeneration and repair of a variety of tissues. Compared with other tissues, bone tissue repair takes longer, and degradation performance that matches bone regeneration can improve the quality of tissue repair. Tissue repair materials based on collagen or hyaluronic acid have a faster degradation rate and are more suitable for soft tissue repair. Natural silk is slowly absorbed in the body, and the degradation time is generally more than half a year. Its degradability is well matched with bone tissue. Silk fibroin can be used as a carrier to achieve efficient loading and controlled release of water-soluble, fat-soluble macromolecules or small molecule drugs, and different types of growth factors.

[0022] Preferably, in S5, the mass volume ratio of the titanium alloy, the modified mesoporous silica and the methacrylate modified silk fibroin solution is 20-30 g:15-35 g:100 mL;

[0023] Preferably, in S5, the modified mesoporous silica is mesoporous silica obtained by surface activation treatment using plasma immersion ion implantation technology;

[0024] Preferably, the processing conditions are: using a GPI-100 gas injector to inject argon into the mesoporous silica, the argon flow rate is 20-40sccm, the radio frequency is 8000-10000W, the pulse voltage is -20~-15kV, and the working pressure is 1×10 -2 -10×10 - 2 Pa, pulse width 80-120µs, pulse frequency 40-60Hz, treatment time 8-10min; the mesoporous silica nanoparticles are of model Sigma-Aldrich 748161, with a particle size of 200nm and a pore size of 4nm;

[0025] Preferably, in S6, the method for preparing oxidized icariin specifically comprises the following steps:

[0026] Dissolving icariin in anhydrous ethanol to obtain an icariin solution; dissolving sodium periodate in distilled water to obtain a sodium periodate aqueous solution, mixing the icariin solution and the sodium periodate aqueous solution, reacting for 3-5 hours in an ice bath in the dark, centrifuging at 1500-4500 rpm for 15-20 minutes, dialyzing with a dialysis bag with a molecular weight cutoff of 14 kD for 2-3 days, and freeze-drying the dialyzate to obtain oxidized icariin;

[0027] Preferably, the amount of icariin added to anhydrous ethanol is 0.2-0.25 g / mL;

[0028] Preferably, the mass volume ratio of sodium periodate to distilled water is 0.12-0.16 g / mL;

[0029] Icariin is the active ingredient of the traditional Chinese medicine Epimedium. In the field of traditional Chinese medicine, it has the effects of nourishing the liver and kidney, removing rheumatism, strengthening muscles and bones, improving immunity, anti-aging, and inhibiting tumors. Existing literature reports that icariin can effectively promote the directional differentiation of BMSCs into chondrocytes and can increase the protein products unique to chondrocytes. In the present invention, icariin is added to the bone support material as a repair factor, and is oxidized to give it an aldehyde group, which synergizes with silk fibroin to form a hydrogel structure, thereby achieving the effect of sustained release of the repair factor.

[0030] Preferably, the medical titanium alloy comprises, by mass percentage, the following: Zn: 2.5-4%, Ca: 1.2-2.1%, Sr: 0.12-0.24%, Al: 0.05-0.08%, and the balance is titanium.

[0031] The present invention provides a repair factor composite bone support material prepared by the above-mentioned preparation method.

[0032] The beneficial effects achieved by the present invention are as follows:

