A cobalt carbide-based catalyst containing an electronic auxiliary agent and having a specific exposed crystal face, and a preparation method and application thereof

By combining rare earth metal salts and main group/transition metal salts, a cobalt carbide catalyst with specific exposed crystal surfaces is prepared, which solves the problem of uncontrollable exposure crystal surface synthesis of cobalt carbide catalysts in the prior art and improves the selection of catalysts and conversion rate, suitable for Fischer Tropsch synthesis reaction.

CN118341460BActive Publication Date: 2024-11-22ZHEJIANG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410782971.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-22
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

In the prior art, the exposed crystal surface synthesis of cobalt carbide-based catalysts under the conditions of electronic additives is uncontrollable, which affects the selectivity and conversion rate of the catalyst.

Method used

Using rare earth metal salt as crystal surface stabilizer, combining main group metal and transition metal salt as electronic additives, cobalt carbide-based catalyst with specific exposed crystal surfaces is prepared by precipitation method and carbonization step, reducing step is omitted, and carbonization is directly carbonized to form ( 101) and (020) surfaces exposed Co2C nanoprismatic structure.

Benefits of technology

The specific exposed crystal surface of the controllable synthesis of cobalt carbide catalyst under mild conditions is achieved, which improves the selectivity of olefins, reduces the selectivity of methane, and increases the conversion rate and catalyst activity of Fischer-Tropsch synthesis reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118341460B_ABST
    Figure CN118341460B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of catalyst preparation, and discloses a cobalt carbide-based catalyst containing an electronic auxiliary agent and having a specific exposed crystal face, as well as a preparation method and application thereof. The preparation method of the cobalt carbide-based catalyst containing an electronic auxiliary agent comprises the following steps: 1) mixing and dissolving a cobalt salt, a crystal face stabilizer, an electronic auxiliary agent and a solvent to obtain a salt solution; 2) mixing and dissolving an alkaline precipitant and a solvent to obtain an alkaline solution; 3) precipitating the salt solution and the alkaline solution by a precipitation method, separating, drying and calcining in an air atmosphere after precipitation; 4) directly carbonizing the calcined product without reducing it to generate a cobalt carbide-based catalyst containing an electronic auxiliary agent and having a specific exposed crystal face. The invention provides the application of the cobalt carbide-based catalyst containing an electronic auxiliary agent in Fischer-Tropsch synthesis. The invention solves the problem of uncontrollable synthesis of exposed crystal faces of cobalt carbide-based catalysts under conditions containing electronic auxiliary agents, and the prepared catalyst has good selectivity and high conversion rate in the Fischer-Tropsch synthesis reaction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of catalyst preparation, and in particular to a cobalt carbide-based catalyst containing an electronic auxiliary agent and having a specific exposed crystal face, and a preparation method and application thereof. Background Art

[0002] Nowadays, C1 chemistry is developing rapidly. The direct conversion of syngas (Syngas, a mixture of H2 and CO) into high value-added products through the Fischer-Tropsch synthesis reaction has attracted great attention. The raw material syngas can be obtained from coal, natural gas, biomass, waste, etc. through gasification reaction. It is a green chemical production process with recyclable carbon resources. The Fischer-Tropsch reaction process is complicated and the product types are diverse. Its complete reaction mechanism has not been established, but it is generally believed to be a surface polymerization reaction. According to the surface polymerization reaction mechanism, the distribution of Fischer-Tropsch synthesis reaction products obeys the Anderson-Schulz-Flory (ASF) product distribution model. This distribution model can predict the selectivity of hydrocarbon products based on the number of carbon atoms in the product molecules. With high added value polyethylene comonomer C 4-8 For example, linear α-olefins have a chain growth factor of about 0.69. 4-8 The selectivity of hydrocarbons can reach up to 46%, the selectivity of methane is about 10%, and the selectivity of other hydrocarbons is about 44%. Therefore, for the Fischer-Tropsch synthesis reaction, how to maintain high activity under mild conditions while breaking through the limitations of the product distribution ASF model, improving the selectivity of the target carbon number product, and reducing the selectivity of methane and non-target products is the biggest research difficulty.

[0003] Fischer-Tropsch synthesis is a structure-sensitive reaction, and its performance is affected by the surface structure of the catalyst, which in turn is determined by the particle size of the active phase and the exposed crystal faces.

[0004] In the previous work, the inventor has authorized a patent on cobalt carbide-based catalysts ("A cobalt carbide-based catalyst for direct preparation of olefins from synthesis gas and its preparation method and application", authorization announcement number: CN105772049B), which discloses a method for preparing a cobalt carbide-based catalyst, including the following steps: 1) mixing a cobalt source with water or a cobalt source, an electronic auxiliary agent with water to obtain a first solution; mixing a precipitant with water to obtain a second solution; 2) adding the first solution and the second solution to water or water and a structural auxiliary agent for precipitation, crystallization, separation, drying, and roasting; 3) reducing the solid obtained in step 2) in a reducing atmosphere, and then carbonizing it in a carbonizing atmosphere. In this patent, electronic auxiliary agents are added to regulate the reaction performance, and their role is mainly electronic effect, which changes the electronic properties of the active phase of cobalt carbide, but cannot stabilize the specific crystal plane of cobalt carbide and cause it to expose the dominant crystal plane, so its active phase cobalt carbide has a spherical morphology.

[0005] In 2016, Zhong Liangshu et al. (Nature, 2016, 538, 84-87) found that prismatic Co2C exposes specific low-index crystal faces, and its (101) face has the function of promoting C 2-4 The (101) and (020) planes both have the effect of inhibiting the formation of CH4. They have extremely excellent FTO reaction performance under mild reaction conditions, and the product distribution breaks through the limitations of the traditional ASF model. The inventors further disclosed a method for preparing a cobalt carbide catalyst in a paper published in 2021 [Zhengjia Li, etc. Formation Mechanism of the Co2C Nanoprisms Studied with the CoCe System in the Fischer−Tropsch to OleinReaction. ACS Catal. 2021, 11, 2746−2753]: Co(NO3)2·6H2O and Ce(NO3)3·6H2O are added to water to form a mixed salt solution (2 mol Co / L). Ammonium carbonate was dissolved in water to form a 2 mol / L alkaline solution. The two solutions were simultaneously added dropwise into a beaker containing 100 mL of water and stirred vigorously (600 rpm). The pH value was maintained at 8.0±0.1 and the precipitation temperature was maintained at 30±1 ℃. After the co-precipitation was completed, it was aged at 30 ℃ for 2 h, washed and filtered, dried at 80 ℃, and calcined at 330 ℃ for 5 h; the catalyst was heated to 300 ℃ at a rate of 1 ℃ / min and heated in a 10 % (v / v) H2 / Ar atmosphere (12,000 mL / (h ·g cat )) was reduced at 300 °C for 5 h, cooled to 250 °C in Ar, and then introduced into the synthesis gas for Fischer-Tropsch synthesis reaction. This study shows that by omitting the carbonization step and controlling the amount of Ce added on the basis of the technical solution of CN105772049B, a Co2C nanoprism structure with specific exposed crystal faces can be synthesized, which can reduce the selectivity of methane and alkanes and improve the selectivity of olefins and the olefin-alkane ratio. In this study, the formation of the exposed crystal faces of the Co2C nanoprism structure is strongly related to the compensatory coordination effect of Ce, and Ce2O3 no longer acts as an electron auxiliary agent, but as a crystal face stabilizer.

