A method for preparing kaolinite-based lithium ion adsorbent
Through the preparation of kaolinite-based lithium ion adsorbent, the aluminum and silicon of kaolinite itself are converted into LiCl·2Al(OH)3·nH2O and active SiO2, which solves the problem of high reagent consumption and adsorption capacity of existing aluminum-based adsorbents. Low problem, achieving efficient lithium ion adsorption and effective utilization of resources.
Patent Information
- Application Number
- CN202410608411.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-16
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-05-16
AI Technical Summary
Existing aluminum-based lithium ion adsorbents consume a large amount of reagents during the lithium extraction process and the adsorption capacity of a single lithium-aluminum composite hydroxide is low.
Kaolinite is used as raw material, and kaolinite-based lithium ion adsorbent is prepared through activation, alkali dissolution, acid conversion and surface grafting. The aluminum and silicon of kaolinite itself are used to convert it into LiCl·2Al(OH)3 ·nH2O and active SiO2 are used to introduce sulfonic acid groups through chemical grafting to prepare organic-inorganic composite lithium ion adsorbents.
The dosage of AlCl3, NaOH and LiCl is reduced, the adsorption capacity of lithium ions and resource utilization rate are improved, and it has high lithium ion adsorption capacity and regeneration performance.
Smart Images

Figure CN118341389B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion enrichment and extraction in lithium-containing energy minerals, and in particular relates to a method for preparing a kaolinite-based lithium ion adsorbent. Background Art
[0002] Lithium extraction from brine is an important source of lithium resources in my country. The adsorption method for separating and extracting lithium ions from brine has the advantages of simple operation, recyclability and low energy consumption.
[0003] At present, the adsorbents for lithium extraction from brine mainly include manganese ion sieves, titanium ion sieves and aluminum adsorbents. Among them, aluminum adsorbents are the only material that has been industrially applied to extract lithium from brine by adsorption. They are characterized by good selectivity and mild regeneration conditions. Their core is LiCl·2Al(OH)3·nH2O or its derived lithium-aluminum composite hydroxide.
[0004] Aluminum-based adsorbents are mostly synthesized by chemical precipitation. During the reaction, the consumption of reagents such as AlCl3, NaOH and LiCl is large, and the economic efficiency is relatively poor. In addition, the use of a single lithium aluminum composite hydroxide as an adsorbent for lithium ions also has a low adsorption capacity. Summary of the invention
[0005] In view of the above analysis, the present invention aims to provide a method for preparing a kaolinite-based lithium ion adsorbent to solve at least one of the problems in the prior art of large reagent consumption of aluminum-based adsorbents and low adsorption capacity of a single lithium aluminum composite hydroxide.
[0006] The purpose of the present invention is mainly achieved through the following technical solutions.
[0007] The invention provides a method for preparing a kaolinite-based lithium ion adsorbent, wherein pulverized natural kaolinite is sequentially activated, alkali-dissolved, acid-converted and surface-grafted to obtain the kaolinite-based lithium ion adsorbent.
[0008] Furthermore, the preparation method comprises the following steps:
[0009] Step 1: crushing natural kaolinite to obtain kaolinite powder, calcining and cooling the kaolinite powder to obtain activated kaolinite powder;
[0010] Step 2: Evenly mix the activated kaolinite powder and the NaOH solution, stir to perform an alkali dissolution reaction, and cool and filter to obtain a filtrate;
[0011] Step 3: Add HCl solution dropwise to the filtrate to adjust the pH to 1-2, and stir to carry out acid conversion reaction;
[0012] Then, LiCl was added to the system to fully dissolve, and the pH was adjusted to 4-5 with NaOH solution, and the reaction was continued by stirring. The reaction product was filtered and dried to obtain a solid phase;
[0013] Step 4: mixing the solid phase with the silane coupling agent and the organic solvent, reacting at 115-125° C. for 20-28 hours, filtering and drying the reaction product to obtain a first powder product;
[0014] Step 5: After mixing the first powder product with the chloroacetic acid solution, adding a NaOH solution to adjust the pH to 8-8.5 for reaction, filtering and drying the reaction product to obtain a second powder product;
[0015] Step 6: Dissolve 2-hydroxyethyl sulfonic acid and NaOH in an organic solvent, mix well with the second powder product and reflux for reaction, filter and wash the reaction product to neutrality and then dry it to obtain a kaolinite-based lithium ion adsorbent.