[0033] The present invention uses medical titanium alloy as a substrate, loads polylactic acid and KGN composite fibers on the surface of the medical titanium alloy after alkali heat activation by electrospinning to form a polymer coating, adds mesoporous silica obtained by surface activation treatment using plasma immersion ion implantation technology, mixes them evenly, soaks them in a hexahydrate zinc nitrate solution, adds a silk fibroin solution obtained by methacrylate modification, obtains a pretreated bone support material, and then soaks it in an oxidized icariin solution to form a hydrophilic three-dimensional network structure gel structure, stably coats the titanium alloy, and obtains a bone support material with good mechanical properties. The invention discloses a composite bone support material which improves the compatibility of medical titanium alloy materials with biological tissues, improves the compatibility of medical titanium alloy materials with biological tissues, reduces the rejection reaction of tissues to metal alloy materials, helps to reduce the inflammatory reaction and promotes wound healing; on the other hand, the hydroxyl group is negatively charged and can react with the positively charged Ca in physiological fluids. 2+Combining to form amorphous calcium phosphate is beneficial to initially improve the bone integration ability of orthopedic implant materials and promote the adsorption of polylactic acid and KGN on the surface of titanium alloy; polylactic acid is an absorbable polymer material with good biocompatibility and promotes tendon repair. KGN (Kartogenin) is a small molecule cartilage differentiation inducer that can induce MSC (bone marrow mesenchymal stem cells) to differentiate into chondrocytes, and the induction effect is ideal, which helps to promote the regeneration of chondrocytes. The synergistic effect of polylactic acid and KGN can improve the repair and regeneration of bone cells; the mesoporous Silica is surface activated by plasma immersion ion implantation technology to obtain modified mesoporous silica, which increases its specific surface area, roughness and porosity. After the modified mesoporous silica is mixed with titanium alloy material, the modified mesoporous silica has a small particle size of nanometers. The surface of the treated titanium alloy has a certain viscosity due to the coating of polylactic acid. At the same time, the pore structure formed by nanofibers can fix a part of the modified mesoporous silica. Under the entanglement of methacrylate-modified silk fibroin, the modified mesoporous silica and titanium alloy can be mixed. The treated titanium alloy material is physically combined to form a pretreated bone support material; it is immersed in a hexahydrate zinc nitrate solution to improve the antibacterial property of the bone support material; the silk fibroin is modified with methacrylate to improve the solubility, biocompatibility and blood compatibility of the silk fibroin, and the introduction of double bonds can provide a good cell adhesion matrix for the surrounding tissues, promote the migration and proliferation of bone cells, and thus accelerate the repair and regeneration of bone tissue. The amino group of the silk fibroin reacts with the aldehyde group of oxidized icariin to tightly connect the two together to form a three-dimensional In the porous hydrogel, the carboxyl groups of silk fibroin undergo amidation reaction with the amino groups in the bone tissue matrix, forming cross-linking again, thereby increasing the porosity of the hydrogel on the titanium alloy surface, promoting the deposition of hydroxyapatite, and achieving the technical effect of sustained release of icariin as a repair factor. In addition, icariin, as an active ingredient in traditional Chinese medicine, has anti-inflammatory properties and can avoid bone tissue infection. Due to the formation of multiple cross-links, it helps to achieve adhesion between the hydrogel and the damaged bone tissue, improve the stability of the hydrogel material and the gel strength, thereby improving the mechanical properties of the bone support material. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 The graphs show the test results of tensile strength and elongation at break of the bone support materials prepared in Examples 1-3 and Comparative Examples 1-4 of the present invention.

[0035] Figure 2 The graph shows the compressive strength and elastic modulus test results of the bone support materials prepared in Examples 1-3 and Comparative Examples 1-4 of the present invention.

[0036] Figure 3This is a graph showing the corrosion resistance test results of the bone support materials prepared in Example 1 and Comparative Examples 1 and 3 of the present invention.

[0037] Figure 4 The graph is a test result of the cell adhesion performance of the bone support materials prepared in Examples 1-3 and Comparative Examples 1-4 of the present invention.

[0038] Figure 5 The graph is a test result of the antibacterial properties of the bone support materials prepared in Examples 1-3 of the present invention and Comparative Examples 4 and 5.

[0039] Figure 6 This is a graph showing the anti-inflammatory performance test results of the bone support materials prepared in Examples 1-3 of the present invention and Comparative Examples 3 and 4.

[0040] Figure 7 This is a graph showing the repair factor release test results of the bone support materials prepared in Example 1 of the present invention and Comparative Examples 3 and 4.

[0041] Figure 8 This is a scanning electron microscope image of the surface morphology of the bone support material prepared in Example 1 of the present invention.

[0042] Fig. 9 This is a scanning electron microscopic image of the bone support material prepared in Example 1 of the present invention after mineralization in simulated body fluid for 28 days.

[0043] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION

[0044] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0045] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0046] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.

[0047] Example 1

[0048] A method for preparing a repair factor composite bone support material, specifically comprising the following steps:

[0049] S1. Select a disk-shaped medical titanium alloy with a diameter of 10.0 mm and a thickness of 0.25 mm, grind and polish the sample with silicon sandpaper of 800 mesh, 1000 mesh, 1500 mesh and 2000 mesh, soak it in 1.0 mol / L sodium hydroxide solution at 50°C for 20 h, clean it with ethanol, acetone and deionized water for 30 min, dry it and set it aside;

[0050] S2, dissolving 10 mg KGN in 1 mL acetone to obtain a KGN solution; dissolving 2.0 g polylactic acid in 10 mL of a mixed solvent of acetone and N,N-dimethylformamide in a volume ratio of 6:1 to obtain a polylactic acid solution; mixing 1 mL KGN solution and 10 mL polylactic acid solution to obtain a spinning solution for standby use;