[0006] The selectivity of the catalyst is not only related to the surface structure of the active phase, but also closely related to the composition of the catalyst. Generally, the electronic properties of the active center can be adjusted by adjusting the type and content of the electronic additive, thereby regulating the product selectivity. For prismatic Co2C-based catalysts, the research on additives mainly focuses on the role of alkali metals, alkaline earth metals, Mn and Ce in the formation of exposed crystal faces of Co2C, and there are few reports on research on electronic additives. The inventors' previous work showed that further adding Zn electronic additives to the technical scheme for synthesizing Co2C nanoprisms disclosed in the paper [ZhengjiaLi, etc. Formation Mechanism of the Co2C Nanoprisms Studied with the CoCeSystem in the Fischer−Tropsch to Olein Reaction. ACS Catal. 2021, 11, 2746−2753] did not result in a cobalt carbide-based catalyst with a specific exposed crystal face, as shown in Comparative Example 2. This is because the active phase Co2C is thermodynamically metastable under hydrogen conditions in FTO. The addition of electronic additives will cause the surface energy of its exposed crystal surface to change, the anisotropy of the growth rate to decrease, and finally spherical Co2C to be generated.

[0007] Therefore, in the existing synthesis technology, there is a common problem that the exposed crystal face synthesis of Co2C-based catalysts containing electronic additives is uncontrollable. Therefore, it is necessary to develop a new method for the controllable synthesis of the exposed crystal face of Co2C-based catalysts. Summary of the invention

[0008] The primary technical problem to be solved by the present invention is the problem of uncontrollable synthesis of exposed crystal faces of cobalt carbide-based catalysts under the conditions of containing electronic additives in the prior art. A method for preparing a cobalt carbide-based catalyst with specific exposed crystal faces containing electronic additives is provided, and the preparation method is simple and quick.

[0009] The second technical problem to be solved by the present invention is to provide a cobalt carbide-based catalyst containing an electron auxiliary agent and having a specific exposed crystal face.

[0010] The third technical problem to be solved by the present invention is to provide the application of the cobalt carbide-based catalyst with specific exposed crystal faces containing an electronic auxiliary agent in Fischer-Tropsch synthesis. The prepared catalyst has good selectivity and high conversion rate.

[0011] In order to solve the above technical problems, the technical solution adopted by the present invention is as follows:

[0012] In a first aspect, the present invention provides a method for preparing a cobalt carbide-based catalyst having a specific exposed crystal face and containing an electron auxiliary agent, comprising the following steps:

[0013] 1) Mixing and dissolving a cobalt salt, a crystal surface stabilizer, an electronic auxiliary agent and a solvent to obtain a salt solution; the crystal surface stabilizer is one or more rare earth metal salts, and the rare earth metal is one or more of lanthanide metals, scandium and yttrium; the electronic auxiliary agent is one or more of main group metal salts and transition metal salts; wherein the molar ratio of cobalt salt: crystal surface stabilizer: electronic auxiliary agent is 1:0.01-3:0.0001-10, and the molar amount of the cobalt salt is calculated based on the molar amount of Co atoms;

[0014] 2) mixing and dissolving an alkaline precipitant and a solvent to obtain an alkaline solution;

[0015] 3) precipitating the salt solution of step 1) and the alkaline solution of step 2) by a precipitation method, and then crystallizing, separating, drying, and calcining in an air atmosphere after precipitation, or directly separating, drying, and calcining in an air atmosphere without crystallization after precipitation;

[0016] 4) The calcined product obtained in step 3) is directly carbonized without reduction (the reduction refers to the high-temperature reduction step commonly used in the existing cobalt carbide-based catalyst preparation method in a reducing atmosphere (such as hydrogen or a mixture of hydrogen and an inert gas)) to generate a cobalt carbide-based catalyst containing an electron auxiliary agent and having specific exposed crystal faces, wherein the specific exposed crystal faces refer to (101) and / or (020) faces.

[0017] Preferably, the preparation method further comprises: loading the calcined product obtained in step 3) with an alkali metal auxiliary agent by an impregnation method, drying, and then calcining in an air atmosphere to perform the operation of step 4). The alkali metal auxiliary agent may be one or more of the alkali metal bases and alkali metal salts known in the art. The alkali metal base may be lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, and cesium hydroxide. The alkali metal salt may be one or more of an inorganic alkali metal salt and an organic alkali metal salt, such as an inorganic alkali metal salt such as lithium nitrate, lithium carbonate, lithium sulfate, sodium nitrate, sodium carbonate, potassium nitrate, rubidium nitrate, and cesium nitrate, such as an organic alkali metal salt such as lithium acetate, sodium acetate, potassium acetate, and sodium citrate. The molar ratio of the cobalt salt to the alkali metal auxiliary agent is controlled to be 1:0.0001-5, more preferably 1:0.0001-0.8, such as 1:0.01 or 1:0.04, wherein the molar amount of the cobalt salt is based on the molar amount of Co atoms. The drying conditions are as follows: the drying temperature is 0-200°C, more preferably 60-120°C; the drying time is 1-24 hours, more preferably 4-12 hours. The roasting conditions are as follows: the roasting temperature is 200-800°C, more preferably 300-500°C; the roasting time is 1-36 hours, more preferably 2-8 hours.

[0018] In the above technical solution, the cobalt salt can be one or more of various available organic cobalt salts and inorganic cobalt salts known in the art. The organic cobalt salt can be one or more of organic cobalt sources such as cobalt formate and cobalt acetate; the inorganic cobalt salt can be one or more of inorganic cobalt sources such as cobalt nitrate, cobalt chloride, and cobalt sulfate. More preferably, the cobalt salt is cobalt nitrate and / or cobalt acetate.

[0019] In the above technical solution, the crystal plane stabilizer can be one or more rare earth metal salts known in the art, and the metal element in the rare earth metal salt can be one or more of lanthanide metals, scandium and yttrium, and more preferably the metal element is one or both of lanthanum and cerium.

[0020] In the above technical solution, the electronic auxiliary agent can be one or more of the main group metal salts and transition metal salts known in the art, preferably one or more of the salts of metals such as magnesium, calcium, vanadium, chromium, manganese, gallium, and indium.

[0021] In the above technical solution, the solvent can be one or more of water and organic solvents known in the art. The organic solvent can be one or more of formaldehyde, ethanol, toluene, tetrahydrofuran and other organic solvents.