[0016] Furthermore, in step 1, the calcination temperature is 550-650° C., and the calcination time is 1-3 hours.
[0017] Furthermore, in step 2, the alkali dissolution reaction temperature is 110-125° C., and the alkali dissolution reaction time is 6-12 h.
[0018] Furthermore, in step 1, the particle size of the kaolinite powder is 160-200 mesh.
[0019] Furthermore, in step 2, the mass volume ratio of the activated kaolinite powder to the NaOH solution is 45-55:220-260 g / mL, and the concentration of NaOH is 80-160 g / L.
[0020] Furthermore, the mass ratio of the activated kaolinite powder to LiCl is 8-12:1.
[0021] Furthermore, the mass volume ratio of the activated kaolinite powder to the silane coupling agent is 45-55:5-10 g / mL, and the mass volume ratio of the activated kaolinite powder to toluene is 45-55:220-260 g / mL.
[0022] Furthermore, the mass volume ratio of the activated kaolinite powder to the chloroacetic acid solution is 45-55:220-260 g / mL, and the concentration of the chloroacetic acid solution is 0.5-1 g / L.
[0023] Furthermore, in step 6, the mass ratio of 2-hydroxyethyl sulfonic acid to NaOH is 1-3:0.5-1, and the mass volume ratio of 2-hydroxyethyl sulfonic acid to ethanol is 1-3:220-260 g / mL.
[0024] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects.
[0025] A) The preparation method of the kaolinite-based lithium ion adsorbent provided by the present invention uses cheap and easily available natural kaolinite as a raw material, and fully utilizes the aluminum and silicon of the kaolinite itself by activation, alkali dissolution, acid conversion and surface grafting without adding an external aluminum source and silicon source, converts the aluminum source in the kaolinite powder into LiCl·2Al(OH)3·nH2O, converts the silicon in the kaolinite powder into active SiO2 and introduces sulfonic acid groups by chemical grafting, so as to prepare an organic-inorganic composite lithium ion adsorbent loaded on the material. Compared with the conventional inorganic lithium aluminum composite hydroxide synthesized by using AlCl3, NaOH and LiCl chemical reagents, the amount of AlCl3, NaOH and LiCl is significantly reduced, and new lithium ion adsorption sites are introduced, which is not only beneficial to the extraction of lithium resources in brine, but also beneficial to the effective utilization of kaolinite resources.
[0026] B) The preparation method of the kaolinite-based lithium ion adsorbent provided by the present invention comprises crushing and calcining the kaolinite, so as to activate the kaolinite which is insoluble in acid and alkali, so as to facilitate the subsequent reaction between the activated kaolinite powder and the NaOH solution; reacting the NaOH with the activated kaolinite powder, so that the aluminum source in the activated kaolinite powder is converted into sodium aluminate (NaAlO2), and the silicon source in the activated kaolinite powder is converted into sodium silicate (Na2SiO4); adding HCl to adjust the pH to 1-2 is aimed at converting Na2SiO4 into active SiO2, At the same time, NaAlO2 is converted into AlCl3, and then LiCl is added and the pH is adjusted to neutral, the purpose of which is to convert AlCl3 into LiCl·2Al(OH)3·nH2O; the active SiO2 surface hydroxyl group reacts with a silane coupling agent to introduce an amino group (-NH2); the amino group is dehydrogenated and dechlorinated with chloroacetic acid to connect a carboxyl group (-COOH), i.e. -NH-COOH; the carboxyl group reacts with the hydroxyl group of 2-hydroxyethylsulfonic acid to undergo a dehydration reaction, thereby connecting a sulfonic acid group to the SiO2 surface, i.e. -NH-COO-(CH2)2-SO3H.
[0027] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained through the contents particularly pointed out in the embodiments of the description and the drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] The drawings are only for the purpose of illustrating particular embodiments and are not to be considered limiting of the present invention. Like reference symbols denote like components throughout the drawings.