[0051] S3, applying an external voltage of 10 kV to the spinning solution obtained in S2 through an electrospinning process, with a propulsion rate of 1.2 mL / h, so that a jet is formed under the action of an external electric field, and the jet is received by the titanium alloy treated by S1, with a distance of 15 cm between the syringe nozzle and the titanium alloy, a drum speed of 1000 rpm, and a time of 4 min, so that the jet is finally solidified into nanofibers on the surface of the titanium alloy, and a titanium alloy loaded with polylactic acid and KGN composite fibers is obtained for standby use;

[0052] S4, adding 20g of natural silk cocoons to 1L of 0.05mol / L sodium carbonate aqueous solution, boiling at 100°C for 20min, then rinsing with cold water, repeating the same treatment twice, drying, and obtaining degummed silk, adding 100mL of 9.2mol / L lithium bromide aqueous solution to 20g of degummed silk, dissolving at 65°C for 1h, dialyzing for 12h, obtaining a silk fibroin solution, adding 5mL of glycidyl methacrylate, stirring for 3h, dialyzing for 24h, obtaining a methacrylate-modified silk fibroin solution, and setting aside;

[0053] S5, mixing 20g of titanium alloy treated in S3 with 15g of modified mesoporous silica, adding 0.5mol / L hexahydrate zinc nitrate solution for soaking, placing at room temperature for 24h, freeze-drying, adding 100ml of methacrylate modified silk fibroin solution obtained in S4, stirring evenly at 4°C, freeze-drying at -2°C, obtaining a pretreated bone support material for standby use;

[0054] S6. Dissolve 50 mg of oxidized icariin in 100 mL of 50% by mass ethanol aqueous solution to obtain an oxidized icariin solution. Soak the pretreated bone support material obtained in S5 in the oxidized icariin solution, react at 4°C for 20 hours, wash with deionized water, and freeze-dry to obtain a repair factor composite bone support material.

[0055] The mesoporous silica used in this embodiment is mesoporous silica nanoparticles, model Sigma-Aldrich748161, with a particle size of 200 nm and a pore size of 4 nm. The modified mesoporous silica is mesoporous silica obtained by surface activation treatment using plasma immersion ion implantation technology; the treatment conditions are: argon gas is injected into the mesoporous silica using a GPI-100 gas injector, with an argon gas flow rate of 20 sccm, a radio frequency of 8000 W, a pulse voltage of -20 kV, and a working pressure of 1×10 -2 Pa, pulse width 80µs, pulse frequency 40Hz, and processing time 8min.

[0056] The preparation method of oxidized icariin specifically comprises the following steps:

[0057] Dissolve 10 g of icariin in 50 mL of anhydrous ethanol to obtain an icariin solution; dissolve 6 g of sodium periodate in 50 mL of distilled water to obtain an aqueous sodium periodate solution; mix the icariin solution and the aqueous sodium periodate solution, react for 3 h in an ice bath in the dark, centrifuge at 2000 rpm for 20 min, dialyze for 68 h using a dialysis bag with a molecular weight cutoff of 14 kD, and lyophilize the dialyzate to obtain oxidized icariin.

[0058] The present invention provides a repair factor composite bone support material prepared by the above-mentioned preparation method.

[0059] Figure 8 The surface morphology of the bone support material prepared in Example 1 of the present invention is shown in a scanning electron microscope image. The bone support material prepared in Example 1 was immersed in 20 mL of simulated body fluid and maintained in a water bath environment at 37°C. The simulated body fluid was replaced every 24 hours. After 28 days, the sample pieces were taken out and cleaned with deionized water, and then dried at low temperature. The surface morphology of each group of samples was observed under SEM. Fig. 9 This is a scanning electron microscopic image of the bone support material prepared in Example 1 of the present invention after mineralization in simulated body fluid for 28 days.

[0060] Example 2

[0061] A method for preparing a repair factor composite bone support material, specifically comprising the following steps:

[0062] S1. Select a disk-shaped medical titanium alloy with a diameter of 12.0 mm and a thickness of 0.3 mm, grind and polish the sample with 800 mesh, 1000 mesh, 1500 mesh and 2000 mesh silicon sandpaper in turn, soak it in 1.4 mol / L sodium hydroxide solution at 55°C for 22 hours, clean it with ethanol, acetone and deionized water for 35 minutes by ultrasonic vibration in turn, dry it and set it aside;

[0063] S2, dissolving 22.5 mg KGN in 1.5 mL acetone to obtain a KGN solution; dissolving 2.5 g polylactic acid in 10 mL of a mixed solvent of acetone and N,N-dimethylformamide in a volume ratio of 6:1 to obtain a polylactic acid solution; mixing 1.5 mL KGN solution and 10 mL polylactic acid solution to obtain a spinning solution for standby use;