[0022] In the above technical solution, the alkaline precipitant may be one or more of the alkalis and alkaline salts known in the art. The alkali may be one or more of lithium hydroxide, sodium hydroxide, potassium hydroxide, ammonia water and the like; the alkaline salt may be one or more of sodium carbonate, ammonium carbonate, sodium bicarbonate, potassium carbonate and the like. More preferably, it is one or more of sodium hydroxide, sodium carbonate and ammonium carbonate.

[0023] In the above technical scheme, in step 1), the molar ratio of the cobalt salt to the crystal surface stabilizer, the electronic auxiliary agent, and the solvent is 1:0.01~3:0.0001~10:10~2000, more preferably 1:0.01~1:0.01~2:10~500, such as 1:0.05:0.05:20, 1:0.03:0.1:65 or 1:0.1:1:100, wherein the molar amount of the cobalt salt is based on the molar amount of Co atoms therein.

[0024] In the above technical solution, in step 2), calculated based on the alkaline precipitant, the molar ratio of the alkaline precipitant to the solvent is 1:10-1500, more preferably 1:10-200, such as 1:25, 1:50 or 1:100.

[0025] In the above technical scheme, in step 3), the precipitation method can be a forward / reverse single drop precipitation method or a double drop co-precipitation method known in the art. The forward / reverse single drop precipitation method refers to adding one of the alkaline solution and the salt solution dropwise into the other solution at a certain temperature and pH value, and the double drop co-precipitation method refers to adding the alkaline solution and the salt solution dropwise into a certain solvent (such as deionized water, ethanol, etc.) at a certain temperature and pH value.

[0026] In the above technical solution, in step 3), the precipitation temperature is 0~120°C, more preferably 20~60°C, such as 20~25°C, 25~30°C or 30~35°C; the precipitation pH value is controlled at 7~12, more preferably 7~9, such as 7~7.5, 7.5~8 or 8~8.5.

[0027] In the above technical solution, in step 3), the crystallization temperature is 0~200°C, more preferably 20~100°C, such as 20~30°C, 30~40°C or 40~50°C; the crystallization time is 0~48 hours, more preferably 0~24 hours, such as 0~4 hours, 4~8 hours or 8~12 hours.

[0028] In the above technical solution, in step 3), the drying temperature is 0-200°C, more preferably 40-120°C, such as 40-60°C, 60-80°C or 80-100°C; the drying time is 1-24 hours, more preferably 4-16 hours, such as 4-8 hours, 8-12 hours or 12-16 hours.

[0029] In the above technical solution, in step 3), the calcination temperature is 200-800°C, more preferably 300-600°C, such as 300-350°C, 350-400°C or 400-450°C; the calcination time is 1-36 hours, more preferably 2-12 hours, such as 2-4 hours, 4-6 hours or 6-8 hours.

[0030] In the above technical solution, in step 4), the carbonization atmosphere can be one or more carbonization gases known in the art, preferably carbonization gas A, a mixed gas of carbonization gas A and hydrogen, or a mixed gas of carbonization gas A and an inert gas, wherein the carbonization gas A is selected from one or more of carbon monoxide, carbon monoxide, methane, ethane, and ethylene, and the volume percentage of hydrogen in the mixed gas of carbonization gas A and hydrogen is not higher than 80%. More preferably, the carbonization atmosphere is a mixed gas of carbon monoxide and argon, such as a 10% carbon monoxide-argon mixed gas.

[0031] In the above technical solution, in step 4), the carbonization conditions are: carbonization temperature is 100-600 °C, more preferably 300-500 °C, carbonization pressure is 0.1-10 MPa, more preferably 0.1-1 MPa, volume space velocity is 500-100000 h -1 , preferably 2000~10000 h -1 , the carbonization time is no more than 24 hours, more preferably 1 to 12 hours; such as: the carbonization temperature is 100 to 250°C, 250 to 300°C, 300 to 400°C, 400 to 500°C or 500 to 600°C; the carbonization pressure is 0.1 to 0.7 MPa, 0.7 to 0.8 MPa, 0.8 to 1 MPa, 1 to 2 MPa, 2 to 3 MPa, 3 to 5 MPa, 5 to 6 MPa, 6 to 7 MPa, 7 to 8 MPa or 8 to 10 MPa; the volume space velocity is 500 to 2000 h -1 , 2000~4000 h -1 , 4000~5000 h -1 , 5000~8000 h -1 , 8000~10000h -1 ; The carbonization time is 1 to 4 hours, 4 to 5 hours, 5 to 8 hours, 8 to 12 hours or 12 to 24 hours.

[0032] In a second aspect, the present invention provides a cobalt carbide-based catalyst having a specific exposed crystal face and containing an electronic auxiliary agent, which is prepared according to the preparation method described in the first aspect.

[0033] In a third aspect, the present invention provides the use of the cobalt carbide-based catalyst with specific exposed crystal faces containing an electronic auxiliary agent as described in the second aspect in Fischer-Tropsch synthesis.

[0034] In the above technical scheme, the Fischer-Tropsch synthesis reaction conditions are: reaction temperature is 150-500 °C, preferably 200-300 °C, reaction pressure is 0.1-10 MPa, preferably 0.1-1 MPa, volume space velocity is 500-100000 h -1 , preferably 1000~40000 h -1 , the molar ratio of H2 to CO is 1:10-10:1, preferably 1:3-3:1; such as: the reaction temperature is 150-200°C, 200-230°C, 230-240°C, 240-250°C, 250-260°C, 260-270°C, 270-300°C or 300-500°C; the reaction pressure is 0.1-0.5 MPa, 0.5-1 MPa or 1-10 MPa; the volume space velocity is 500-1000 h -1 1000~2000h -1, 2000~4000 h -1 or 4000~100000 h -1 ; The molar ratio of H2 to CO is 1:10~1:3, 1:3~2:1, 2:1~3:1 or 3:1~10:1.

[0035] In the above technical solution, the Fischer-Tropsch synthesis reaction is carried out in a fixed bed, a slurry bed or a fluidized bed, more preferably a fixed bed or a slurry bed.

[0036] Compared with the prior art, the present invention has the following beneficial effects:

[0037] The present invention uses a crystal plane stabilizer to compensate for the dangling bonds on the surface of the coordinated cobalt species, reduces the surface energy, and coordinates the step design of carbonization without reduction to promote the exposure of the dominant crystal plane under the condition of an electron auxiliary agent, and can controllably synthesize cobalt carbide with specific exposed crystal planes. The cobalt carbide mainly presents a prismatic morphology, is more conducive to the generation of olefin products, and reduces the selectivity of methane by-products. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 2 is the XRD diagram of the cobalt carbide-based catalyst obtained in Example 1 and Comparative Examples 1 and 2. It can be seen that the active center of the cobalt carbide-based catalyst is Co2C.