[0029] Figure 1aThis is a SEM image of the kaolinite raw material in Example 3 of the present invention;
[0030] Figure 1b This is a SEM image of the adsorbent prepared in Example 3 of the present invention;
[0031] Figure 2 This is the XRD pattern of the adsorbent prepared in Example 3 of the present invention. DETAILED DESCRIPTION
[0032] The preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used together with the embodiments of the present invention to illustrate the principles of the present invention, but are not used to limit the scope of the present invention.
[0033] The invention provides a method for preparing a kaolinite-based lithium ion adsorbent, wherein pulverized natural kaolinite is sequentially activated, alkali-dissolved, acid-converted and surface-grafted to obtain the kaolinite-based lithium ion adsorbent.
[0034] Specifically, the above preparation method comprises the following steps:
[0035] Step 1: crushing natural kaolinite to obtain kaolinite powder, placing the kaolinite powder in a nickel crucible, calcining at 550-650° C. for 1-3 hours, and cooling to room temperature to obtain activated kaolinite powder;
[0036] Step 2: Evenly mix the activated kaolinite powder and the NaOH solution, stir at 110-125° C. for 6-12 hours for alkaline dissolution reaction, and obtain a filtrate after cooling and filtration;
[0037] Step 3: Slowly add 1 mol / L HCl solution to the filtrate, adjust the pH to 1-2, and stir to carry out acid conversion reaction for 3-6 hours;
[0038] Then, LiCl was added to the system to fully dissolve, and the pH was adjusted to 4-5 with 1 mol / L NaOH solution, and the reaction was continued with stirring for 3-6 hours. The reaction product was filtered and dried at 58-62°C to obtain a solid phase;
[0039] Step 4: reacting the solid phase with a silane coupling agent (e.g., KH550) and an organic solvent (e.g., toluene) at 115-125° C. for 20-28 hours, filtering the reaction product and drying it at 110-130° C. for 20-28 hours to obtain a first powder product;
[0040] Step 5: After mixing the first powder product with the chloroacetic acid solution, add a NaOH solution to adjust the pH to 8-8.5, react for 20-28 hours, filter the reaction product and dry it at 58-62° C. to constant weight to obtain a second powder product;
[0041] Step 6: Dissolve 2-hydroxyethyl sulfonic acid and NaOH in an organic solvent (e.g., ethanol), mix well with the second powder product, and reflux at 110-130° C. for 20-28 hours. Filter and wash the reaction product to neutrality, and then dry at 58-62° C. to constant weight to obtain a kaolinite-based lithium ion adsorbent.
[0042] The kaolinite-based lithium ion adsorbent comprises spherical particles and nanosheets attached to the surface of the spherical particles. The spherical particles are chemically grafted SiO2, and the nanosheets are LiCl·2Al(OH)3·nH2O.
[0043] Compared with the prior art, the preparation method of the kaolinite-based lithium ion adsorbent provided by the present invention uses cheap and easily available natural kaolinite as a raw material, and fully utilizes the aluminum and silicon of the kaolinite itself by activation, alkali dissolution, acid conversion and surface grafting without adding an external aluminum source and silicon source, converts the aluminum source in the kaolinite powder into LiCl·2Al(OH)3·nH2O, converts the silicon in the kaolinite powder into active SiO2 and introduces sulfonic acid groups by chemical grafting, so as to prepare an organic-inorganic composite lithium ion adsorbent loaded on the material. Compared with the conventional inorganic lithium aluminum composite hydroxide synthesized by using AlCl3, NaOH and LiCl chemical reagents, the amount of AlCl3, NaOH and LiCl is significantly reduced, and new lithium ion adsorption sites are introduced, which is not only beneficial to the extraction of lithium resources in brine, but also beneficial to the effective utilization of kaolinite resources.