[0064] S3, applying an external voltage of 15 kV to the spinning solution obtained in S2 through an electrospinning process, with a propulsion rate of 1.4 mL / h, so that a jet is formed under the action of an external electric field, and the jet is received by the titanium alloy treated by S1, with a distance of 15 cm between the syringe nozzle and the titanium alloy, a drum speed of 2000 rpm, and a time of 5 min, so that the jet is finally solidified into nanofibers on the surface of the titanium alloy, and a titanium alloy loaded with polylactic acid and KGN composite fibers is obtained for standby use;

[0065] S4, adding 22g of natural silk cocoons to 1L of 0.05mol / L sodium carbonate aqueous solution, boiling at 100°C for 25min, then rinsing with cold water, repeating the same treatment twice, drying, and obtaining degummed silk, adding 100mL of 9.2mol / L lithium bromide aqueous solution to 22g of degummed silk, dissolving at 70°C for 1.5h, dialyzing for 12h, obtaining a silk fibroin solution, adding 6mL of glycidyl methacrylate, stirring for 4h, dialyzing for 24h, obtaining a methacrylate-modified silk fibroin solution, and setting aside;

[0066] S5, mixing 25g of titanium alloy treated in S3 with 25g of modified mesoporous silica, adding 0.5mol / L hexahydrate zinc nitrate solution for soaking, placing at room temperature for 24h, freeze-drying, adding 100ml of methacrylate modified silk fibroin solution obtained in S4, stirring evenly at 4°C, freeze-drying at -2°C, obtaining a pretreated bone support material for standby use;

[0067] S6. Dissolve 200 mg of oxidized icariin in 100 mL of 55% by mass ethanol aqueous solution to obtain an oxidized icariin solution. Soak the pretreated bone support material obtained in S5 in the oxidized icariin solution, react at 4°C for 22 hours, wash with deionized water, and freeze-dry to obtain a repair factor composite bone support material.

[0068] The preparation method of modified mesoporous silica and oxidized icariin is implemented with reference to Example 1.

[0069] The present invention provides a repair factor composite bone support material prepared by the above-mentioned preparation method.

[0070] Example 3

[0071] A method for preparing a repair factor composite bone support material, specifically comprising the following steps:

[0072] S1. Select a rod-shaped medical titanium alloy with a diameter of 3.0 mm and a thickness of 10.0 mm, grind and polish the sample with 800 mesh, 1000 mesh, 1500 mesh and 2000 mesh silicon sandpaper in turn, soak it in 1.8 mol / L sodium hydroxide solution at 60°C for 24 h, clean it with ethanol, acetone and deionized water by ultrasonic vibration for 40 min in turn, dry it and set it aside;

[0073] S2, dissolving 40 mg KGN in 2 mL acetone to obtain a KGN solution; dissolving 3.0 g polylactic acid in 10 mL of a mixed solvent of acetone and N,N-dimethylformamide in a volume ratio of 6:1 to obtain a polylactic acid solution; mixing 2 mL of the KGN solution and 10 mL of the polylactic acid solution to obtain a spinning solution for standby use;

[0074] S3, applying an external voltage of 20 kV to the spinning solution obtained in S2 through an electrospinning process, with a propulsion rate of 1.6 mL / h, so that a jet is formed under the action of an external electric field, and the jet is received by the titanium alloy treated by S1, with a distance of 15 cm between the syringe nozzle and the titanium alloy, a drum speed of 3000 rpm, and a time of 6 min, so that the jet is finally solidified into nanofibers on the surface of the titanium alloy, and a titanium alloy loaded with polylactic acid and KGN composite fibers is obtained for standby use;

[0075] S4, adding 24g of natural silk cocoons to 1L of 0.05mol / L sodium carbonate aqueous solution, boiling at 100°C for 30min, then rinsing with cold water, repeating the same treatment 3 times, drying, and obtaining degummed silk, adding 100mL of 9.2mol / L lithium bromide aqueous solution to 24g of degummed silk, dissolving at 75°C for 2h, dialyzing for 12h, obtaining a silk fibroin solution, adding 7mL of glycidyl methacrylate, stirring for 5h, dialyzing for 24h, obtaining a methacrylate-modified silk fibroin solution, and setting aside;

[0076] S5, 30g of titanium alloy treated in S3 and 35g of modified mesoporous silica were mixed, and 0.5mol / L zinc nitrate hexahydrate solution was added for soaking, and the mixture was placed at room temperature for 24h, and freeze-dried, and 100ml of methacrylate modified silk fibroin solution obtained in S4 was added, and the mixture was stirred evenly at 4°C, and freeze-dried at -2°C to obtain a pretreated bone support material for standby use;

[0077] S6. Dissolve 300 mg of oxidized icariin in 100 mL of 60% by mass ethanol aqueous solution to obtain an oxidized icariin solution. Soak the pretreated bone support material obtained in S5 in the oxidized icariin solution, react at 4°C for 24 hours, wash with deionized water, and freeze-dry to obtain a repair factor composite bone support material.