[0039] Figure 2 a, b, c, d, e and f are TEM images of the cobalt carbide-based catalysts obtained in Example 1, Comparative Example 1, Comparative Example 2, Example 2, Example 3 and Example 17, respectively. DETAILED DESCRIPTION

[0040] The technical solution of the present invention is described below through specific examples. It should be understood that the one or more method steps mentioned in the present invention do not exclude the existence of other method steps before and after the combination step or the insertion of other method steps between these explicitly mentioned steps; it should also be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to limit the scope of the present invention. The change or adjustment of the relative relationship thereof shall also be regarded as the scope of the present invention without substantially changing the technical content.

[0041] The technical details of the present invention are described in detail by the following examples. It should be noted that the examples are only used to further illustrate the technical features of the present invention, rather than to limit the present invention.

[0042] [Example 1]

[0043] The salt solution was obtained by stirring and dissolving the cobalt acetate: cerium nitrate: zinc nitrate: water at a molar ratio of 1:1:0.05:25. The alkaline solution was obtained by stirring and dissolving the sodium carbonate: water at a molar ratio of 1:25. The catalyst was prepared by double drop coprecipitation method, the precipitation temperature was 40 °C, the pH value was controlled at 7.5, a certain amount of deionized water was prepared according to the mass ratio of cobalt: water = 1:25, and the salt solution and the alkaline solution were added dropwise to the deionized water at the same time. After the addition was completed, crystallization was carried out at a temperature of 60 °C for 2 hours, centrifuged, and the obtained solid product was dried at 100 °C in an oven for 4 hours, and the dried solid was calcined at 350 °C in a muffle furnace for 6 hours. Carbonization was carried out in a tubular furnace, at 250 °C, 0.1 MPa, for 4 hours in a 10% CO / Ar mixed atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction temperature was 260 ℃, the pressure was 0.1 MPa, and the space velocity was 2000 h -1 The XRD and TEM characterization results of its cobalt carbide-based catalyst showed that Co2C nanostructures with specific exposed crystal faces were successfully synthesized under the conditions of electron-assisted agents, such as Figure 1 and Figure 2 As shown in a.

[0044] [Example 2]

[0045] The salt solution was obtained by stirring and dissolving the cobalt nitrate: cerium nitrate: manganese nitrate: water at a molar ratio of 1:0.1:2:30. The alkaline solution was obtained by stirring and dissolving the ammonium carbonate: water at a molar ratio of 1:30. The catalyst was prepared by double-drop coprecipitation method, the precipitation temperature was 30 °C, the pH value was controlled at 8, a certain amount of deionized water was prepared according to the mass ratio of cobalt: water = 1:60, and the salt solution and the alkaline solution were added dropwise to the deionized water at the same time. After the addition was completed, crystallization was carried out at a temperature of 30 °C for 4 hours, filtration was performed, and the obtained solid product was dried at 80 °C in an oven for 10 hours, and the dried solid was calcined at 400 °C in a muffle furnace for 3 hours. Carbonization was carried out in a tubular furnace at 300 °C, 1 MPa, carbonization for 5 hours in a 10% CH4 / Ar atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=1 was used as the raw gas, the reaction temperature was 260 ℃, the pressure was 0.1 MPa, and the space velocity was 2000 h -1 TEM characterization results of its cobalt carbide-based catalyst showed that it was successful in controlling the synthesis of Co2C nanostructures with specific exposed crystal faces under the conditions of electron-assisted agents, such as Figure 2 As shown in d.

[0046] [Example 3]

[0047] The salt solution was obtained by stirring and dissolving the cobalt acetate: cerium nitrate: magnesium carbonate: water at a molar ratio of 1:0.1:0.5:80. The alkaline solution was obtained by stirring and dissolving the potassium hydroxide: water at a molar ratio of 1:500. The catalyst was prepared by a single drop precipitation method, the precipitation temperature was 60 °C, the salt solution was added dropwise to the alkaline solution, and the final pH value was controlled at 8. After the addition was completed, crystallization was carried out at a temperature of 180 °C for 2 hours, centrifuged, and the obtained solid product was dried in an oven at 80 °C for 12 hours, and the dried solid was calcined in a muffle furnace at 500 °C for 4 hours. Carbonization was carried out in a tubular furnace at 250 °C, 10 MPa, for 4 hours in a CO atmosphere, and the space velocity was 10000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=0.5 was used as the raw gas, the reaction was carried out at 240 ℃, 0.1 MPa, and the space velocity was 2000 h -1 TEM characterization results of its cobalt carbide-based catalyst showed that it was successful in controlling the synthesis of Co2C nanostructures with specific exposed crystal faces under the conditions of electron-assisted agents, such as Figure 2 As shown in e.

[0048] [Example 4]

[0049] The salt solution was obtained by stirring and dissolving the cobalt chloride: cerium acetate: manganese acetate: water at a molar ratio of 1:0.2:0.5:50. The alkaline solution was obtained by stirring and dissolving the sodium carbonate: water at a molar ratio of 1:200. The catalyst was prepared by a single drop precipitation method, the precipitation temperature was 60 °C, the alkaline solution was added dropwise to the salt solution, and the final pH value was controlled at 8. After the addition was completed, crystallization was carried out at a temperature of 60 °C for 2 hours, centrifuged, and the obtained solid product was dried in an oven at 80 °C for 12 hours, and the dried solid was calcined in a muffle furnace at 330 °C for 4 hours. Carbonization was carried out in a tubular furnace at 250 °C, 0.1 MPa, for 4 hours in a pure CH4 atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=1:3 was used as the raw gas, the reaction was carried out at 240 ℃, 0.1 MPa, and the space velocity was 2000 h -1 .

[0050] [Example 5]

[0051] The salt solution was obtained by stirring and dissolving the cobalt nitrate: praseodymium nitrate: vanadium nitrate: water at a molar ratio of 1:0.01:2:25. The alkaline solution was obtained by stirring and dissolving the potassium hydroxide: water at a molar ratio of 1:15. The catalyst was prepared by a single drop precipitation method, the precipitation temperature was 80 °C, the salt solution was added dropwise to the alkaline solution, and the final pH value was controlled at 8.5. After the addition was completed, crystallization was carried out at a temperature of 60 °C for 12 hours, centrifuged, and the obtained solid product was dried in an oven at 80 °C for 12 hours, and the dried solid was calcined in a muffle furnace at 330 °C for 4 hours. Carbonization was carried out in a tubular furnace at 250 °C, 0.1 MPa, for 4 hours in a 15% CH4 / N2 atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=3 was used as the raw gas, the reaction temperature was 240 ℃, the pressure was 0.1 MPa, and the space velocity was 2000 h -1 .

[0052] [Example 6]

[0053] The salt solution was obtained by stirring and dissolving the cobalt nitrate: scandium nitrate: silver nitrate: water at a molar ratio of 1:0.3:4:50. The alkaline solution was obtained by stirring and dissolving the sodium hydroxide: water at a molar ratio of 1:75. The catalyst was prepared by double-drop coprecipitation method, the precipitation temperature was 55 °C, the pH value was controlled at 9, a certain amount of deionized water was prepared according to the mass ratio of cobalt: water = 1:50, and the salt solution and the alkaline solution were simultaneously added dropwise to the deionized water. After the addition was completed, crystallization was carried out at a temperature of 40 °C for 8 hours, filtration and separation were carried out, and the obtained solid product was dried at 120 °C in an oven for 8 hours, and the dried solid was calcined at 400 °C in a muffle furnace for 5 hours. Carbonization was carried out in a tubular furnace, at 250 °C, 5 MPa, for 4 hours in a pure C2H4 atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction temperature was 250 ℃, the pressure was 0.1 MPa, and the space velocity was 40000 h -1 .