[0044] Specifically, since kaolinite is insoluble in acid and alkali under normal conditions, in the above step 1, the kaolinite is crushed and calcined to activate the kaolinite that is insoluble in acid and alkali, so that the activated kaolinite powder and the NaOH solution react in the subsequent step (i.e., step 2); in the above step 2, NaOH is reacted with the activated kaolinite powder to convert the aluminum source in the activated kaolinite powder into sodium aluminate (NaAlO2), and the silicon source in the activated kaolinite powder into sodium silicate (Na2SiO4); in the above step 3, The purpose of adding HCl to adjust the pH to 1-2 is to convert Na2SiO4 into active SiO2 and NaAlO2 into AlCl3. Then, LiCl is added and the pH is adjusted to neutral, the purpose of which is to convert AlCl3 into LiCl·2Al(OH)3·nH2O. In the above step 4, the hydroxyl groups on the surface of active SiO2 react with a silane coupling agent to introduce amino groups (-NH2). In the above step 5, the amino groups are dehydrogenated and dechlorinated with chloroacetic acid to connect carboxyl groups (-COOH), i.e., -NH-COOH. In the above step 6, the carboxyl group reacts with the hydroxyl group of 2-hydroxyethylsulfonic acid to undergo a dehydration reaction, thereby connecting sulfonic acid groups on the surface of SiO2, i.e., -NH-COO-(CH2)2-SO3H.
[0045] Considering that the specific surface area of kaolinite powder will affect the subsequent reaction, in order to promote the subsequent reaction, in the above step 1, the particle size of kaolinite powder is 160-200 mesh.
[0046] In order to fully alkaline dissolve the kaolinite powder, in the above step 2, the mass volume ratio of the activated kaolinite powder to the NaOH solution is 45-55:220-260 g / mL, and the concentration of NaOH is 80-160 g / L.
[0047] Illustratively, in the above preparation method, the mass ratio of activated kaolinite powder to LiCl is 8 to 12:1.
[0048] In the above preparation method, the mass volume ratio of the activated kaolinite powder and the silane coupling agent is 45-55:5-10 g / mL, and the mass volume ratio of the activated kaolinite powder and toluene is 45-55:220-260 g / mL.
[0049] The mass volume ratio of the activated kaolinite powder and the chloroacetic acid solution is 45-55:220-260 g / mL, and the concentration of the chloroacetic acid solution is 0.5-1 g / L.
[0050] In the above step 6, the mass ratio of 2-hydroxyethyl sulfonic acid to NaOH is 1-3:0.5-1, and the mass volume ratio of 2-hydroxyethyl sulfonic acid to ethanol is 1-3:220-260 g / mL.
[0051] After testing, the kaolinite-based lithium ion adsorbent prepared by the preparation method of the present invention has a lithium ion adsorption capacity of 3.3-4.3 mg per gram of kaolinite-based lithium ion adsorbent. After 5 cycles of adsorption-desorption, the lithium ion adsorption capacity of kaolinite-based lithium ion adsorbent per gram is 2.8-3.8 mg, which has high lithium ion adsorption capacity and regeneration performance.
[0052] In order to investigate the lithium ion adsorption and regeneration performance of the kaolinite-based lithium ion adsorbent, the above step 6 further includes the following steps:
[0053] Step a: Add 1.0 g of adsorbent into a conical flask containing 25 mL of brine, the lithium ion concentration of the brine is 85.76 mg / L, and oscillate and adsorb for 12 hours at room temperature. Use ICP-OES to determine the lithium ion concentration in the brine, and calculate the amount of lithium ions adsorbed in the brine, where the adsorption amount is expressed as the lithium ion adsorption per unit mass of bauxite, i.e. mg / (g kaolinite).
[0054] Step b: After the adsorbent after adsorbing lithium ions in step a is shaken and desorbed with 50 mL of dilute HCl solution with pH=4 at room temperature for 6 hours, the adsorbent is dried for later use.
[0055] Step c: Repeat steps a to b at least 5 times to test the recycling performance of the adsorbent.
[0056] Examples 1 to 3 of the present invention and Comparative Examples 1 to 4 are described in detail below.
[0057] Example 1
[0058] The preparation method of the kaolinite-based lithium ion adsorbent provided in this embodiment comprises the following steps:
[0059] (1) After natural kaolinite is crushed, 160-200 mesh powder is collected, 50 g of the powder is placed in a nickel crucible, calcined at 550° C. for 3 h, and then cooled to room temperature for use.