[0078] The preparation method of modified mesoporous silica and oxidized icariin is implemented with reference to Example 1.

[0079] The present invention provides a repair factor composite bone support material prepared by the above-mentioned preparation method.

[0080] Comparative Example 1

[0081] This comparative example provides a repair factor composite bone support material and a preparation method thereof, which differs from Example 1 only in that polylactic acid is not included, and the remaining components, component contents, and preparation methods are the same as those of Example 1.

[0082] Comparative Example 2

[0083] This comparative example provides a repair factor composite bone support material and a preparation method thereof, which is different from Example 1 only in that modified mesoporous silica is not included, and the remaining components, component contents, and preparation methods are the same as those of Example 1.

[0084] Comparative Example 3

[0085] This comparative example provides a repair factor composite bone support material and a preparation method thereof, which differs from Example 1 only in that methacrylate-modified silk fibroin is not included, and the remaining components, component contents, and preparation methods are the same as those of Example 1.

[0086] Comparative Example 4

[0087] This comparative example provides a repair factor composite bone support material and a preparation method thereof, which is different from Example 1 only in that icariin is not subjected to oxidation treatment, and the remaining components, component contents, and preparation methods are the same as those in Example 1.

[0088] Comparative Example 5

[0089] This comparative example provides a repair factor composite bone support material and a preparation method thereof, which differs from Example 1 only in that it does not include the zinc nitrate hexahydrate solution immersion treatment, and the remaining components, component contents, and preparation methods are the same as those of Example 1.

[0090] Performance testing and result analysis

[0091] Mechanical properties test of bone support materials:

[0092] The bone support materials prepared in Examples 1-3 and Comparative Examples 1-4 were extruded into sample strips with a diameter of 20 mm×10 mm×100 μm (length×width×thickness). After the samples were completely formed, they were placed in a stretching device for a tensile test at a tensile rate of 1.0 mm / min and a tensile force of 50 N. The samples were stretched until they broke, and the tensile strength and elongation at break of each group of bone support materials were calculated. After the bone support materials prepared in Examples 1-3 and Comparative Examples 1-4 were made into sample strips, they were placed on the platform of a universal mechanical testing machine and compressed along the long axis of the sample strip at a speed of 0.5 mm / min. The compression was stopped when the deformation was 10%, and the compressive strength and elastic modulus were calculated.

[0093] Bone support material corrosion resistance test:

[0094] A Shanghai Chenhua CHI660E electrochemical workstation three-electrode system was used, the auxiliary electrode was a platinum electrode, the reference electrode was a saturated calomel electrode, the bone support materials prepared in Example 1 and Comparative Examples 1 and 3 were used as research electrodes, and a 3% NaCl aqueous solution was selected as the corrosive liquid to measure the corrosion resistance.

[0095] Bone support material cell adhesion performance test:

[0096] MC3T3-E1 mouse embryonic osteoblasts were selected as experimental cells and cultured using DMEM medium containing 10% fetal bovine serum and 1% penicillin / streptomycin. The osteoblasts were co-cultured on the surface of the bone support materials prepared in Examples 1-3 and Comparative Examples 1-4 in a 96-well plate for 24 hours, and then taken out and repeatedly washed with PBS buffer to remove cells that failed to attach successfully; 30 μL CCK-8 solution and 300 μL culture medium were added to each well under light-proof conditions, and culture was continued for 12 hours, and then 100 μL of the supernatant was aspirated and the absorbance (OD) was measured using an ELISA reader, and the wavelength was set to 450 nm. The cell adhesion rate was calculated according to the following formula: Adhesion rate = (number of adherent cells / total number of cells) × 100%.

[0097] Antibacterial performance test of bone support materials:

[0098] The bone support materials prepared in Examples 1-3 and Comparative Examples 4 and 5 were placed in corresponding groups on a 48-well plate, with 3 samples in each group, and the concentration of the Escherichia coli solution was adjusted to 10 6 CFU / mL, then add 300μL of Escherichia coli liquid to each well, and cover it with a sterile PE film, flatten it so that the liquid evenly covers the sample surface. To prevent the liquid on the sample surface from volatilizing, add sterile water to the gaps around the 48-well plate to provide a certain humidity. After incubating in a 37℃ electric constant temperature incubator for 6 hours, wash the bacteria on the sample surface with PBS solution and collect them. Take 100μL of the eluate and drop it on the nutrient agar medium plate, spread it evenly, invert it at 37℃ and incubate it for 24 hours, take out the plate, take pictures and count the number of live colonies on the fully automatic colony analyzer, and detect its antibacterial properties.