[0054] [Example 7]

[0055] The salt solution was obtained by stirring and dissolving the cobalt nitrate: cerium nitrate: chromium sulfate: ethanol at a molar ratio of 1:0.02:0.5:50. The alkaline solution was obtained by stirring and dissolving the ammonium carbonate: water at a molar ratio of 1:100. The catalyst was prepared by double-drop coprecipitation method, the precipitation temperature was 30 °C, the pH value was controlled at 8, a certain amount of anhydrous ethanol was prepared according to the mass ratio of cobalt: ethanol = 1:100, and the salt solution and the alkaline solution were added dropwise to the anhydrous ethanol at the same time. After the addition was completed, crystallization was carried out at a temperature of 60 °C for 2 hours, centrifuged, and the obtained solid product was dried in an oven at 80 °C for 12 hours, and the dried solid was calcined at 330 °C in a muffle furnace for 5 hours. Carbonization was carried out in a tubular furnace at 250 °C, 1 MPa, carbonization for 4 hours in a pure CH4 atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction was carried out at 230 ℃, 0.1 MPa, and the space velocity was 500 h -1 .

[0056] [Example 8]

[0057] The salt solution was obtained by stirring and dissolving the cobalt sulfate: cerium nitrate: indium nitrate: ethanol at a molar ratio of 1:1:0.5:50. The alkaline solution was obtained by stirring and dissolving the sodium bicarbonate: water at a molar ratio of 1:50. The catalyst was prepared by double drop coprecipitation method, the precipitation temperature was 80 °C, the pH value was controlled at 9, a certain amount of deionized water was prepared according to the mass ratio of cobalt: water = 1:80, and the salt solution and the alkaline solution were added dropwise to the deionized water at the same time. After the addition was completed, crystallization was carried out at a temperature of 60 °C for 2 hours, centrifuged, and the obtained solid product was dried in an oven at 80 °C for 12 hours, and the dried solid was calcined in a muffle furnace at 330 °C for 5 hours. Carbonization was carried out in a tubular furnace, at 250 °C, 0.1 MPa, for 4 hours in a pure C2H6 atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction temperature was 250 ℃, the pressure was 0.1 MPa, and the space velocity was 1000 h -1 .

[0058] [Example 9]

[0059] The salt solution was obtained by stirring and dissolving the cobalt nitrate: lanthanum acetate: lead nitrate: water at a molar ratio of 1:0.05:2:125. The alkaline solution was obtained by stirring and dissolving the ammonia water: ammonium carbonate: water at a molar ratio of 1:1:150. The catalyst was prepared by double drop coprecipitation method. The precipitation temperature was 20 °C, the pH value was controlled at 7.5, a certain amount of deionized water was prepared according to the mass ratio of cobalt: water = 1:10, and the salt solution and the alkaline solution were added to the deionized water at the same time. After the addition was completed, the product was crystallized at 60 °C for 4 hours, centrifuged, and the solid product was dried at 80 °C in an oven for 10 hours, and the dried solid was calcined at 330 °C in a muffle furnace for 3 hours. The calcined solid was impregnated with an equal volume of cobalt: lithium hydroxide at a molar ratio of 1:0.1, dried at 100 °C for 12 hours, and the dried solid was calcined at 300 °C for 6 hours. Carbonization was carried out in a tube furnace at 500 °C, 1 MPa, for 5 h in a 10% CH4 / Ar atmosphere with a space velocity of 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction temperature was 270 ℃, the pressure was 0.1 MPa, and the space velocity was 100000 h -1 .

[0060] [Example 10]

[0061] The salt solution was obtained by stirring and dissolving cobalt acetate: cerium nitrate: zinc acetate: ethanol at a molar ratio of 1:1:0.3:25. The alkaline solution was obtained by stirring and dissolving sodium bicarbonate: water at a molar ratio of 1:100. The catalyst was prepared by a single drop precipitation method, the precipitation temperature was 30 °C, the salt solution was added dropwise to the alkaline solution, and the final pH value was controlled at 8. After the addition was completed, crystallization was carried out at a temperature of 60 °C for 4 hours, centrifuged, and the obtained solid product was dried in an oven at 80 °C for 10 hours, and the dried solid was calcined at 330 °C in a muffle furnace for 4 hours. Carbonization was carried out in a tubular furnace at 300 °C, 3 MPa, for 5 hours in a 10% CO / Ar atmosphere, and the space velocity was 500 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction was carried out at 260 ℃, 10 MPa, and the space velocity was 2000 h -1 .

[0062] [Example 11]

[0063] The salt solution was obtained by stirring and dissolving the cobalt nitrate: lanthanum nitrate: ammonium metavanadate: water at a molar ratio of 1:1:0.1:1000. The alkaline solution was obtained by stirring and dissolving the sodium carbonate: water at a molar ratio of 1:1000. The catalyst was prepared by a single drop precipitation method, the precipitation temperature was 20 °C, the alkaline solution was added dropwise to the salt solution, and the final pH value was controlled at 8. After the addition was completed, crystallization was carried out at a temperature of 60 °C for 2 hours, centrifuged, and the obtained solid product was dried in an oven at 80 °C for 10 hours, and the dried solid was calcined in a muffle furnace at 330 °C for 4 hours. Carbonization was carried out in a tubular furnace at 300 °C, 8 MPa, for 1 hour in a 10% C2H4 / Ar atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction temperature was 150 ℃, the pressure was 0.1 MPa, and the space velocity was 2000 h -1 .

[0064] [Example 12]

[0065] The salt solution was obtained by stirring and dissolving the cobalt nitrate: cerium nitrate: potassium chromate: water at a molar ratio of 1:0.01:0.3:15. The alkaline solution was obtained by stirring and dissolving the sodium carbonate: water at a molar ratio of 1:10. The catalyst was prepared by double drop coprecipitation method, the precipitation temperature was 30 °C, the pH value was controlled at 8, a certain amount of deionized water was prepared according to the mass ratio of cobalt: water = 1:20, and the two solutions were added to the deionized water at the same time. After the addition was completed, crystallization was carried out at a temperature of 60 °C for 5 hours, centrifuged, and the obtained solid product was dried at 80 °C in a vacuum oven for 10 hours, and the dried solid was calcined at 330 °C in a muffle furnace for 5 hours. Carbonization was carried out in a tubular furnace, at 100 °C, 5 MPa, for 24 hours in a 50% CO2 / Ar atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=1.5 was used as the raw gas, the reaction was carried out at 240 ℃, 0.1 MPa, and the space velocity was 2000 h -1 .