[0060] (2) The calcined kaolinite powder in step (1) was mixed evenly with 250 mL of 80 g / L NaOH solution, stirred and reacted at 120° C. for 6 h, cooled and filtered, and the filtrate was stored for later use.
[0061] (3) Slowly add 1 mol / L HCl solution to the filtrate in step (2), adjust the pH to 1.5, and stir the reaction for 3 hours. Then add 5 g LiCl, and after it is fully dissolved, adjust the pH to 5.0 with 1 mol / L NaOH solution, and continue to stir the reaction for 4 hours. After filtration, the solid phase is dried at 60°C to constant weight for use.
[0062] (4) The solid phase in step (3) was reacted with 5 mL of silane coupling agent KH550 and 250 mL of toluene at 120° C. for 24 h and then filtered. The solid phase was dried at 120° C. for 24 h and then set aside.
[0063] (5) The powder in step (4) was mixed with 250 mL of 0.5 g / L chloroacetic acid solution, and NaOH solution was added to adjust the pH to 8.2. After reacting for 24 h, the mixture was filtered and the solid phase was dried at 60 °C to constant weight.
[0064] (6) 1.5 g of 2-hydroxyethyl sulfonic acid and 0.6 g of NaOH were dissolved in 250 mL of ethanol, mixed evenly with the powder in step (5), refluxed at 120° C. for 24 h, filtered and washed to neutrality, and then dried at 60° C. to constant weight to obtain a kaolinite-based lithium ion adsorbent.
[0065] (7) Lithium ion adsorption and regeneration performance: 1.0 g of the adsorbent was weighed and mixed with 25 mL of brine in a conical flask. The mixture was adsorbed at room temperature for 6 h. The adsorption capacity of lithium ions was 3.45 mg / (g kaolinite). After 5 cycles of adsorption-desorption, the adsorbent adsorbed 2.82 mg / (g kaolinite).
[0066] Example 2
[0067] The preparation method of the kaolinite-based lithium ion adsorbent provided in this embodiment comprises the following steps:
[0068] (1) After natural kaolinite is crushed, a powder of 160-200 mesh is collected, and 50 g of the powder is placed in a nickel crucible, calcined at 600° C. for 3 h, and then cooled to room temperature for use.
[0069] (2) The calcined kaolinite powder in step (1) was mixed evenly with 230 mL of a 120 g / L NaOH solution, stirred and reacted at 110° C. for 10 h, cooled and filtered, and the filtrate was stored for later use.
[0070] (3) Slowly add 1 mol / L HCl solution to the filtrate in step (2), adjust the pH to 1.0, and stir the reaction for 5 hours. Then add 4.5 g LiCl, and after it is fully dissolved, adjust the pH to 4.5 with 1 mol / L NaOH solution, and continue to stir the reaction for 5 hours. After filtration, the solid phase is dried at 60°C to constant weight for use.
[0071] (4) The solid phase in step (3) was reacted with 8 mL of silane coupling agent KH550 and 230 mL of toluene at 115° C. for 26 h and then filtered. The solid phase was dried at 110° C. for 28 h and then set aside.
[0072] (5) The powder in step (4) was mixed with 225 mL of 0.8 g / L chloroacetic acid solution, and NaOH solution was added to adjust the pH to 8.0. After reacting for 26 h, the mixture was filtered and the solid phase was dried at 60° C. to constant weight.
[0073] (6) 2.0 g of 2-hydroxyethyl sulfonic acid and 0.8 g of NaOH were dissolved in 230 mL of ethanol, mixed evenly with the powder in step (5), refluxed at 125° C. for 22 h, filtered and washed to neutrality, and then dried at 60° C. to constant weight to obtain a kaolinite-based lithium ion adsorbent.
[0074] (7) Lithium ion adsorption and regeneration performance: 1.0 g of the adsorbent was weighed and mixed with 25 mL of brine in a conical flask. The mixture was adsorbed at room temperature for 6 h. The adsorption capacity of lithium ions was 4.05 mg / (g kaolinite). After 5 cycles of adsorption-desorption, the adsorbent adsorbed 3.36 mg / (g kaolinite).