[0099] Bone support material anti-inflammatory performance test:

[0100] Mouse macrophage-like cell line RAW264.7 cells were inoculated and cultured on the surface of the bone support materials prepared in Examples 1-3 and Comparative Examples 3 and 4 and cultured for 3 days. The concentration of inflammatory factor TNF-α in the culture supernatant of RAW264.7 cells was detected by flow cytometry to evaluate the anti-inflammatory effect of the bone support materials.

[0101] Bone support material repair factor release test:

[0102] The bone support material samples prepared in Example 1 and Comparative Examples 3 and 4 were immersed in phosphate buffer and stored at 37° C. The test was conducted for 40 days, and the supernatant was taken out on the 1st, 7th, 14th, 21st, 28th, 35th and 42nd day, and the concentration of the repair factor in the solution was detected using an ICP-MS device.

[0103] Results Analysis

[0104] Figure 1 The graphs are test results of tensile strength and elongation at break of bone support materials prepared in Examples 1-3 and Comparative Examples 1-4 of the present invention. Figure 2The test results of the compressive strength and elastic modulus of the bone support materials prepared in Examples 1-3 and Comparative Examples 1-4 of the present invention are shown in FIG. As shown in the figure, the tensile properties and compressive properties of the bone support materials prepared in Comparative Examples 1-4 are significantly lower than those of the bone support materials prepared in Examples 1-3, wherein the tensile strength and compressive strength of Comparative Example 1 are the lowest. The bone support material prepared in Comparative Example 1 does not include polylactic acid, and only KGN chondrogenic differentiation inducer is loaded on the surface of the titanium alloy, indicating that adding polylactic acid by electrospinning and loading it on the surface of the titanium alloy is helpful to improve the mechanical properties of the titanium alloy; Comparative Example 2 does not include modified Mesoporous silica will also reduce the mechanical properties; Comparative Example 3 does not include methacrylate-modified silk fibroin. As a natural polymer material, silk fibroin has good mechanical properties, indicating that a Schiff base reaction occurs between the amino group of silk fibroin and the aldehyde group of oxidized icariin, thereby improving the stability of the gel on the surface of the titanium alloy, thereby helping to improve the mechanical properties of the bone support material; In Comparative Example 4, icariin is not oxidized, and icariin does not contain an aldehyde group, and cannot undergo a Schiff base reaction with the modified silk fibroin, and cannot form a stable gel structure to coat the titanium alloy, which will reduce its mechanical properties.

[0105] Figure 3 The figure is a test result of the corrosion resistance of the bone support material prepared by Example 1 of the present invention and Comparative Examples 1 and 3. As shown in the figure, compared with the bone support materials prepared by Comparative Examples 1 and 3, the self-corrosion current density of the bone support material prepared by Example 1 of the present invention is significantly reduced, and the self-corrosion potential is significantly increased, indicating that the orthopedic implant material prepared by Example 1 has excellent corrosion resistance. The bone support material prepared in Example 1 is based on a metal titanium alloy, and polylactic acid and KGN composite fibers are loaded on the surface by electrospinning, and modified mesoporous silica obtained by surface activation treatment by plasma immersion ion implantation technology is added, and the surface is immersed in an antibacterial active solution, and silk fibroin modified by methyl acrylate and oxidized icariin are added. The presence of polylactic acid fiber can form a stable protective film on the surface of the titanium alloy, reducing the wear degree of the titanium alloy. Due to the presence of the modified silk fibroin, its amino group reacts with the aldehyde group of oxidized icariin to form a Schiff base reaction, thereby forming a stable three-dimensional hydrogel structure, avoiding direct contact between the titanium alloy and the bone tissue matrix, thereby causing rapid corrosion.

[0106] Figure 4The results of the cell adhesion test of the bone support materials prepared in Examples 1-3 and Comparative Examples 1-4 of the present invention are shown in the figure. As shown in the figure, the cell adhesion rates of the bone support materials prepared in Examples 1-3 are 35.1%, 36.3% and 34.9%, respectively, while the cell adhesion rates of the bone support materials prepared in Comparative Examples 1-4 are only 27.5%, 24.3%, 22.8% and 29.4%, respectively; the bone support material prepared in Comparative Example 1 does not include polylactic acid, which cannot provide more surface area for the adhesion of bone cells, thereby reducing its cell adhesion rate; Comparative Example 2 does not include modified Mesoporous silica, the reason for the decrease in cell adhesion rate is that the addition of modified mesoporous silica helps to increase the specific surface area of ​​the titanium alloy, improve its roughness and porosity, provide more bioactive sites for the titanium alloy, and promote the adsorption and proliferation of bone cells; Comparative Example 3 does not include modified silk fibroin, does not introduce double bonds, lacks the presence of adhesive groups, reduces the migration and proliferation of bone cells, and thus slows down the bone tissue repair and regeneration process; In Comparative Example 4, icariin is not oxidized and cannot interact with the modified silk fibroin to form an adhesive gel structure, thereby reducing its adhesion performance.