[0066] [Example 13]

[0067] The salt solution was obtained by stirring and dissolving the cobalt nitrate: lanthanum nitrate: zirconium nitrate: water at a molar ratio of 1:0.6:3:100. The alkaline solution was obtained by stirring and dissolving the sodium carbonate: water at a molar ratio of 1:50. The catalyst was prepared by double-drop coprecipitation method, the precipitation temperature was 15 °C, the pH value was controlled at 7.5, a certain amount of deionized water was prepared according to the mass ratio of cobalt: water = 1:100, and the salt solution and the alkaline solution were added dropwise to the deionized water at the same time. After the addition was completed, crystallization was carried out at a temperature of 70 °C for 6 hours, centrifuged, and the obtained solid product was dried in an oven at 80 °C for 10 hours, and the dried solid was calcined at 300 °C in a muffle furnace for 5 hours. Carbonization was carried out in a tubular furnace, at 600 °C, 0.1 MPa, for 5 hours in a pure CO2 atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction temperature was 500 ℃, the pressure was 0.1 MPa, and the space velocity was 2000 h -1 .

[0068] [Example 14]

[0069] The salt solution was obtained by stirring and dissolving the cobalt nitrate: cerium acetate: copper chloride: water at a molar ratio of 1:0.2:0.2:100. The alkaline solution was obtained by stirring and dissolving the sodium carbonate: water at a molar ratio of 1:50. The catalyst was prepared by double-drop coprecipitation method, the precipitation temperature was 25 °C, the pH value was controlled at 9, a certain amount of deionized water was prepared according to the mass ratio of cobalt: water = 1:80, and the salt solution and the alkaline solution were simultaneously added dropwise to the deionized water. After the addition was completed, crystallization was carried out at a temperature of 70 °C for 6 hours, centrifuged, and the obtained solid product was dried at 80 °C in a vacuum oven for 10 hours, and the dried solid was calcined at 300 °C in a muffle furnace for 5 hours. Carbonization was carried out in a tubular furnace at 300 °C, 10 MPa, carbonization for 5 hours in a pure CO atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction temperature was 260 ℃, the pressure was 0.1 MPa, and the space velocity was 2000 h -1 .

[0070] [Example 15]

[0071] The salt solution was obtained by stirring and dissolving the cobalt acetate: cerium nitrate: bismuth nitrate: water at a molar ratio of 1:0.5:3:50. The alkaline solution was obtained by stirring and dissolving the ammonium carbonate: water at a molar ratio of 1:100. The catalyst was prepared by a single drop precipitation method, the precipitation temperature was 90 °C, the salt solution was added dropwise to the alkaline solution, and the final pH value was controlled at 9. After the addition was completed, crystallization was carried out at a temperature of 150 °C for 72 hours, filtered and separated, and the obtained solid product was dried at 80 °C in a vacuum oven for 48 hours, and the dried solid was calcined at 500 °C in a muffle furnace for 4 hours. Carbonization was carried out in a tubular furnace at 300 °C, 10 MPa, carbonization for 5 hours in a pure CO2 atmosphere, and the space velocity was 4000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction temperature was 270 ℃, the pressure was 0.1 MPa, and the space velocity was 2000 h -1 .

[0072] [Example 16]

[0073] 1) Stir and dissolve cobalt chloride: lanthanum acetate: ruthenium nitrate: water in a molar ratio of 1:2:0.3:120 to obtain a salt solution. Stir and dissolve potassium carbonate: ammonium carbonate: water in a molar ratio of 1:5:50 to obtain an alkaline solution. The catalyst was prepared by a single drop precipitation method, the precipitation temperature was 50 °C, the alkaline solution was added dropwise to the salt solution, and the pH value was controlled at 7.5. After the addition was completed, crystallization was carried out at a temperature of 100 °C for 10 hours, centrifuged, and the obtained solid product was dried at 120 °C in a vacuum oven for 48 hours, and the dried solid was calcined at 300 °C in a muffle furnace for 4 hours. Carbonization was carried out in a tubular furnace at 300 °C, 6MPa, for 5 hours in a 10% CO2 / Ar atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction was carried out at 240 ℃, 0.1 MPa, and the space velocity was 2000 h -1 .

[0074] [Example 17]

[0075] The salt solution was obtained by stirring and dissolving the cobalt nitrate: cerium acetate: molybdenum nitrate: water at a molar ratio of 1:0.1:0.15:50. The alkaline solution was obtained by stirring and dissolving the ammonium carbonate: water at a molar ratio of 1:100. The catalyst was prepared by a single drop precipitation method, the precipitation temperature was 0 °C, the salt solution was added dropwise to the alkaline solution, and the final pH value was controlled at 7. After the addition was completed, the product was crystallized at 120 °C for 12 hours, centrifuged, and the solid product was dried at 80 °C in an oven for 24 hours, and the dried solid was calcined at 400 °C in a muffle furnace for 6 hours. The calcined solid was impregnated with an equal volume of cobalt: sodium carbonate at a molar ratio of 1:0.2, dried at 100 °C for 12 hours, and calcined at 400 °C for 6 hours. Carbonization was performed in a tubular furnace at 400 °C, 2 MPa, and carbonization for 12 hours in a pure CH4 atmosphere with a space velocity of 2000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction temperature was 300 ℃, the pressure was 0.1 MPa, and the space velocity was 2000 h -1 TEM characterization results of its cobalt carbide-based catalyst showed that it was successful in controlling the synthesis of Co2C nanostructures with specific exposed crystal faces under the conditions of electron-assisted agents, such as Figure 2 As shown in f.

[0076] [Example 18]

[0077] The salt solution was obtained by stirring and dissolving the cobalt acetate: lanthanum nitrate: chromium nitrate: water at a molar ratio of 1:0.05:1:25. The alkaline solution was obtained by stirring and dissolving the potassium hydroxide: water at a molar ratio of 1:25. The catalyst was prepared by a single drop precipitation method, the precipitation temperature was 90 °C, the salt solution was added dropwise to the alkaline solution, and the final pH value was controlled at 10. After the addition was completed, the product was crystallized at 80 °C for 72 hours, centrifuged, and the solid product was dried at 60 °C in a vacuum oven for 48 hours, and the dried solid was calcined at 330 °C in a muffle furnace for 12 hours. The calcined solid was impregnated with an equal volume of cobalt: sodium carbonate at a molar ratio of 1:0.4, dried at 120 °C for 4 hours, and calcined at 500 °C for 4 hours. Carbonization was performed in a tubular furnace at 400 °C, 0.1 MPa, for 8 hours in a 25% CH4 / Ar atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=1 was used as the raw gas, the reaction was carried out at 230 ℃, 0.2 MPa, and the space velocity was 2000 h -1 .