[0075] Example 3
[0076] The preparation method of the kaolinite-based lithium ion adsorbent provided in this embodiment comprises the following steps:
[0077] (1) After natural kaolinite is crushed, 160-200 mesh powder is collected, 50 g of the powder is placed in a nickel crucible, calcined at 650° C. for 2 h, and then cooled to room temperature for use.
[0078] (2) The calcined kaolinite powder in step (1) was mixed evenly with 250 mL of a 160 g / L NaOH solution, stirred and reacted at 120° C. for 12 h, cooled and filtered, and the filtrate was stored for later use.
[0079] (3) Slowly add 1 mol / L HCl solution to the filtrate in step (2), adjust the pH to 1.0, and stir the reaction for 6 hours. Then add 5 g LiCl, and after it is fully dissolved, adjust the pH to 4.0 with 1 mol / L NaOH solution, and continue to stir the reaction for 6 hours. After filtration, the solid phase is dried at 60°C to constant weight for use.
[0080] (4) The solid phase in step (3) was reacted with 10 mL of silane coupling agent KH550 and 250 mL of toluene at 120° C. for 24 h and then filtered. The solid phase was dried at 120° C. for 24 h and then set aside.
[0081] (5) The powder in step (4) was mixed with 250 mL of 1.0 g / L chloroacetic acid solution, and NaOH solution was added to adjust the pH to 8.5. After reacting for 24 h, the mixture was filtered and the solid phase was dried at 60 °C to constant weight.
[0082] (6) 2.5 g of 2-hydroxyethyl sulfonic acid and 1.0 g of NaOH were dissolved in 250 mL of ethanol, mixed evenly with the powder in step (5), refluxed at 120° C. for 24 h, filtered and washed to neutrality, and then dried at 60° C. to constant weight to obtain a kaolinite-based lithium ion adsorbent.
[0083] (7) Lithium ion adsorption and regeneration performance: 1.0 g of the adsorbent was weighed and mixed with 25 mL of brine in a conical flask. The mixture was adsorbed at room temperature for 6 h. The adsorption capacity of lithium ions was 4.28 mg / (g kaolinite). After 5 cycles of adsorption-desorption, the adsorbent adsorbed 3.62 mg / (g kaolinite).
[0084] The SEM images of the kaolinite raw material and the adsorbent in Example 3 of the present invention are shown in Figure 1a to Figure 1b , the XRD pattern of the adsorbent is shown in Figure 2 . Figure 1a The raw material of kaolinite presents a stacked flake structure with a smooth surface. Figure 1b It can be seen that there is no obvious kaolinite lamellar structure, and spherical particles and irregular nanosheets appear in the sample. In addition, a large number of nanosheets are attached to the surface of the spherical particles. The spherical particles are chemically grafted SiO2, and the nanosheets are LiCl·2Al(OH)3·nH2O.
[0085] Figure 2 The XRD spectrum shows obvious diffraction peaks of LiCl·2Al(OH)3·nH2O, indicating that LiCl·2Al(OH)3·nH2O exists in the adsorbent. It can be seen that the method of the present invention can transform kaolinite and prepare a lithium ion adsorption material composited with grafted SiO2 and LiCl·2Al(OH)3·nH2O.
[0086] Comparative Example 1
[0087] The specific method is the same as that in Example 3, except that only steps 1 to 3 are performed, and the grafting reactions of steps 4 and 6 are not performed. The prepared adsorbent is used for adsorbing lithium ions in brine. The adsorbent prepared in this way has an adsorption capacity of 2.84 mg / (g kaolinite) for lithium ions.
[0088] Comparative Example 2
[0089] The specific method is the same as that in Example 3, except that NaOH in step 2 is replaced by Na2CO3, and other conditions remain unchanged. The prepared adsorbent is used for adsorption of lithium ions in brine. The adsorbent prepared in this way has an adsorption capacity of 0.92 mg / g for lithium ions.
[0090] Comparative Example 3
[0091] The specific method is the same as that of Example 3, except that the process in step 3 is changed to not adjusting the pH to 1.0 first, but directly adding LiCl. After sufficient dissolution, the pH is adjusted to 4.0 and then reacted. The prepared adsorbent is used for adsorption of lithium ions in brine. The adsorbent prepared in this way has an adsorption capacity of 3.12 mg / g for lithium ions.