[0107] Figure 5 The antibacterial property test results of the bone support materials prepared by Examples 1-3 and Comparative Examples 4 and 5 of the present invention are shown in the figure. As shown in the figure, the antibacterial rates of the bone support materials prepared by Examples 1-3 are 87.3%, 86.5% and 88.1%, respectively, while the antibacterial rates of the bone support materials prepared by Comparative Examples 4 and 5 are 79.6% and 67.8%, respectively; in Comparative Example 4, icariin is not oxidized, and icariin, as an active ingredient of the traditional Chinese medicine Epimedium, is an oxidized icariin obtained by aldehyde modification at the C-3 position, which has antibacterial activity, and thus reduces its antibacterial property; Comparative Example 5 does not include a hexahydrate zinc nitrate solution, and zinc ions are released into the surrounding environment, combined with phospholipids and proteins on the bacterial cell membrane, destroying the integrity of the cell membrane, causing leakage of intracellular substances, causing bacterial death or growth restriction, thereby reducing the risk of infection. Since zinc ions are not introduced in Comparative Example 5, the antibacterial property of the bone support material is greatly reduced.

[0108] Figure 6 The anti-inflammatory performance test results of the bone support materials prepared by Examples 1-3 of the present invention and Comparative Examples 3 and 4 are shown in the figure. As shown in the figure, the TNF-α concentrations of the Example 1-3 groups are 218.5 pg / mL, 209.8 pg / mL and 224.6 pg / mL, respectively, while the TNF-α concentrations of the Comparative Examples 3 and 4 groups are as high as 262.4 pg / mL and 298.6 pg / mL, respectively. The cells cultured on the surface of the bone support materials prepared by Examples 1-3 release less inflammatory factors, indicating that the bone support materials prepared by Examples 1-3 have good anti-inflammatory properties, and silk fibroin and oxidized icariin act synergistically to provide anti-inflammatory effects on the bone support materials.

[0109] Figure 7 The figure is a test result of the release of repair factors of the bone support materials prepared in Example 1 and Comparative Examples 3 and 4 of the present invention. As shown in the figure, the release of the repair factors in the bone support material prepared in Example 1 is relatively slow, and the release amount of the repair factors reaches 0.68 ng / mL after 42 days. Compared with Example 1, the release of the repair factors in the bone support materials prepared in Comparative Examples 3 and 4 is relatively fast. After 42 days, the release amounts of the repair factors in Comparative Examples 3 and 4 are as high as 0.79 ng / mL and 0.85 ng / mL, respectively; it indicates that the silk fibroin modified by glycidyl methacrylate and oxidized icariin are added to the titanium alloy, and the Schiff base reaction occurs between the amino group of the silk fibroin and the aldehyde group of the oxidized icariin to form a three-dimensional porous cross-linked hydrogel structure, which is conducive to the slow and orderly release of the repair factors.

[0110] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.