[0078] [Example 19]

[0079] The salt solution was obtained by stirring and dissolving the cobalt nitrate: lanthanum acetate: zirconium nitrate: water at a molar ratio of 1:0.8:0.3:35. The alkaline solution was obtained by stirring and dissolving the ammonium carbonate: water at a molar ratio of 1:25. The catalyst was prepared by double drop coprecipitation method, the precipitation temperature was 90 °C, the pH value was controlled at 9, a certain amount of deionized water was prepared according to the mass ratio of cobalt: water = 1:10, and the salt solution and the alkaline solution were simultaneously added dropwise to the deionized water. After the addition was completed, the product was crystallized at 80 °C for 72 hours, centrifuged, and the solid product was dried at 80 °C in an oven for 48 hours, and the dried solid was calcined at 330 °C in a muffle furnace for 12 hours. The calcined solid was impregnated with an equal volume of cobalt: potassium hydroxide at a molar ratio of 1:0.2, dried at 60 °C for 12 hours, and the dried solid was calcined at 400 °C for 4 hours. Carbonization was carried out in a tube furnace at 400 °C, 0.1 MPa, for 8 h in a 30% CO / Ar atmosphere with a space velocity of 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=0.5 was used as the raw gas, the reaction was carried out at 270 ℃, 0.3 MPa, and the space velocity was 2000 h -1 .

[0080] [Example 20]

[0081] The salt solution was obtained by stirring and dissolving the cobalt nitrate: cerium nitrate: ruthenium nitrate: water at a molar ratio of 1:0.5:0.6:40. The alkaline solution was obtained by stirring and dissolving the potassium carbonate: water at a molar ratio of 1:30. The catalyst was prepared by double drop coprecipitation method, the precipitation temperature was 90 °C, the pH value was controlled at 9, a certain amount of deionized water was prepared according to the mass ratio of cobalt: water = 1:15, and the salt solution and the alkaline solution were simultaneously added dropwise to the deionized water. After the addition was completed, the product was crystallized at 120 °C for 72 hours, centrifuged, and the solid product was dried at 80 °C in an oven for 48 hours, and the dried solid was calcined at 330 °C in a muffle furnace for 12 hours. The calcined solid was impregnated with an equal volume of cobalt: lithium nitrate at a molar ratio of 1:0.1, dried at 80 °C for 12 hours, and calcined at 500 °C for 5 hours. Carbonization was carried out in a tube furnace at 400 °C, 0.1 MPa, for 8 h in a 20% CO / Ar atmosphere with a space velocity of 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=1.5 was used as the raw gas, the reaction was carried out at 240 ℃, 1 MPa, and the space velocity was 2000 h -1 .

[0082] [Example 21]

[0083] The salt solution was obtained by stirring and dissolving the molar ratio of cobalt nitrate: cerium nitrate: zinc nitrate: water = 1:0.6:0.5:25. The alkaline solution was obtained by stirring and dissolving the molar ratio of sodium carbonate: water = 1:25. The catalyst was prepared by double drop coprecipitation method, the precipitation temperature was 50 ℃, the pH value was controlled at 8.5, a certain amount of deionized water was prepared according to the mass ratio of cobalt: water = 1:25, the salt solution and the alkaline solution were added dropwise to the deionized water at the same time, after the addition was completed, centrifuged, and the obtained solid product was dried in an oven at 100 ℃ for 4 hours, and the dried solid was calcined at 350 ℃ in a muffle furnace for 6 hours. Carbonization was carried out in a tubular furnace, in a mixed atmosphere of H2 and CO (H2 / CO=1, v / v) at 250 ℃, 0.1 MPa, carbonization for 4 hours, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction temperature was 260 ℃, the pressure was 0.1 MPa, and the space velocity was 2000 h -1 .

[0084] [Example 22]

[0085] The salt solution was obtained by stirring and dissolving the cobalt nitrate: cerium nitrate: zinc nitrate: water at a molar ratio of 1:0.03:0.2:25. The alkaline solution was obtained by stirring and dissolving the sodium carbonate: water at a molar ratio of 1:25. The catalyst was prepared by double drop coprecipitation method, the precipitation temperature was 30 ℃, the pH value was controlled at 8.0, a certain amount of deionized water was prepared according to the mass ratio of cobalt: water = 1:25, and the salt solution and the alkaline solution were simultaneously added dropwise to the deionized water. After the addition was completed, the product was crystallized at 30 ℃ for 2 hours, filtered and separated, and the solid product was dried at 80 ℃ in an oven for 12 hours, and the dried solid was calcined at 330 ℃ for 6 hours. Carbonization was carried out in a tubular furnace, in a mixed atmosphere of H2 and CO (H2 / CO=1, v / v) at 250 ℃, 0.2 MPa, carbonization for 10 hours, and the space velocity was 8000h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction temperature was 260 ℃, the pressure was 0.1 MPa, and the space velocity was 3000h -1 .

[0086] [Comparative Example 1]

[0087] The salt solution was obtained by stirring and dissolving the cobalt acetate: water at a molar ratio of 1:25. The alkaline solution was obtained by stirring and dissolving the sodium carbonate: water at a molar ratio of 1:25. The catalyst was prepared by double-drop co-precipitation method, the precipitation temperature was 40 °C, and the pH value was controlled at 7.5. After the addition was completed, crystallization was carried out at a temperature of 60 °C for 2 hours, centrifuged, and the obtained solid product was dried in an oven at 100 °C for 4 hours, and the dried solid was calcined at 350 °C for 6 hours. Carbonization was carried out in a tubular furnace at 250 °C, 0.1 MPa, for 4 hours in a pure H2 atmosphere, and the space velocity was 8000 h -1 The fixed bed was used as the reactor, the synthesis gas with H2 / CO=2 was used as the raw gas, the reaction temperature was 260 ℃, the pressure was 0.1 MPa, and the space velocity was 2000 h -1 , the XRD and TEM characterization results of its cobalt carbide-based catalyst showed that without adding crystal face stabilizers and electronic additives, although Co2C phase could be generated, specific exposed crystal faces could not be generated, such as Figure 1 and Figure 2 As shown in b.

[0088] [Comparative Example 2]

[0089] The salt solution was obtained by stirring and dissolving the cobalt nitrate: cerium nitrate: zinc nitrate: water at a molar ratio of 1:0.03:0.2:25. The alkaline solution was obtained by stirring and dissolving the sodium carbonate: water at a molar ratio of 1:25. The catalyst was prepared by double-drop coprecipitation method, the precipitation temperature was 30 °C, the pH value was controlled at 8.0, a certain amount of deionized water was prepared according to the mass ratio of cobalt: water = 1:25, and the salt solution and the alkaline solution were simultaneously added dropwise to the deionized water. After the addition was completed, crystallization was carried out at a temperature of 30 °C for 2 hours, filtration and separation were carried out, and the obtained solid product was dried in an oven at 80 °C for 12 hours, and the dried solid was calcined at 330 °C for 6 hours. Using a fixed bed as a reactor, reduction was carried out at 300 °C, 0.1 MPa, and 5 hours in a 10% H2 / Ar atmosphere, with a space velocity of 12000 h -1 , using H2 / CO=2 synthesis gas as raw gas, reaction at 260 ℃, 0.1 MPa, and space velocity of 3000 h -1 The XRD and TEM characterization results of the cobalt carbide-based catalyst show that the addition of the crystal surface stabilizer Ce and the electron auxiliary agent Zn at the same time can generate the Co2C phase, but the electron auxiliary agent Zn will affect the crystal surface stabilization effect of Ce, so the cobalt carbide-based catalyst with specific exposed crystal surfaces cannot be generated, and its Co2C nanoparticles have a spherical morphology, such as Figure 1 and Figure 2 As shown in c.