[0092] Comparative Example 4
[0093] The specific method is the same as that in Example 3, except that the concentration of NaOH in step 2 is adjusted to 40 g / L while the other conditions remain unchanged. The prepared adsorbent is used for adsorption of lithium ions in brine. The adsorbent prepared in this way has an adsorption capacity of 1.70 mg / g for lithium ions.
[0094] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for preparing a kaolinite-based lithium ion adsorbent, characterized in that: The crushed natural kaolinite is activated, alkali-dissolved, acid-converted and surface-grafted in sequence to obtain a kaolinite-based lithium ion adsorbent; The preparation method comprises the following steps: Step 1: crushing natural kaolinite to obtain kaolinite powder, calcining and cooling the kaolinite powder to obtain activated kaolinite powder; Step 2: Evenly mix the activated kaolinite powder and the NaOH solution, stir to perform an alkali dissolution reaction, and cool and filter to obtain a filtrate; Step 3: Add HCl solution dropwise to the filtrate to adjust the pH to 1-2, and stir to carry out acid conversion reaction; Then, LiCl was added to the system to fully dissolve, and the pH was adjusted to 4-5 with NaOH solution, and the reaction was continued by stirring. The reaction product was filtered and dried to obtain a solid phase; Step 4: mixing the solid phase with the silane coupling agent and the organic solvent, reacting at 115-125° C. for 20-28 hours, filtering and drying the reaction product to obtain a first powder product; Step 5: After mixing the first powder product with the chloroacetic acid solution, adding a NaOH solution to adjust the pH to 8-8.5 for reaction, filtering and drying the reaction product to obtain a second powder product; Step 6: dissolving 2-hydroxyethyl sulfonic acid and NaOH in an organic solvent, mixing the mixture with the second powder product and then subjecting the mixture to reflux reaction, filtering the reaction product, washing it to neutrality, and drying it to obtain a kaolinite-based lithium ion adsorbent; In the step 2, the mass volume ratio of the activated kaolinite powder to the NaOH solution is 45-55:220-260 g / mL, and the concentration of NaOH is 80-160 g / L.
2. The method for preparing a kaolinite-based lithium ion adsorbent according to claim 1, characterized in that: In the step 1, the calcination temperature is 550-650° C., and the calcination time is 1-3 hours.
3. The method for preparing a kaolinite-based lithium ion adsorbent according to claim 1, characterized in that: In the step 2, the alkali dissolution reaction temperature is 110-125° C., and the alkali dissolution reaction time is 6-12 hours.
4. The method for preparing a kaolinite-based lithium ion adsorbent according to claim 1, characterized in that: In the step 1, the particle size of the kaolinite powder is 160-200 meshes.
5. The method for preparing a kaolinite-based lithium ion adsorbent according to claim 1, characterized in that: The mass ratio of the activated kaolinite powder to LiCl is 8-12:
1.
6. The method for preparing a kaolinite-based lithium ion adsorbent according to claim 1, characterized in that: In step 4, the organic solvent is toluene, the mass volume ratio of the activated kaolinite powder and the silane coupling agent is 45-55:5-10 g / mL, and the mass volume ratio of the activated kaolinite powder and toluene is 45-55:220-260 g / mL.
7. The method for preparing a kaolinite-based lithium ion adsorbent according to claim 1, characterized in that: The mass volume ratio of the activated kaolinite powder to the chloroacetic acid solution is 45-55:220-260 g / mL, and the concentration of the chloroacetic acid solution is 0.5-1 g / L.
8. The method for preparing a kaolinite-based lithium ion adsorbent according to claim 1, characterized in that: In step 6, the organic solvent is ethanol, the mass ratio of 2-hydroxyethyl sulfonic acid to NaOH is 1-3:0.5-1, and the mass volume ratio of 2-hydroxyethyl sulfonic acid to ethanol is 1-3:220-260 g / mL.
Citation Information
Patent Citations
Hierarchical pore structure silicon-based negative electrode material for lithium battery and preparation method of hierarchical pore structure silicon-based negative electrode material
CN104577049A
Heavy metal ion adsorbent and preparation method and application thereof
CN106076279A