[0111] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a repair factor composite bone support material, characterized in that: The preparation method comprises the following steps: S1. Select a medical titanium alloy, extrude it into a titanium plate or rod, grind and polish the sample with 800 mesh, 1000 mesh, 1500 mesh and 2000 mesh silicon sandpaper, soak it in 1.0-1.8 mol / L sodium hydroxide solution at 50-60°C for 20-24h, clean it with ethanol, acetone and deionized water ultrasonically for 30-40min, dry it and set it aside; S2, dissolving KGN in acetone to obtain a KGN solution; dissolving polylactic acid in a mixed solvent of acetone and N,N-dimethylformamide in a volume ratio of 6:1 to obtain a polylactic acid solution; mixing the KGN solution and the polylactic acid solution to obtain a spinning solution for standby use; S3, applying an external voltage to the spinning solution obtained in S2 through an electrostatic spinning process, so that a jet is formed under the action of an external electric field, and the jet is received by the titanium alloy treated by S1, so that the jet is finally solidified into nanofibers on the surface of the titanium alloy, thereby obtaining a titanium alloy loaded with polylactic acid and KGN composite fibers for standby use; S4, adding natural silk cocoons to a sodium carbonate aqueous solution with a concentration of 0.05 mol / L, boiling at 100°C for 20-30 min, then rinsing with cold water, repeating the same treatment 2-3 times, drying to obtain degummed silk, adding a lithium bromide aqueous solution with a concentration of 9.2 mol / L, dissolving at 65-75°C for 1-2 h, dialyzing for 12 h, obtaining a silk fibroin solution, adding glycidyl methacrylate, stirring for 3-5 h, dialyzing for 24 h, obtaining a methacrylate-modified silk fibroin solution, and setting aside; S5, mixing the titanium alloy treated by S3 with the modified mesoporous silica, adding a 0.5 mol / L zinc nitrate hexahydrate solution for immersion treatment, placing at room temperature for 24 hours, freeze-drying, adding the methacrylate modified silk fibroin solution obtained by S4, stirring evenly at 4°C, freeze-drying at -2°C, obtaining a pretreated bone support material for standby use; The modified mesoporous silica is obtained by surface activation treatment of mesoporous silica by plasma immersion ion implantation technology. The treatment conditions are: using a GPI-100 gas injector to inject argon gas into the mesoporous silica, the argon gas flow rate is 20-40sccm, the radio frequency is 8000-10000W, the pulse voltage is -20~-15kV, and the working pressure is 1×10 -2 -10×10 -2 Pa, pulse width 80-120µs, pulse frequency 40-60Hz, treatment time 8-10min; S6. Dissolve oxidized icariin in an ethanol aqueous solution with a mass fraction of 50-60% to obtain an oxidized icariin solution with a concentration of 0.5-3 mg / mL, soak the pretreated bone support material obtained in S5 in the oxidized icariin solution, react at 4°C for 20-24 hours, wash with deionized water, and freeze-dry to obtain a repair factor composite bone support material.

2. The method for preparing a repair factor composite bone support material according to claim 1, characterized in that: In S2, the amount of KGN added to acetone is 0.01-0.02 g / mL; the amount of polylactic acid added to the mixed solvent of acetone and N,N-dimethylformamide is 0.2-0.3 g / mL; and the volume ratio of the KGN solution to the polylactic acid solution is 1-2:

10.

3. The method for preparing a repair factor composite bone support material according to claim 2, characterized in that: In S3, the conditions of the electrospinning process are: the external voltage is 10-20 kV, the propulsion rate is 1.2-1.6 mL / h, the distance between the syringe nozzle and the titanium alloy is 15 cm, the drum speed is 1000-3000 rpm, and the time is 4-6 min; the total weight of the polylactic acid and KGN composite fibers accounts for 1-2% of the total dry weight of the bone support material.

4. The method for preparing a repair factor composite bone support material according to claim 3, characterized in that: In S4, the amount of the natural silk cocoons added to the sodium carbonate aqueous solution is 20-24 g / L; the amount of the degummed silk added to the lithium bromide aqueous solution is 0.2-0.24 g / mL; the mass volume ratio of the degummed silk and glycidyl methacrylate is 20-24 g:5-7 mL.

5. The method for preparing a repair factor composite bone support material according to claim 4, characterized in that: In S5, the mass volume ratio of the titanium alloy, the modified mesoporous silica and the methacrylate modified silk fibroin solution is 20-30 g:15-35 g:100 mL.

6. The method for preparing a repair factor composite bone support material according to claim 5, characterized in that: In S6, the method for preparing oxidized icariin specifically comprises the following steps: The icariin solution is dissolved in anhydrous ethanol to obtain an icariin solution; sodium periodate is dissolved in distilled water to obtain an aqueous sodium periodate solution; the icariin solution and the aqueous sodium periodate solution are mixed, reacted for 3-5 hours in an ice bath in the dark, centrifuged at 2000-3000 rpm for 20-30 minutes, dialyzed with a dialysis bag with a molecular weight cutoff of 14 kD for 68-74 hours, and the dialyzate is freeze-dried to obtain oxidized icariin.

7. The method for preparing a repair factor composite bone support material according to claim 6, characterized in that: The amount of icariin added to anhydrous ethanol is 0.2-0.25 g / mL; the mass volume ratio of sodium periodate to distilled water is 0.12-0.16 g / mL.

8. The method for preparing a repair factor composite bone support material according to claim 7, characterized in that: The medical titanium alloy comprises, by mass percentage, 2.5-4% Zn, 1.2-2.1% Ca, 0.12-0.24% Sr, 0.05-0.08% Al, and the balance is titanium.

9. A repair factor composite bone support material, characterized in that: The bone support material is prepared by the preparation method according to any one of claims 1 to 8.