[0090] By comparing Example 22 and Comparative Example 2, it can be seen that the present invention obtains a cobalt carbide-based catalyst with specific exposed crystal faces by carbonization instead of reduction. This catalyst is applied to the Fischer-Tropsch synthesis reaction. Compared with the spherical cobalt carbide-based catalyst of Comparative Example 2, it can improve the CO conversion rate and olefin selectivity while reducing the methane selectivity.

[0091] Table 1 Catalyst reaction results of examples and comparative examples

[0092]

[0093] As can be seen from Table 1, the cobalt carbide-based catalyst promoted by the crystal face stabilizer can be effectively used in the Fischer-Tropsch synthesis reaction, and has high activity and olefin selectivity, and low methane selectivity.

[0094] The above is only a preferred embodiment of the present invention, and is not any formal or substantial limitation of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention, and these improvements and supplements should also be regarded as the protection scope of the present invention. Any technician familiar with this profession, without departing from the spirit and scope of the present invention, can make some changes, modifications and evolutions of the technical content disclosed above, which are equivalent embodiments of the present invention; at the same time, any changes, modifications and evolutions of any equivalent changes made to the above embodiments based on the essential technology of the present invention are still within the scope of the technical solution of the present invention.

Claims

1. A method for preparing a cobalt carbide-based catalyst containing an electron-aiding agent and having a specific exposed crystal face, characterized in that: The preparation method comprises the following steps: 1) Mixing and dissolving a cobalt salt, a crystal surface stabilizer, an electronic auxiliary agent and a solvent to obtain a salt solution; the crystal surface stabilizer is one or more rare earth metal salts, and the metal element in the rare earth metal salt is one or more of lanthanide metals, scandium and yttrium; the electronic auxiliary agent is one or more of main group metal salts and transition metal salts; wherein the molar ratio of cobalt salt: crystal surface stabilizer: electronic auxiliary agent is 1: (0.01-3): (0.0001-10), and the molar amount of the cobalt salt is calculated based on the molar amount of Co atoms; 2) mixing and dissolving an alkaline precipitant and a solvent to obtain an alkaline solution; 3) precipitating the salt solution of step 1) and the alkaline solution of step 2) by a precipitation method, and then crystallizing, separating, drying, and calcining in an air atmosphere after precipitation, or directly separating, drying, and calcining in an air atmosphere without crystallization after precipitation; 4) The calcined product obtained in step 3) is directly carbonized without reduction to generate a cobalt carbide-based catalyst containing an electron auxiliary agent and having a specific exposed crystal face, wherein the specific exposed crystal face refers to a (101) and / or (020) face.

2. The preparation method according to claim 1, characterized in that: The preparation method further comprises: loading the calcined product obtained in step 3) with an alkali metal auxiliary agent by an impregnation method, drying, calcining in an air atmosphere, and then performing the operation of step 4).

3. The preparation method according to claim 2, characterized in that: The alkali metal auxiliary agent is one or more of an alkali metal base and an alkali metal salt; the alkali metal base is lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide or cesium hydroxide; the alkali metal salt is one or more of an inorganic alkali metal salt and an organic alkali metal salt, the inorganic alkali metal salt is lithium nitrate, lithium carbonate, lithium sulfate, sodium nitrate, sodium carbonate, potassium nitrate, rubidium nitrate or cesium nitrate, and the organic alkali metal salt is lithium acetate, sodium acetate, potassium acetate or sodium citrate; The molar ratio of the cobalt salt to the alkali metal additive is controlled to be 1:(0.0001-5), wherein the molar amount of the cobalt salt is based on the molar amount of Co atoms; the calcined product obtained in step 3) is loaded with the alkali metal additive by an impregnation method and dried, and then calcined in an air atmosphere under the following conditions: the calcination temperature is 200-800°C; and the calcination time is 1-36 hours.

4. The preparation method according to any one of claims 1 to 3, characterized in that: In step 1), the cobalt salt is one or more of an organic cobalt salt and an inorganic cobalt salt; the organic cobalt salt is one or both of cobalt formate and cobalt acetate; the inorganic cobalt salt is one or more of cobalt nitrate, cobalt chloride and cobalt sulfate; The metal element in the electronic auxiliary agent is one or more of magnesium, calcium, vanadium, chromium, manganese, gallium and indium.

5. The preparation method according to any one of claims 1 to 3, characterized in that: In step 1), the molar ratio of the cobalt salt to the crystal surface stabilizer, the electronic auxiliary agent, and the solvent is 1:(0.01-3):(0.0001-10):(10-2000).

6. The preparation method according to any one of claims 1 to 3, characterized in that: In step 2), the alkaline precipitant is one or more of an alkali and an alkaline salt, the alkali is one or more of lithium hydroxide, sodium hydroxide, potassium hydroxide, and ammonia water; the alkaline salt is one or more of sodium carbonate, ammonium carbonate, sodium bicarbonate, and potassium carbonate; the molar ratio of the alkaline precipitant to the solvent is 1:(10~1500).

7. The preparation method according to any one of claims 1 to 3, characterized in that: In step 3), the precipitation method is a forward / reverse single drop precipitation method or a double drop co-precipitation method, the precipitation temperature is 0-120°C, and the precipitation pH is controlled at 7-12; In step 3), the crystallization temperature is 0-200°C; the crystallization time is 0-48 hours; In step 3), the calcination temperature is 200-800°C and the calcination time is 1-36 hours.

8. The preparation method according to any one of claims 1 to 3, characterized in that: In step 4), the carbonization atmosphere is a carbonization gas A, a mixed gas of carbonization gas A and hydrogen, or a mixed gas of carbonization gas A and an inert gas, wherein the carbonization gas A is selected from one or more of carbon monoxide, methane, ethane, and ethylene, and the volume percentage of hydrogen in the mixed gas of carbonization gas A and hydrogen is not higher than 80%; In step 4), the carbonization conditions are: carbonization temperature is 100-600 °C, carbonization pressure is 0.1-10 MPa, and volume space velocity is 500-100000 h -1 , the carbonization time shall not exceed 24 hours.

9. A cobalt carbide-based catalyst containing an electron auxiliary agent and having a specific exposed crystal face obtained according to the preparation method of any one of claims 1 to 8.

10. Use of the cobalt carbide-based catalyst with specific exposed crystal faces containing an electron auxiliary agent as claimed in claim 9 in Fischer-Tropsch synthesis.